An offline regeneration and repair method for continuous casting nozzles
By employing a multi-stage physical cleaning and mechanical repair method, the problems of flow channel blockage and surface damage in continuous casting nozzles under high-temperature environments were solved, achieving low-cost, non-destructive regeneration and repair, and reducing the overall scrap rate and maintenance costs.
Patent Information
- Application Number
- CN202611291133.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-10
AI Technical Summary
Continuous casting nozzles are prone to defects such as flow channel blockage, surface scaling, thread corrosion, and sealing surface wear in high-temperature, high-humidity environments and environments containing impurities such as iron oxide scale and protective slag. Existing repair technologies are costly or ineffective, resulting in a high overall scrap rate.
A multi-stage physical cleaning method is adopted, including dry ice spraying, ultrasonic vibration and high-pressure pulse flushing, combined with mechanical defect repair and interchangeable parts, to achieve non-destructive regeneration and repair of nozzles.
It effectively removes hard composite scale inside the nozzle, reduces the overall scrap rate, significantly reduces spare parts procurement and maintenance costs, ensures machine performance, and has high industrial applicability and promotion value.
Abstract
Description
Technical Field
[0001] This application relates to the field of continuous casting equipment maintenance technology, specifically to an offline regeneration and repair method for continuous casting nozzles. Background Technology
[0002] In the continuous casting process of steel enterprises, the air-water atomizing nozzles in the secondary cooling zone are exposed to high temperature, high humidity, and circulating cooling water containing impurities such as iron oxide scale and protective slag for extended periods. This makes them highly susceptible to defects such as flow channel blockage, surface scaling, thread corrosion, and wear on sealing surfaces. Currently, the treatment of nozzles after production mainly falls into two categories: one is direct scrapping and replacement with new parts, resulting in significant resource waste and spare parts cost pressure; the other is the use of repair processes. However, existing high-end repair technologies such as laser cladding and precision welding rely on expensive equipment, resulting in extremely high investment and maintenance costs, making them difficult to popularize in small and medium-sized steel mills. Traditional simple pickling or water washing processes can only remove surface scale and cannot effectively remove hard composite scale within the micro-flow channels, nor can they repair physical damage to threads, sealing surfaces, and nozzles. This leads to poor atomization performance and sealing failure in repaired nozzles, resulting in extremely low reuse rates. Therefore, there is an urgent need for a repair method that can achieve non-destructive nozzle regeneration and ensure operational performance through physical means without relying on high-end hot processing equipment. Summary of the Invention
[0003] To address the problems of high repair costs and poor results of simple repairs leading to high overall scrap rates in existing continuous casting nozzle technologies, this application proposes an offline regeneration and repair method for continuous casting nozzles, enabling low-cost, non-destructive regeneration and graded reuse of offline nozzles.
[0004] To achieve the above objectives, this application adopts the following technical solution: An offline regeneration and repair method for continuous casting nozzles includes: acquiring multiple nozzle components to be repaired after damage classification screening and full disassembly; performing multi-level physical synergistic cleaning on the nozzle components to remove adhering substances; performing mechanical defect repair on the cleaned nozzle components, and interchanging and assembling the repaired nozzle components based on dimensional inspection results to obtain reconstituted nozzle components; assembling the reconstituted nozzle components to obtain a regenerated nozzle, and determining the application level of the regenerated nozzle based on offline performance verification results.
[0005] As one implementation method, multi-stage physical synergistic cleaning is performed on the nozzle components to be repaired to remove the deposits on the nozzle components, including: dry ice blasting cleaning of the nozzle components to be repaired, using the low-temperature embrittlement and impact of dry ice particles to peel off the hard scale on the surface of the nozzle components to be repaired; ultrasonic vibration cleaning of the nozzle components to be repaired after dry ice blasting cleaning, using ultrasonic cavitation to peel off loose impurities in the micropores of the nozzle components to be repaired; and high-pressure pulse flushing of the nozzle components to be repaired after ultrasonic vibration cleaning, combined with flexible unblocking tools to unclog the blocked channels of the nozzle components to be repaired.
[0006] In one implementation method, the dry ice blasting cleaning uses dry ice particles with a particle size of 0.8-1.2 mm and a blasting pressure of 0.5-0.7 MPa, which are aimed at the nozzle inlet, inner flow channel, and vortex cavity. In the ultrasonic vibration cleaning, the nozzle component to be repaired is placed in a room temperature pure water ultrasonic cleaning tank and vibrated for 20-30 minutes. In the high-pressure pulse flushing, high-pressure pure water with a pressure of 10-12 MPa is used to pulse flush the water inlet, air inlet, mixing channel, and atomizing micropores of the nozzle component to be repaired. The flexible unblocking tool includes nylon needles of different specifications and ultra-fine fiber soft brushes, which are used to thoroughly clean the atomizing micropores one by one.
[0007] As one implementation method, multiple nozzle components to be repaired are obtained after damage classification screening and full disassembly, including: performing a preliminary visual and flow channel inspection on the continuous casting nozzles coming off the production line, classifying them into repairable parts, degraded parts, and directly scrapped parts; using the repairable parts and the degraded parts as nozzles to be repaired, and discarding the directly scrapped parts; fully disassembling the nozzles to be repaired, and removing damaged and deformed vulnerable parts to obtain the multiple nozzle components to be repaired; wherein, the repairable parts are nozzles with flow channel scaling or nozzle orifice blockage and no structural damage to the substrate; the degraded parts are nozzles with slight local deformation and no material loss; and the directly scrapped parts are nozzles with substrate cracking, nozzle chipping or perforation, or severe corrosion.
[0008] As one implementation method, mechanical defect repair is performed on the cleaned nozzle components, including: for thread corrosion, manual tapping or threading is performed using a standard tap or die of the corresponding specification to remove rust and impurities from the thread surface; if the thread is chipped, stripped, or severely worn beyond tolerance, the corresponding component is scrapped; for wear on the sealing surface, metallographic sandpaper is used for step-by-step grinding and surface polishing compound polishing; if the wear depth of the sealing surface is greater than 0.2mm or penetrating scratches appear, the corresponding component is scrapped; for nozzle wear, an ultra-fine polishing head and micro-orifice polishing compound are used for polishing repair; if the nozzle diameter enlargement is greater than 8% of the original size, the corresponding component is scrapped; for minor bumps and deformations of the housing, cold straightening is performed using special tooling; if straightening is not possible, the corresponding component is scrapped.
[0009] As one implementation method, the repaired nozzle components are interchanged and reassembled based on dimensional inspection results to obtain reconstituted nozzle components. This includes: inspecting the key dimensions of the repaired nozzle components and grouping the qualified nozzle components as intact components; replacing the damaged nozzle components with the intact components to complete the interchangeability; and assembling the reconstituted nozzle components to obtain a regenerated nozzle, which includes: applying high-temperature anti-seize grease and sealing grease to the threaded mating surfaces and sealing contact surfaces, replacing the seals with brand new standard seals, and assembling the reconstituted nozzle components according to standard torque.
[0010] As one implementation method, the application level of the regenerated nozzle is determined based on the offline performance verification results, including: connecting the regenerated nozzle to a water-air test bench to simulate the actual working conditions of continuous casting secondary cooling, and conducting performance testing under a normal temperature clean water medium with a set water pressure of 0.2-0.4MPa and an air pressure of 0.15-0.5MPa; detecting the water flow rate, atomization angle, droplet uniformity, and water-air sealing performance of the regenerated nozzle, and comparing them with the standard parameters of a brand new nozzle; when the water flow rate deviation is less than or equal to ±5%, the atomization angle deviation is between 0° and 3°, there is no air or water leakage, and the atomization is uniform and without flow deviation, the regenerated nozzle is deemed to have passed the verification; based on the category of the repairable part or the degraded part to which the verified regenerated nozzle belongs, its corresponding application level is determined.
[0011] As one implementation method, the application level includes a normal application level and a downgraded application level. When the regenerated nozzle belongs to the category of the downgraded part and passes the inspection, its application level is determined to be the downgraded application level. The regenerated nozzle of the downgraded application level is only used in the weak cooling zone of the secondary cooling of continuous casting and is prohibited from being put into the strong cooling zone. When the regenerated nozzle belongs to the category of the repairable part and passes the inspection, its application level is determined to be the normal application level. After the application level is determined, the regenerated nozzle is sprayed with rust inhibitor and affixed with a unique repair label containing the repair date, specifications and downgraded category before being put into storage.
[0012] As one implementation method, before performing multi-stage physical synergistic cleaning on the nozzle components to be repaired, the method further includes: using a high-pressure water jet with a pressure of 70-90 MPa to perform a rough cleaning on the nozzle components to be repaired, to remove the thick layer of oxide scale and muddy scale on the surface; after the multi-stage physical synergistic cleaning is completed, using dry compressed air to blow the nozzle components to be repaired in all directions to ensure that there is no water or dust accumulation in the flow channel and on the surface.
[0013] As one implementation method, the cleaning media of the multi-stage physical synergistic cleaning includes only pure water, dry ice and compressed air; the repair methods of the mechanical defect repair include only mechanical grinding, tapping, cold straightening and polishing; the material of the nozzle component to be repaired is stainless steel, and the multi-stage physical synergistic cleaning and the mechanical defect repair are performed at room temperature. Beneficial effects
[0014] The offline regeneration and repair method for continuous casting nozzles provided in this application utilizes a multi-stage physical synergistic cleaning mechanism. By leveraging the low-temperature embrittlement and impact of dry ice blasting, the cavitation effect of ultrasonic vibration, and the physical synergistic effect of high-pressure pulse combined with flexible unblocking, it achieves non-destructive and thorough removal of hard composite scale in the nozzle's micro-channels without the use of strong chemical acids or thermal processing. This avoids substrate corrosion and dimensional changes, and solves the technical problem that traditional simple cleaning methods cannot remove deep-seated scale.
[0015] Meanwhile, this application establishes a component interchangeability and downgraded application strategy based on damage classification. By finely classifying and screening the nozzles off the production line and completely disassembling them, only components with severe structural damage are scrapped, while intact substrates are preserved. The use of available parts is maximized through interchangeability and combination, which significantly reduces the overall scrap rate. Combined with strict offline performance verification and graded application restrictions, the cooling performance and safety of the regenerated nozzles are ensured when they are used on the machine. Under the premise of ensuring production quality, the cost of spare parts procurement and equipment operation and maintenance is greatly reduced, which has extremely high industrial applicability and promotion value. Detailed Implementation Example 1
[0016] This embodiment provides an offline regeneration and repair method for continuous casting nozzles. This method abandons traditional high-cost hot working repair or simple chemical cleaning processes, achieving low-cost, non-destructive regeneration of offline nozzles through purely physical and mechanical means. Specifically, the offline regeneration and repair method for continuous casting nozzles includes the following steps: Step S100: Obtain multiple nozzle components to be repaired after damage grading screening and full disassembly.
[0017] Specifically, this step aims to accurately identify recyclable substrates and components from batches of continuously casting nozzles and transform them into independently processable component units. Through visual inspection and initial flow channel patency checks, nozzles with structural damage (such as substrate cracking or severe corrosion perforation) are directly discarded, retaining only those with repairable defects such as scaling, minor wear, or localized deformation. The nozzles to be repaired are then completely disassembled into individual components such as nozzle heads, inner cores, connectors, and seals, while discarding easily damaged or aged parts. This damage-based full disassembly strategy avoids the waste of resources that would otherwise lead to the scrapping of the entire unit due to localized damage, providing a material basis for subsequent refined repair of individual components.
[0018] Step S200: Perform multi-stage physical synergistic cleaning on the nozzle components to be repaired to remove any adhering substances from the nozzle components.
[0019] This step utilizes the synergistic effect of multiple physical mechanisms to thoroughly remove complex scale within the microchannels without damaging the stainless steel substrate. Due to the complex internal channel structure and tiny pore size of continuous casting nozzles, a single cleaning method often struggles to simultaneously remove hard scale and unblock micropores. This embodiment employs a multi-stage synergistic physical cleaning approach, using an ordered combination of different physical actions to target and remove surface scale, crevices, and deep-pore blockages. The entire process relies solely on physical energy, without the use of any chemical pickling agents, thus avoiding the risk of intergranular corrosion and ensuring the integrity and dimensional stability of the nozzle substrate material.
[0020] Step S300: Perform mechanical defect repair on the cleaned nozzle parts to be repaired, and interchange and match the repaired nozzle parts based on the dimensional inspection results to obtain reconstituted nozzle parts.
[0021] This process comprises two core components: defect repair and resource reconfiguration. In the mechanical defect repair phase, physical damage exposed after cleaning, such as thread corrosion, scratches on sealing surfaces, nozzle burrs, or minor deformation of the housing, is repaired using purely mechanical machining methods to restore the geometric accuracy and functional fit of the parts. In the interchangeable assembly phase, critical dimensions of the repaired parts are inspected. Qualified parts are grouped into a usable resource pool, and intact salvaged parts replace those scrapped due to excessive damage. This "repair + assembly" model breaks the traditional "original parts, original fit" limitation of maintenance, enabling resource-based reconfiguration of parts across nozzles and significantly improving the overall utilization rate of parts.
[0022] In step S400, the reconstituted nozzle components are assembled to obtain a regenerated nozzle, and the application level of the regenerated nozzle is determined based on the offline performance verification results.
[0023] This step completes the final molding and quality grading of the regenerated nozzles. Following standard assembly procedures, the reassembled components are assembled into a complete regenerated nozzle. Offline performance verification under simulated real-world conditions verifies whether its flow rate, atomization angle, and sealing performance meet usage requirements. Based on the verification results and the original damage type of the components, qualified regenerated nozzles are classified into different application levels, such as normal application level or downgraded application level limited to specific areas. This grading mechanism ensures the performance reliability of nozzles used in production while providing a compliant application path for regenerated nozzles with slightly deviated performance but still usable value, further tapping into the remaining value of used nozzles.
[0024] Example 2 This embodiment, based on Embodiment 1, further defines the specific implementation method of multi-stage physical synergistic cleaning. As one implementation method, multi-stage physical synergistic cleaning is performed on the nozzle components to be repaired to remove deposits, including: dry ice blasting cleaning of the nozzle components to be repaired, utilizing the low-temperature embrittlement and impact of dry ice particles to peel off hard scale from the surface of the nozzle components; ultrasonic oscillation cleaning of the nozzle components after dry ice blasting cleaning, utilizing ultrasonic cavitation to peel off loose impurities within the micropores of the nozzle components; and high-pressure pulse flushing of the nozzle components after ultrasonic oscillation cleaning, combined with flexible unblocking tools to unclog the blocked channels of the nozzle components.
[0025] Specifically, the three cleaning steps described above are not simply an independent superposition, but rather a physical synergistic removal mechanism designed to address the hard, complex scaling characteristics within the micro-channels of continuous casting nozzles. In step S201, dry ice blasting cleaning, the dry ice particles instantly sublimate and absorb heat upon contact with the scaling surface. This causes the iron oxide scale and calcium-magnesium scale adhering to the stainless steel substrate to develop micro-cracks due to rapid contraction. Simultaneously, the high-speed kinetic energy of the particles mechanically peels the embrittled hard scale from the substrate. This process is non-abrasive cleaning and does not alter the original dimensions of the nozzle's precision channels. In step S202, ultrasonic vibration cleaning, the high-frequency cavitation bubbles generated by ultrasound in pure water can penetrate deep into micron-level gaps and dead corners of the vortex cavity that are difficult for dry ice blasting to reach. The localized shock waves released when the bubbles collapse completely dislodge any loose but still adhered impurities. In step S203, high-pressure pulse flushing, the pulsating shear force of the high-pressure water flow, combined with the mechanical contact of the flexible unclogging tool, forces the scale and sludge that were treated in the first two steps but not yet removed from the blocked channels, thereby achieving gradient non-destructive cleaning from the macroscopic surface to the microscopic deep pores. This synergistic mechanism effectively solves the technical problem that a single cleaning method cannot simultaneously achieve both the removal rate of hard scale and the unobstructed flow of micropores.
[0026] In practice, the process parameters for each cleaning step can be adjusted according to the nozzle specifications and the degree of scaling. For example, in dry ice blasting cleaning, the particle size of the dry ice can be selected as 0.8-1.2 mm, the blasting pressure is controlled within the range of 0.5-0.7 MPa, and multi-angle blasting is performed targeting the nozzle inlet, inner flow channel, and vortex cavity to ensure that the embrittlement and peeling effect covers all key scaling areas. If the particle size is too small or the pressure is too low, the impact kinetic energy will be insufficient to peel off dense, hard scale; if the particle size is too large or the pressure is too high, it may cause unnecessary erosion risk to the surface of precision flow channels. In ultrasonic oscillation cleaning, the nozzle parts to be repaired are placed in a room temperature pure water ultrasonic cleaning tank and oscillated for 20-30 minutes. This time window is sufficient to ensure that cavitation fully penetrates the micropores and avoids damage to the passivation film on the substrate surface caused by prolonged immersion. In high-pressure pulse flushing, high-pressure pure water at a pressure of 10-12 MPa is used to pulse flush the water inlet, air inlet, mixing channel and atomizing micropore of the nozzle components to be repaired. This pressure level can provide sufficient flushing force to remove residual scale and sludge, while being below the safety threshold that would cause plastic deformation of thin-walled structures.
[0027] For delicate areas such as atomizing micropores that are easily damaged, flexible cleaning tools include nylon needles of different sizes and microfiber brushes for thorough cleaning of each atomizing micropore. Nylon and microfiber are chosen because their hardness is significantly lower than that of stainless steel, allowing for the physical removal of residue from the pore walls without scratching the inner surface. It is particularly important to note that this embodiment strictly prohibits the use of abrasive materials such as steel shot or iron shot for sandblasting, and also prohibits the use of wire brushes to vigorously grind the nozzle channels. These hard media can easily embed into the channel surface or cause the nozzle orifice diameter to enlarge, thereby damaging the nozzle's atomization performance and dimensional accuracy, which contradicts the non-destructive regeneration goal pursued in this application.
[0028] Example 3 Based on Example 1, this embodiment further specifies the detailed process for obtaining multiple nozzle components to be repaired after damage grading screening and full disassembly, as well as the detailed operating procedures for performing mechanical defect repair on the cleaned nozzle components to be repaired.
[0029] Specifically, in step S100, the continuous casting nozzles coming off the production line undergo a preliminary visual and flow channel inspection, categorizing them into repairable parts, downgraded parts, and directly scrapped parts. This three-tiered classification strategy constitutes the pre-approval mechanism for resource utilization in this application. Repairable parts are defined as nozzles with flow channel scaling or nozzle orifice blockage but no structural damage to the substrate; these parts can be restored to brand-new standards after cleaning and repair. Downgraded parts are defined as nozzles with minor local deformation but no material loss; their substrate integrity remains, but their geometric accuracy is compromised. While repairing them may not meet the stringent conditions of the strong cooling zone, they can still function in the weak cooling zone. Directly scrapped parts refer to nozzles with substrate cracks, nozzle chipping or perforation, or severe corrosion; such damage exceeds the physical repair boundary, and forced repair is not only costly but also poses safety hazards. Based on this classification, repairable and downgraded parts are selected as nozzles to be repaired and proceed to subsequent processes, while directly scrapped parts are discarded, thus avoiding unnecessary processing costs from the outset. Subsequently, the nozzle to be repaired was completely disassembled, breaking it down into individual metal structural components. Damaged and deformed gaskets, sealing rings, and other vulnerable parts were removed, resulting in multiple nozzle components to be repaired. This complete disassembly process allowed subsequent cleaning and repair to penetrate every mating surface and the interior of every micropore, eliminating cleaning blind spots and inspection blind areas present in the assembled state, thus providing the necessary conditions for precise repair.
[0030] After completing multi-stage physical cleaning, step S300 involves mechanical defect repair of the cleaned nozzle components. This process employs differentiated purely mechanical treatment methods based on the damage characteristics of different parts, and sets strict quantitative scrap thresholds to ensure repair quality. Specifically, for thread corrosion defects, manual tapping or threading is performed using standard taps or dies of the corresponding specifications to remove rust and impurities from the thread surface and restore the fit accuracy of the thread pair. If the inspection reveals chipped threads, stripped threads, or severe wear exceeding tolerances, it indicates that the thread's load-bearing capacity has been lost, and the corresponding component is directly scrapped to prevent the nozzle from falling off under high temperature and high pressure conditions due to connection failure. For sealing surface wear defects, metallographic sandpaper is used for step-by-step grinding combined with surface polishing paste to eliminate microscopic scratches and restore surface smoothness. If the wear depth of the sealing surface is greater than 0.2mm or penetrating scratches appear, it means that the sealing pressure cannot be effectively established, and even replacing the gasket cannot compensate for the gap. In this case, the corresponding component is directly scrapped to prevent water and air leakage during installation. To address nozzle wear defects, precision polishing and repair are performed using an ultra-fine polishing head and micro-orifice-specific polishing compound to remove carbon deposits and burrs. Since the nozzle orifice diameter directly determines the atomization angle and flow distribution, if the orifice diameter enlargement exceeds 8% of its original size, the atomization cone angle will deviate from the design range and fail subsequent performance verification; therefore, the nozzle must be scrapped. For minor impact deformation of the housing, cold straightening is performed using specialized tooling, utilizing the elastic recovery characteristics of stainless steel to restore its dimensions. If the deformation exceeds the material's yield strength, making straightening impossible, or if straightening introduces a risk of cracking, the corresponding component is scrapped.
[0031] The quantitative thresholds set during the aforementioned mechanical defect repair process (such as 0.2mm wear depth and 8% orifice enlargement) are not arbitrarily selected, but are based on engineering verification data of the sealing reliability and atomization performance tolerance of the continuous casting secondary cooling nozzle. These thresholds constitute the safety boundary of the "object access - defect handling" sub-process, ensuring that only parts with substantial regeneration value will enter the subsequent interchangeable assembly stage.
[0032] Example 4 This embodiment, based on Embodiments 1 and 3, further defines the specific implementation methods for interchangeable grouping, standardized assembly, offline performance verification, and application level determination. As one implementation method, the repaired nozzle components are interchangeably grouped based on dimensional inspection results to obtain reconstituted nozzle components. This includes: inspecting the key dimensions of the repaired nozzle components, grouping the qualified components as intact components; and replacing the damaged nozzle components with the intact components to complete the interchangeable grouping.
[0033] Specifically, this interchangeable assembly step is the core link in realizing the resource utilization of parts. After the mechanical defect repair described in Example 3 is completed, it is not simply a matter of reassembling the original nozzle parts, but rather breaking away from the traditional maintenance mindset of "original parts, original fittings". By using conventional measuring tools such as vernier calipers, micrometers, and plug gauges, a full inspection is carried out on key parameters such as nozzle orifice diameter, throttling core outer diameter, thread fit dimensions, and sealing surface flatness, and intact parts with geometric accuracy restored to the design tolerance range are selected. When a nozzle head is scrapped due to excessive orifice enlargement, but its inner core and joint are still intact, a matching nozzle head can be matched and replaced from other nozzles that are scrapped due to shell deformation but have intact nozzle heads. This cross-nozzle part reorganization strategy allows nozzles that might otherwise be scrapped as a whole to be reborn through "patchwork", significantly improving the comprehensive utilization rate of waste materials.
[0034] After completing the interchangeable assembly, the reconstituted nozzle components are assembled to obtain the recycled nozzle. This includes: applying high-temperature anti-seize grease and sealing grease to the threaded mating surfaces and sealing contact surfaces, replacing the seals with brand new standard ones, and assembling the reconstituted nozzle components according to the standard torque. Applying high-temperature anti-seize grease not only facilitates subsequent disassembly and maintenance but also prevents the stainless steel threads from seizing in a high-temperature, humid environment; the sealing grease is used to fill microscopic gaps and assist the sealing ring in establishing a reliable sealing barrier. Sealing gaskets and sealing rings are disposable consumable parts; reuse of old parts is strictly prohibited, and all must be replaced with brand new standard parts conforming to original factory specifications. During assembly, a torque wrench is used to strictly tighten to the standard torque. This avoids both excessive torque causing cracking of the thin-walled shell or deformation of the inner core due to compression, and insufficient torque causing water and air leaks after installation, ensuring that the assembly quality of the recycled nozzle is consistent with that of the brand new nozzle.
[0035] As one implementation method, the application level of the regenerated nozzle is determined based on the offline performance verification results, including: connecting the regenerated nozzle to a water-air test bench to simulate the actual working conditions of continuous casting secondary cooling, and conducting performance testing under a normal temperature clean water medium with a set water pressure of 0.2-0.4MPa and an air pressure of 0.15-0.5MPa; detecting the water flow rate, atomization angle, droplet uniformity, and water-air sealing performance of the regenerated nozzle, and comparing them with the standard parameters of a brand new nozzle; when the water flow rate deviation is less than or equal to ±5%, the atomization angle deviation is between 0° and 3°, there is no air or water leakage, and the atomization is uniform and without flow deviation, the regenerated nozzle is deemed to have passed the verification; based on the category of repairable or downgraded parts to which the verified regenerated nozzle belongs, its corresponding application level is determined.
[0036] Specifically, the above parameter ranges of water pressure 0.2-0.4MPa and air pressure 0.15-0.5MPa cover the actual working intervals of the vast majority of air-water atomizing nozzles in the secondary cooling zone of continuous casting, and the calibration carried out under this working condition can truly reflect the operation state of the nozzle after being installed on the machine. The flow deviation ≤ ±5% ensures the precise control of the cooling water amount for the cast slab, avoiding uneven surface temperature of the cast slab caused by water amount fluctuation; the atomization angle deviation of 0° to 3° ensures the accuracy of the spray coverage area, preventing the occurrence of cooling blind zones or overlapping overcooling zones; no air leakage and no water leakage are the basic premise for the safe operation of the system. Only reconditioned nozzles that meet all the above quantitative indicators at the same time are judged to be qualified in calibration, and any item exceeding the standard requires re-disassembly and inspection or direct scrapping. This acceptance mechanism based on objective data eliminates the uncertainty of manual subjective judgment, and provides a reliable quality benchmark for subsequent graded applications.
[0037] As an implementation mode, the application grades include a normal application grade and a degraded application grade; when the category of the reconditioned nozzle is a degraded use part and the calibration is qualified, its application grade is determined as the degraded application grade, and the reconditioned nozzles of the degraded application grade are only allowed to be used in the secondary cooling weak cooling zone of continuous casting, and are prohibited from being put into the strong cooling section; when the category of the reconditioned nozzle is a repairable part and the calibration is qualified, its application grade is determined as the normal application grade; the reconditioned nozzles with determined application grades are sprayed with antirust agent, and pasted with exclusive repair marks containing the repair date, specification and model, and degradation category before being put into storage.
[0038] Specifically, the setting of the degraded application grade is a key strategy of the present application to balance resource utilization rate and production safety. Although the class B degraded use parts have passed the performance calibration after repair, their substrates have experienced slight deformation or local damage, and there may be residual stress or microstructure changes inside the material, so there are potential risks when they are subjected to high-strength thermal shock and mechanical vibration in the strong cooling section for a long time. Therefore, by strictly limiting their physical application scenarios to the weak cooling zone with lower cooling intensity and relatively mild working conditions, the remaining functional value is fully utilized, and the cast slab quality accidents caused by performance degradation are avoided. On the contrary, the class A repairable parts have no structural damage to the substrate, and can be completely restored to the brand-new standard after repair, so they are given the normal application grade and allowed to be used in all fan-shaped sections of the whole line. In addition, the exclusive repair mark is not only the basis for inventory management, but also an important means for on-site error prevention. By prominently marking information such as "degradation-B", it can effectively prevent operators from mistakenly installing degraded nozzles at key positions of the strong cooling section.
[0039] Example 5 This embodiment, based on Embodiment 1, further defines the integrity of the process flow and environmental boundaries to enhance the technical attributes of pure physical-mechanical repair. As one implementation method, before performing multi-stage physical synergistic cleaning on the nozzle components to be repaired, it also includes: using a high-pressure water jet at 70-90 MPa to perform a rough cleaning of the nozzle components to be repaired, removing thick layers of oxide scale and muddy scale from the surface. Specifically, this pretreatment step aims to solve the problem of uneven thickness of deposits on the surface of the downstream nozzles. After long-term service, the outer surface of continuous casting nozzles is often covered with a dense mixture of millimeters-sized oxide scale and muddy scale. If directly entering the dry ice blasting or ultrasonic cleaning process, it will not only rapidly consume expensive dry ice media, but also cause ultrasonic energy attenuation due to the excessive thickness of the dirt layer, reducing the micropore cleaning efficiency. The first step uses a high-pressure water jet of 70-90MPa to quickly remove macroscopic thick scale by utilizing the water wedge effect and shear force. This pressure range has been verified by engineering to effectively remove stubborn outer layer dirt while remaining within the safe threshold of the yield strength of the stainless steel substrate. This avoids the risk of plastic deformation of thin-walled flow channels due to excessive water pressure, thus creating homogenized operating conditions for subsequent precision cleaning.
[0040] As one implementation method, after multi-stage physical cleaning, dry compressed air is used to thoroughly purge the nozzle components to be repaired, ensuring that the flow channels and surfaces are free of water and dust. Specifically, this post-treatment step is a crucial closed loop for ensuring the storage stability and assembly quality of the regenerated nozzles. Since the cleaning medium contains pure water, if it remains in micro-flow channels or threaded gaps, it can easily induce pitting or electrochemical corrosion of stainless steel during storage. Furthermore, during subsequent assembly, moisture mixed with lubricating grease can cause grease emulsification failure. Dry compressed air purging utilizes the kinetic energy and low dew point characteristics of high-speed airflow to forcibly displace the liquid water film and suspended particles between blind holes and mating surfaces, ensuring that the components meet the dry and clean standards for immediate assembly or storage. It should be understood that although dry compressed air is preferred as the purging medium in this embodiment, nitrogen or other inert gases can also be used as alternatives, provided they have equivalent dehumidification and dust removal capabilities, as long as the cleanliness requirements of being oil-free, water-free, and dust-free are met.
[0041] To further clarify the technical boundaries of this application and support low cost and environmental protection, this embodiment makes the following exclusive limitations on the process media and environmental conditions: The cleaning media for multi-stage physical synergistic cleaning include only pure water, dry ice, and compressed air; the repair methods for mechanical defects include only mechanical grinding, tapping, cold straightening, and polishing. In the cleaning stage, the use of chemical pickling agents such as hydrochloric acid, nitric acid, and hydrofluoric acid, as well as various organic solvents, is completely eliminated, fundamentally eliminating the risk of intergranular corrosion of stainless steel and the cost of waste liquid treatment; in the repair stage, thermal processing processes such as laser cladding, argon arc welding, and plasma cladding are explicitly excluded, avoiding problems such as thermal deformation of the substrate, deterioration of metallographic structure, and residual stress concentration caused by local high temperature input. This combination of purely physical and mechanical methods means that the repair process does not require expensive environmental protection equipment and special welding equipment, significantly reducing the equipment investment threshold and operation and maintenance complexity.
[0042] Furthermore, the nozzle components to be repaired are made of stainless steel, and the multi-stage physical cleaning and mechanical defect repair are performed at room temperature. On the one hand, this avoids the carbide precipitation and corrosion resistance reduction that may be caused by heating cleaning or heat treatment, thus maintaining the original metallurgical properties of the material; on the other hand, room temperature operation eliminates the dependence on constant temperature workshops or heating devices, significantly reducing energy consumption. The entire repair process can be completed at ambient temperature, and together with the aforementioned pure media and pure mechanical limitations, a green, low-carbon, and highly economical regenerative repair technology system is constructed.
[0043] Example 6 To further verify the effectiveness and economy of the offline regeneration and repair method for continuous casting nozzles provided in this application in actual industrial production, the following description uses a project to repair secondary cooling nozzles for square-rectangular billet continuous casting at a steel plant as an example. In this application scenario, the objects to be repaired are 1320 air-water atomizing nozzles produced at the steel plant, all made of 316L stainless steel. Their service conditions have resulted in widespread accumulation of iron oxide scale, calcium and magnesium scale blockage, and varying degrees of mechanical damage. The project team strictly followed the process flow described in Examples 1 to 5 above, and carried out a complete set of regeneration and repair operations on this batch of nozzles, including damage classification and screening, multi-level physical synergistic cleaning, mechanical defect repair, interchangeable assembly, standardized assembly, and offline performance verification.
[0044] In the damage classification and screening step S100, a clear classification result was obtained by visually inspecting and initially inspecting the flow channels of 1320 nozzles that were taken off the production line. Among them, 324 nozzles, accounting for about 24.5%, were classified as repairable parts (Class A). These nozzles have intact substrates and only have defects such as scale buildup in the flow channels or nozzle blockage, which can be restored by cleaning. 740 nozzles, accounting for about 56.1%, were classified as degraded parts (Class B). These nozzles have localized damage such as slight impact deformation of the outer shell or small-scale collapse of the nozzle outline, but no material loss, and have the potential to be regenerated through mechanical repair and interchangeable parts. 256 nozzles, accounting for about 19.4%, were classified as directly scrapped parts (Class C). These nozzles were rejected due to irreversible structural damage such as substrate cracking, nozzle chipping and perforation, or severe corrosion. This grading data objectively reflects the distribution pattern of continuous casting nozzle damage after the line runs, indicating that more than 80% of the nozzles still have varying degrees of regeneration value, thus confirming the necessity of establishing a refined grading and screening mechanism to improve resource utilization.
[0045] After completing subsequent multi-stage physical cleaning, mechanical defect repair, and interchangeable assembly processes, the repair results were significant. For the 740 Class B downgraded parts, after cleaning, shaping, assembly, and rigorous offline performance testing, 472 nozzles ultimately met the qualification standards, achieving an actual reuse rate of 63.8% for Class B nozzles. Combined with the 324 fully repaired and qualified Class A nozzles, the overall reuse rate of this batch of 1320 nozzles reached 60.3%. This means that nearly 800 nozzles that might have been scrapped were put back into production, significantly reducing spare parts procurement costs. Regarding application and disposal, the 324 qualified Class A nozzles were marked as normal application grade and allowed normal online use in all fan-shaped sections of the continuous casting secondary cooling zone; the 472 qualified Class B nozzles were determined to be downgraded application grade and affixed with a special label containing "Repair-B (For Weak Cooling Zones)," strictly limiting their use to the weak cooling areas at the ends of fan-shaped sections and prohibiting their use in critical positions of the strong cooling sections; the remaining unqualified parts and Class C scrapped parts were collected and disposed of uniformly. This practical application case fully demonstrates that the application, through a purely mechanical collaborative cleaning and graded interchangeable grouping strategy, can maximize the residual value of used nozzles while ensuring machine safety, thus achieving a balance between technical feasibility and economic benefits.
[0046] The above description is merely a specific implementation of this application, but the scope of protection of this application is not limited thereto.
Claims
1. An offline regeneration and repair method for continuous casting nozzles, characterized in that, include: Multiple nozzle components that have undergone damage grading screening and full disassembly were obtained and are intended for repair. Multi-stage physical synergistic cleaning is performed on the nozzle components to be repaired to remove the attached substances from the nozzle components; Mechanical defects are repaired on the cleaned nozzle components to be repaired, and the repaired nozzle components are interchanged and reassembled based on the dimensional inspection results to obtain reconstituted nozzle components; The reconstituted nozzle components are assembled to obtain a regenerated nozzle, and the application level of the regenerated nozzle is determined based on the offline performance verification results.
2. The offline regeneration and repair method for continuous casting nozzles according to claim 1, characterized in that, The multi-stage physical cleaning process performed on the nozzle components to be repaired to remove adhering substances includes: Dry ice blasting cleaning is performed on the nozzle components to be repaired, using the low-temperature embrittlement and impact of dry ice particles to peel off the hard scale on the surface of the nozzle components to be repaired; The nozzle components to be repaired after dry ice blasting are subjected to ultrasonic vibration cleaning, which utilizes ultrasonic cavitation to remove loose impurities in the micropores of the nozzle components to be repaired. After ultrasonic cleaning, the nozzle components to be repaired are subjected to high-pressure pulse flushing, and a flexible unblocking tool is used to clear the blocked channels of the nozzle components to be repaired.
3. The offline regeneration and repair method for continuous casting nozzles according to claim 2, characterized in that, In the dry ice blasting cleaning process, the dry ice particles have a particle size of 0.8-1.2 mm and a blasting pressure of 0.5-0.7 MPa. The dry ice is blasted into the nozzle inlet, the inner cavity flow channel, and the vortex cavity. In the ultrasonic vibration cleaning process, the nozzle component to be repaired is placed in a room temperature pure water ultrasonic cleaning tank and vibrated for 20-30 minutes. In the high-pressure pulse flushing, high-pressure pure water with a pressure of 10-12MPa is used to pulse flush the water inlet, air inlet, mixing channel and atomizing micropore of the nozzle component to be repaired. The flexible unblocking tool includes nylon needles of different sizes and microfiber soft brushes, which are used to thoroughly clean the atomized micropores one by one.
4. The offline regeneration and repair method for continuous casting nozzles according to claim 1, characterized in that, The acquisition of multiple nozzle components to be repaired, after damage grading screening and full disassembly, includes: The continuous casting nozzles that come off the production line undergo a preliminary visual and flow channel inspection and are classified into repairable parts, downgraded parts, and directly scrapped parts. The repairable parts and the degraded parts are used as nozzles to be repaired, while the directly scrapped parts are discarded. The nozzle to be repaired is completely disassembled, and damaged and deformed vulnerable parts are removed to obtain the multiple nozzle components to be repaired; The repairable part is a nozzle with flow channel scaling or nozzle blockage and no structural damage to the substrate; the degraded part is a nozzle with slight local deformation and no material loss; the directly scrapped part is a nozzle with substrate cracking, nozzle chipping or perforation, or severe corrosion.
5. The offline regeneration and repair method for continuous casting nozzles according to claim 4, characterized in that, The mechanical defect repair of the nozzle components to be repaired after cleaning includes: For thread corrosion, use a standard tap or die of the corresponding specification to manually tap or thread the threads to remove rust and impurities from the thread surface; if the threads are chipped, stripped, or severely worn beyond tolerance, the corresponding parts should be scrapped directly. For wear on the sealing surface, use metallographic sandpaper to polish in stages and surface polishing paste to polish; if the wear depth of the sealing surface is greater than 0.2mm or there are penetrating scratches, the corresponding parts should be scrapped directly; For nozzle wear, use an ultra-fine polishing head and micro-orifice polishing compound for polishing and repair; if the nozzle diameter enlargement exceeds 8% of the original size, the corresponding parts are scrapped directly. For minor impacts and deformations to the casing, special tooling is used for cold straightening; if the deformation cannot be corrected, the corresponding parts are scrapped.
6. The offline regeneration and repair method for continuous casting nozzles according to claim 5, characterized in that, The repaired nozzle components are interchanged and reassembled based on the dimensional detection results to obtain reconstructed nozzle components, including: The key dimensions of the nozzle components to be repaired after repair are inspected, and the nozzle components that pass the inspection are collected as intact components. The intact parts are used to replace the damaged and unusable nozzle parts to be repaired, thus completing the interchangeable assembly. The assembly of the reconstituted nozzle components to obtain the regenerated nozzle includes: Apply high-temperature anti-seize grease and sealing grease to the threaded mating surfaces and sealing contact surfaces, replace with brand new standard seals, and assemble the reconstructed nozzle components according to the standard torque.
7. The offline regeneration and repair method for continuous casting nozzles according to claim 6, characterized in that, The process of determining the application level of the regenerating nozzle based on offline performance verification results includes: The regeneration nozzle was connected to a water-air test bench to simulate the actual working conditions of secondary cooling in continuous casting, and its performance was tested under a normal temperature clean water medium with a water pressure of 0.2-0.4MPa and an air pressure of 0.15-0.5MPa. The water flow rate, atomization angle, droplet uniformity, and water-air sealing performance of the regenerated nozzle were tested and compared with the standard parameters of a brand new nozzle. When the water flow deviation is less than or equal to ±5%, the atomization angle deviation is between 0° and 3°, there is no air or water leakage, and the atomization is uniform without deviation, the regeneration nozzle is deemed to be qualified. Based on the category of the repairable part or the degraded part to which the qualified regenerated nozzle belongs, its corresponding application level is determined.
8. The offline regeneration and repair method for continuous casting nozzles according to claim 7, characterized in that, The application levels include normal application levels and downgraded application levels; When the regenerated nozzle belongs to the category of the downgraded part and passes the inspection, its application level is determined to be the downgraded application level. The regenerated nozzle of the downgraded application level is only used in the weak cooling zone of the secondary cooling of continuous casting and is prohibited from being put into the strong cooling zone. When the regenerated nozzle belongs to the category of repairable parts and passes the inspection, its application level is determined to be the normal application level; After determining the application level, the regenerated nozzles are sprayed with rust inhibitor and affixed with a unique repair label containing the repair date, specifications, and downgrade category before being put into storage.
9. The offline regeneration and repair method for continuous casting nozzles according to claim 1, characterized in that, Before performing multi-stage physical synergistic cleaning on the nozzle components to be repaired, the method further includes: The nozzle components to be repaired are roughly cleaned using a high-pressure water jet with a pressure of 70-90MPa to remove the thick layer of oxide scale and muddy scale from the surface. After the multi-stage physical cleaning is completed, dry compressed air is used to blow the nozzle components to be repaired in all directions to ensure that there is no water or dust in the flow channel and on the surface.
10. The offline regeneration and repair method for continuous casting nozzles according to claim 1, characterized in that, The cleaning media for the multi-stage physical synergistic cleaning include only pure water, dry ice, and compressed air. The repair methods for mechanical defects include only mechanical grinding, tapping, cold straightening, and polishing. The nozzle component to be repaired is made of stainless steel, and the multi-stage physical synergistic cleaning and mechanical defect repair are performed at room temperature.