A fragrance-releasing porous titanium alloy and its preparation method

Porous titanium alloys were prepared by powder metallurgy, and combined with pore-forming agents and sintering processes to form a porous structure for loading fragrances. This solved the shortcomings of porous titanium alloys in fragrance slow release and realized the preparation of porous titanium alloys with excellent fragrance release persistence and structural stability.

CN123060094APending Publication Date: 2026-11-10SOUTH CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611455341.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing porous titanium alloys lack design options for carrying and slow-release volatile fragrances. Traditional aromatherapy carriers are deficient in terms of structural designability, mechanical strength, wear and corrosion resistance, and fragrance release persistence.

Method used

Using a powder metallurgy approach, a porous titanium alloy matrix is ​​prepared by mixing titanium-based powder with pore-forming agent powder, cold pressing, pore-forming agent dissolution, vacuum drying, and vacuum sintering. This matrix is ​​then immersed in fragrance to form a porous structure that supports the fragrance. The pore size and porosity are controlled to achieve adjustable fragrance release.

Benefits of technology

The prepared fragrance-releasing porous titanium alloy can continuously release fragrance in an open environment at room temperature, significantly prolonging the fragrance residue time, maintaining the corrosion resistance and structural stability of the titanium alloy, and expanding its application to high-end jewelry, personal wearable devices and home decoration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060094A_ABST
    Figure CN123060094A_ABST
Patent Text Reader

Abstract

This invention discloses a fragrance-releasing porous titanium alloy and its preparation method. The porous titanium alloy comprises a porous titanium alloy matrix with a porous structure and a fragrance loaded within the porous structure. The preparation method includes: mixing titanium-based powder with a pore-forming agent powder, cold-pressing, dissolving the pore-forming agent, vacuum drying, and vacuum sintering to obtain a porous titanium alloy matrix; immersing the matrix in a fragrance, utilizing its porous structure to load the fragrance; and removing free fragrance from the surface to obtain a porous titanium alloy capable of continuously releasing fragrance, i.e., a fragrance-releasing porous titanium alloy. This preparation method employs a powder metallurgy approach, offering advantages such as high freedom in component design, pore structure control, and mold shape customization. The fragrance-releasing porous titanium alloy prepared by this invention combines the corrosion resistance, structural stability, and fragrance-releasing function of titanium alloys, and can be used in high-end jewelry, personal wearable devices, home decoration, and other functional metal products requiring long-lasting fragrance release.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of titanium and titanium alloy materials and functional porous metal materials, specifically relating to a fragrance-releasing porous titanium alloy and its preparation method. Background Technology

[0002] Titanium alloys possess characteristics such as low density, high specific strength, good corrosion resistance, excellent surface texture, and excellent biocompatibility, and have been widely used in aerospace, biomedical, chemical equipment, and high-end consumer products. With the development of personal wearable devices, decorative materials, and healthy home products, titanium alloy materials, which combine metallic texture, structural stability, and added functions, have high application value.

[0003] Porous titanium alloys are an important type of porous metallic material. Compared to traditional casting or machining methods for preparing porous titanium alloys, powder metallurgy is more suitable for preparing titanium alloy components with complex shapes, lightweight construction, and adjustable pore parameters. Furthermore, by combining powder ratios, pore-forming agent parameters, mold shapes, and sintering processes, the composition, shape, and pore structure of porous titanium alloy components can be designed and prepared.

[0004] However, the existing functions of porous titanium alloys are mainly focused on lightweighting, filtration and separation, energy absorption, bio-tissue ingrowth, or mechanical support, with a lack of design and application as carriers and slow-release agents for volatile fragrances. On the other hand, current fragrance-emitting products typically take the form of aromatherapy plaster, ceramics, wood, aromatherapy tablets, or essential oil diffusers. While these carriers possess a certain capacity for fragrance adsorption and release, they still have limitations in terms of structural designability, mechanical strength, wear and corrosion resistance, and fragrance release persistence.

[0005] Therefore, there is an urgent need to provide a new type of functional metal material that combines the advantages of free forming of titanium-based powder metallurgy with the function of sustained release of fragrance. This material can maintain the excellent physical and chemical properties and high-end metallic appearance of titanium alloys, while utilizing the adjustable porous structure as the loading space for fragrance to achieve adjustable release of fragrance and long-lasting fragrance. Summary of the Invention

[0006] To overcome the shortcomings of existing technologies, the primary objective of this invention is to provide a method for preparing a fragrance-releasing porous titanium alloy. This method includes: mixing titanium-based powder with a pore-forming agent powder; cold-pressing, dissolving the pore-forming agent, vacuum drying, and vacuum sintering to obtain a porous titanium alloy matrix; immersing the matrix in fragrance, utilizing its porous structure to load the fragrance; and removing free fragrance from the surface to obtain a porous titanium alloy capable of continuously releasing fragrance, i.e., a fragrance-releasing porous titanium alloy. This preparation method, by controlling the pore-forming agent content, particle size, and sintering conditions, can obtain a porous titanium alloy matrix with adjustable pore size, porosity, and fragrance loading, thereby achieving the design of different fragrance release rates. Compared with traditional casting or machining methods for preparing porous titanium alloys, the preparation method of this invention adopts a powder metallurgy route, offering advantages such as high freedom in component design, pore structure control, and mold shape customization.

[0007] The second objective of this invention is to provide a porous titanium alloy with sustained-release fragrance. This porous titanium alloy solves the problems of low designability of existing fragrance carrier structures, insufficient appearance durability, poor fragrance release duration, and insufficient development of functional applications for porous titanium alloys. Compared with traditional fragrance carriers, the porous titanium alloy with sustained-release fragrance of this invention combines the corrosion resistance, structural stability, and sustained-release function of titanium alloys, and can be used in high-end jewelry, personal wearable devices, home decoration, and other functional metal products requiring long-lasting fragrance release.

[0008] The primary objective of this invention is achieved through the following technical solution:

[0009] A method for preparing a fragrance-slow-release porous titanium alloy includes the following steps:

[0010] (1) Powder mixing: Titanium-based powder and pore-forming agent powder are mixed in proportion and homogenized to prepare a uniformly mixed powder;

[0011] (2) Cold pressing: The mixed powder is loaded into a mold and cold pressed under inert gas protection to prepare a compact;

[0012] (3) Pore-forming agent dissolution and vacuum drying: The compact is immersed in a liquid medium to dissolve and remove the pore-forming agent powder, and then vacuum dried to obtain a titanium alloy billet with a porous structure, i.e., a porous titanium alloy billet.

[0013] (4) Vacuum sintering: Vacuum sintering is performed on the porous titanium alloy billet to obtain a porous titanium alloy matrix;

[0014] (5) Fragrance loading: The porous titanium alloy matrix is ​​immersed in fragrance to load the fragrance onto the porous titanium alloy matrix. After removing the porous titanium alloy matrix, the free fragrance on the surface is removed to prepare a fragrance-slow-release porous titanium alloy.

[0015] Preferably, in step (1), the titanium-based powder is selected from at least one of pure titanium powder and titanium alloy powder; the particle size of the titanium-based powder is 17~53 μm; the pore-forming agent powder is a water-soluble pore-forming agent powder that can be removed from the compact; the amount of pore-forming agent powder added is 7.8~13.8 wt.%, and the particle size of the pore-forming agent powder is 50~55 μm.

[0016] Preferably, the titanium alloy powder is at least one of α-type titanium alloy powder, near-α-type titanium alloy powder, α+β-type titanium alloy powder, and β-type titanium alloy powder.

[0017] Preferably, the pure titanium powder is TA1 or TA2 powder; the titanium alloy powder is at least one of TA15, TC4, TC11 or TB6 powder; more preferably, the titanium-based powder is TC4 powder.

[0018] Preferably, the water-soluble pore-forming agent powder is at least one of NaCl or KCl powder.

[0019] Preferably, the pore-forming agent powder is NaCl powder.

[0020] Preferably, in step (1), the powder mixing and homogenization are carried out under inert gas protection, the powder mixing speed is 250~350 r / min, and the time is 4~5 h.

[0021] Preferably, the powder is mixed at a speed of 300 r / min for 4 hours.

[0022] Preferably, in step (2), the pressure of the cold pressing is 300~400 MPa and the holding time is 30~60 s.

[0023] Preferably, in step (3), the liquid medium is purified water, preferably distilled water; the pore-forming agent dissolution temperature is 50~70℃, preferably 60℃, and the pore-forming agent dissolution time is 2~4 h; the vacuum drying temperature is 70~90℃, preferably 80℃, and the drying time is 8~12 h.

[0024] Preferably, in step (4), the temperature of vacuum sintering is 1200~1300℃ and the holding time is 4~6 h.

[0025] Preferably, in step (5), the fragrance is a single fragrance or a compound fragrance; the single fragrance is a natural fragrance or a synthetic fragrance; the compound fragrance is composed of a flavoring and at least one single fragrance; and the soaking time of the fragrance is 8 to 12 hours.

[0026] Preferably, when the fragrance is a natural fragrance, the natural fragrance is a plant essential oil or a natural fragrance raw material; when the fragrance is a synthetic fragrance, the synthetic fragrance is at least one of alcohols, phenols, ethers, esters, aldehydes, ketones and terpenes.

[0027] Preferably, the flavoring is at least one of thymol, menthol, eucalyptol, and eugenol.

[0028] The second objective of this invention is achieved by the following technical solution:

[0029] A fragrance-releasing porous titanium alloy is prepared by the above-described preparation method.

[0030] Preferably, the fragrance-releasing porous titanium alloy includes a porous titanium alloy matrix and a fragrance loaded within the pores of the porous titanium alloy matrix; the porous titanium alloy matrix has a porous structure, and the fragrance is loaded within the porous structure by immersion, enabling the fragrance-releasing porous titanium alloy to continuously release fragrance in an open environment at room temperature.

[0031] Preferably, the porous titanium alloy matrix is ​​prepared by mixing titanium-based powder and pore-forming agent powder, cold pressing, pore-forming agent dissolution, vacuum drying and vacuum sintering.

[0032] Preferably, the fragrance-releasing porous titanium alloy has an average pore size of 60-90 μm, a density of 55%-70%, and a fragrance loading of 0.50-0.80 g / cm³.

[0033] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0034] 1) The preparation method of the fragrance-releasing porous titanium alloy described in this invention differs from the method of simply coating fragrance onto a dense metal surface. Instead, a porous structure is formed in the titanium alloy matrix by using a pore-forming agent, so that the pores become the space for fragrance loading and slow release.

[0035] 2) The method for preparing the fragrance-releasing porous titanium alloy described in this invention can obtain a porous titanium alloy matrix with relatively controllable pore size and density by adjusting the amount of pore-forming agent added, particle size, cold pressing and sintering parameters, which is beneficial for controlling the fragrance loading and release stability.

[0036] 3) Compared with free fragrances, the fragrance-releasing porous titanium alloy of the present invention can significantly delay fragrance volatilization and exhibit a longer fragrance residue time and a higher fragrance residue rate in an open environment at room temperature;

[0037] 4) The method for preparing the fragrance-releasing porous titanium alloy described in this invention uses powder metallurgy to prepare porous titanium alloys. It can combine powder ratio, pore-forming agent parameters, mold shape and sintering process control to achieve the designable preparation of porous titanium alloy components in terms of composition, shape and pore structure.

[0038] 5) The fragrance-releasing porous titanium alloy described in this invention retains the characteristics of titanium alloys such as corrosion resistance, high strength and stable appearance, and can expand the application of titanium alloys in high-end jewelry, personal wearable devices, healthy home furnishings and functional decorative materials. Attached Figure Description

[0039] Figure 1 Image of the fragrance-releasing porous titanium alloy sample prepared in Example 1;

[0040] Figure 2 A scanning electron microscope image of the fragrance-releasing porous titanium alloy prepared in Example 1;

[0041] Figure 3 This is a scanning electron microscope image of the fragrance-releasing porous titanium alloy prepared in Example 2;

[0042] Figure 4 This is a scanning electron microscope image of the fragrance-releasing porous titanium alloy prepared in Example 3;

[0043] Figure 5 A scanning electron microscope image of the fragrance-releasing porous titanium alloy prepared in Example 4;

[0044] Figure 6 The graph shows the change in fragrance residue rate over time of the fragrance-releasing porous titanium alloys prepared in Examples 1 to 4 in an open environment at room temperature.

[0045] Figure 7 The graph shows the natural residual rate of the four free fragrances (thymol, menthol, eucalyptol, and eugenol) in Comparative Example 1 over time in an open environment at the same room temperature. Detailed Implementation

[0046] The present invention will be further described below with reference to embodiments and comparative examples, but the scope of protection of the present invention is not limited to the following embodiments. Without departing from the concept of the present invention, those skilled in the art can make appropriate adjustments to the type of titanium-based material, the amount of pore-forming agent, the type of fragrance, and the loading conditions.

[0047] Aroma Residue Rate Test Method

[0048] To evaluate the aroma sustained-release performance, the initial aroma loading in the sample on day 0 was taken as 100%. The sample was placed in an open environment at room temperature, and the amount of residual aroma in the sample was weighed or measured every 2 days. The aroma residue rate of the porous titanium alloy was calculated using the following formula:

[0049]

[0050] in, The mass of the porous titanium alloy matrix before fragrance loading. The initial mass after fragrance loading and removal of surface free fragrance. The sample mass is defined as t days after release. The free fragrance control group had its free fragrance mass on day 0 as 100%, and its natural residue rate was determined under the same environmental conditions. Three parallel samples were set up at each time point.

[0051] Example 1

[0052] A method for preparing a fragrance-slow-release porous titanium alloy includes the following steps:

[0053] 1) Powder mixing: TC4 powder and NaCl powder were prepared and mixed in proportion, wherein the amount of NaCl added was 7.8 wt.% and the average particle size was 50 μm; the mixture was carried out under inert gas protection at 300 r / min for 4 h to obtain a uniformly mixed powder.

[0054] 2) Cold pressing: The mixed powder is loaded into the mold cavity, argon gas is introduced into the mold cavity and then unidirectional cold pressing is performed. The cold pressing pressure is 300 MPa and the holding time is 30 s to obtain the pressed blank.

[0055] 3) Pore-forming agent dissolution and vacuum drying: The compact was completely immersed in distilled water at 60℃ and kept at that temperature for 2 h to allow the NaCl powder to dissolve and be removed, forming a porous structure; then the sample was placed in a vacuum drying oven at 80℃ and dried for 8 h to prepare a porous titanium alloy billet;

[0056] 4) Vacuum sintering: The porous titanium alloy billet is placed in a vacuum sintering furnace and held at 1200℃ for 4 h to obtain a porous titanium alloy matrix.

[0057] 5) Fragrance loading: The sintered porous titanium alloy matrix was completely immersed in liquid thymol for 10 hours. After immersion, the sample was removed and the free thymol on the surface was gently wiped off with filter paper to obtain thymol-loaded porous titanium alloy, i.e. fragrance slow-release porous titanium alloy.

[0058] The Archimedes displacement test showed that the sample had a density of 65.3%. Scanning electron microscopy revealed that the fragrance-releasing porous titanium alloy exhibited a uniform porous structure with an average pore size of 70 μm (see...). Figure 2 The thymol loading was calculated to be 0.57 g / cm³ by weighing. Aroma residue was tested in an open environment at room temperature; the results are shown below. Figure 6The aroma residue of the fragrance-slow-release porous titanium alloy (thymol-supported porous titanium alloy) remained at 30%~34% after 12 days, while free thymol was only 2%~4% after 4 days and almost completely evaporated after 6 days (see...). Figure 7 This indicates that the material of the present invention can significantly delay the volatilization of fragrances and improve the ability to retain aroma.

[0059] Example 2

[0060] A method for preparing a fragrance-slow-release porous titanium alloy includes the following steps:

[0061] 1) Powder mixing: TC4 powder and NaCl powder were mixed in proportion, with NaCl added at 10.7 wt.% and an average particle size of 52 μm; the mixture was carried out under inert gas protection at 300 r / min for 4.5 h to obtain a uniformly mixed powder.

[0062] 2) Cold pressing: The mixed powder is loaded into the mold cavity, argon gas is introduced into the mold cavity and then unidirectional cold pressing is performed. The cold pressing pressure is 320 MPa and the holding time is 40 s to obtain the pressed blank.

[0063] 3) Pore-forming agent dissolution and vacuum drying: The compact was completely immersed in distilled water at 60℃ and kept at that temperature for 2.5 h to allow NaCl to dissolve and be removed, forming a porous structure; then the sample was placed in a vacuum drying oven at 80℃ and dried for 9 h to prepare a porous titanium alloy billet.

[0064] 4) Vacuum sintering: The porous titanium alloy billet is placed in a vacuum sintering furnace and held at 1250℃ for 4.5 h to obtain a porous titanium alloy matrix;

[0065] 5) Fragrance loading: The sintered porous titanium alloy matrix was completely immersed in liquid menthol for 10 hours. After immersion, the sample was removed and the free menthol on the surface was gently wiped off with filter paper to obtain menthol-loaded porous titanium alloy, i.e. fragrance slow-release porous titanium alloy.

[0066] The Archimedes displacement method test showed that the sample had a density of 64.7%. Scanning electron microscopy revealed that the material exhibited a uniform porous structure with an average pore size of 75 μm (see...). Figure 3 The menthol loading was calculated to be 0.63 g / cm³ by weighing. Aroma residue was tested in an open environment at room temperature; the results are shown below. Figure 6 The aroma residue of the fragrance-releasing porous titanium alloy (menthol-supported porous titanium alloy) remained at 19%~22% after 12 days, while free menthol was only 3%~7% after 2 days and almost completely evaporated after 4 days (see...). Figure 7 This indicates that the material of the present invention can significantly delay the volatilization of fragrances and improve the ability to retain aroma.

[0067] Example 3

[0068] A method for preparing a fragrance-slow-release porous titanium alloy includes the following steps:

[0069] 1) Powder mixing: TC4 powder and NaCl powder were mixed in proportion, with NaCl added at 12.3 wt.% and an average particle size of 54 μm; the mixture was carried out under inert gas protection at 300 r / min for 4.8 h to obtain a uniformly mixed powder.

[0070] 2) Cold pressing: The mixed powder is loaded into the mold cavity, argon gas is introduced into the mold cavity and then unidirectional cold pressing is performed. The cold pressing pressure is 380 MPa and the holding time is 45 s to obtain the pressed blank.

[0071] 3) Pore-forming agent dissolution and vacuum drying: The compact was completely immersed in distilled water at 60℃ and kept at that temperature for 3 h to allow NaCl to dissolve and be removed, forming a porous structure; then the sample was placed in a vacuum drying oven at 80℃ and dried for 10 h to prepare a porous titanium alloy billet.

[0072] 4) Vacuum sintering: The porous titanium alloy billet is placed in a vacuum sintering furnace and held at 1270 ℃ for 4.8 h to obtain a porous titanium alloy matrix;

[0073] 5) Fragrance loading: The sintered porous titanium alloy matrix was completely immersed in liquid eucalyptol for 10 h. After immersion, the sample was taken out and the free eucalyptol on the surface was gently wiped off with filter paper to obtain eucalyptol loaded porous titanium alloy, i.e. fragrance slow-release porous titanium alloy.

[0074] The Archimedes displacement method test showed that the sample had a density of 63.5%. Scanning electron microscopy revealed that the material exhibited a uniform porous structure with an average pore size of 78 μm (see...). Figure 4 The eucalyptol loading was calculated to be 0.69 g / cm³ by weighing. Aroma residue was tested in an open environment at room temperature; the results are shown below. Figure 6 The aroma residue of the fragrance-slow-release porous titanium alloy (eucalyptol-loaded porous titanium alloy) remained at 11%~14% after 12 days, while free eucalyptol was only 1%~3% after 2 days and almost completely evaporated after 4 days (see...). Figure 7 This indicates that the material of the present invention can significantly delay the volatilization of fragrances and improve the ability to retain aroma.

[0075] Example 4

[0076] A method for preparing a fragrance-slow-release porous titanium alloy includes the following steps:

[0077] 1) Powder mixing: TC4 powder and NaCl powder were mixed in proportion, with NaCl added at 13.8 wt.% and an average particle size of 55 μm; the mixture was carried out under inert gas protection at 300 r / min for 5 h to obtain a uniformly mixed powder.

[0078] 2) Cold pressing: The mixed powder is loaded into the mold cavity, argon gas is introduced into the mold cavity and then unidirectional cold pressing is performed. The cold pressing pressure is 400 MPa and the holding time is 60 s to obtain the pressed blank.

[0079] 3) Pore-forming agent dissolution and vacuum drying: The compact was completely immersed in distilled water at 60℃ and kept at that temperature for 4 h to allow NaCl to dissolve and be removed, forming a porous structure; then the sample was placed in a vacuum drying oven at 80℃ and dried for 12 h to prepare a porous titanium alloy billet.

[0080] 4) Vacuum sintering: The porous titanium alloy billet is placed in a vacuum sintering furnace and held at 1300 ℃ for 6 h to obtain a porous titanium alloy matrix;

[0081] 5) Fragrance loading: The sintered porous titanium alloy matrix was completely immersed in liquid eugenol for 10 h. After immersion, the sample was taken out and the free eugenol on the surface was gently wiped off with filter paper to obtain eugenol-loaded porous titanium alloy, i.e. fragrance slow-release porous titanium alloy.

[0082] The Archimedes displacement method test showed that the sample had a density of 59.6%. Scanning electron microscopy revealed that the material exhibited a uniform porous structure with an average pore size of 81 μm (see...). Figure 5 The eugenol loading was calculated to be 0.72 g / cm³ by weighing. Aroma residue was tested in an open environment at room temperature; the results are shown below. Figure 6 The aroma residue of the fragrance-slow-release porous titanium alloy (eugenol-supported porous titanium alloy) remained at 48%–51% after 12 days, while free eugenol was only 6%–8% after 12 days (see [link to product description]). Figure 7 This indicates that the material of the present invention can significantly delay the volatilization of fragrances and improve the ability to retain aroma.

[0083] Comparative Example 1

[0084] To evaluate the effect of the porous titanium alloy matrix on fragrance volatilization behavior, thymol, menthol, eucalyptol, and eugenol, corresponding to those in Examples 1-4, were used as free fragrance controls. Natural volatilization experiments were conducted in the same open environment at room temperature as the samples supported on the porous titanium alloy. With day 0 as 100% fragrance mass, the remaining fragrance mass was measured at the same time intervals as in the examples, and its natural residue rate was calculated. The results are as follows: Figure 7As shown, compared with free fragrances, fragrances loaded in the pores of porous titanium alloy all exhibited a significantly delayed mass loss process, indicating that the porous structure can provide storage space for fragrances and reduce the effective volatilization rate of fragrances directly exposed to the open environment.

[0085] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A method for preparing a fragrance-slow-release porous titanium alloy, characterized in that, Includes the following steps, (1) Powder mixing: Titanium-based powder and pore-forming agent powder are mixed in proportion and homogenized to prepare a uniformly mixed powder; (2) Cold pressing: The mixed powder is loaded into a mold and cold pressed under inert gas protection to prepare a compact; (3) Pore-forming agent dissolution and vacuum drying: The compact is immersed in a liquid medium to dissolve and remove the pore-forming agent powder, and then vacuum dried to obtain a titanium alloy billet with a porous structure, i.e., a porous titanium alloy billet. (4) Vacuum sintering: Vacuum sintering is performed on the porous titanium alloy billet to obtain a porous titanium alloy matrix; (5) Fragrance loading: The porous titanium alloy matrix is ​​immersed in fragrance to load the fragrance onto the porous titanium alloy matrix. After removing the porous titanium alloy matrix, the free fragrance on the surface is removed to prepare a fragrance-slow-release porous titanium alloy.

2. The method for preparing the fragrance-releasing porous titanium alloy according to claim 1, characterized in that, In step (1), the titanium-based powder is selected from at least one of pure titanium powder and titanium alloy powder; the particle size of the titanium-based powder is 17~53 μm; the pore-forming agent powder is a water-soluble pore-forming agent powder that can be removed from the compact; the amount of pore-forming agent powder added is 7.8~13.8 wt.%, and the particle size of the pore-forming agent powder is 50~55 μm.

3. The method for preparing the fragrance-releasing porous titanium alloy according to claim 2, characterized in that, The titanium alloy powder is at least one of α-type titanium alloy powder, near-α-type titanium alloy powder, α+β-type titanium alloy powder, and β-type titanium alloy powder.

4. The method for preparing the fragrance-releasing porous titanium alloy according to claim 1, characterized in that, The water-soluble pore-forming agent powder is at least one of NaCl or KCl powder.

5. The method for preparing the fragrance-releasing porous titanium alloy according to claim 1, characterized in that, In step (5), the fragrance is a single fragrance or a compound fragrance; the single fragrance is a natural fragrance or a synthetic fragrance; the compound fragrance is composed of a flavoring and at least one single fragrance; the soaking time of the fragrance is 8 to 12 hours.

6. The method for preparing the fragrance-releasing porous titanium alloy according to claim 5, characterized in that, When the fragrance is a natural fragrance, the natural fragrance is a plant essential oil or a natural fragrance raw material; when the fragrance is a synthetic fragrance, the synthetic fragrance is at least one of alcohols, phenols, ethers, esters, aldehydes, ketones and terpenes.

7. The method for preparing the fragrance-releasing porous titanium alloy according to claim 5, characterized in that, The fragrance is at least one of thymol, menthol, eucalyptol, and eugenol.

8. A fragrance-releasing porous titanium alloy, characterized in that, It is prepared according to any one of claims 1 to 7.

9. The fragrance-releasing porous titanium alloy according to claim 8, characterized in that, The fragrance-releasing porous titanium alloy includes a porous titanium alloy matrix and a fragrance loaded within the pores of the porous titanium alloy matrix; the porous titanium alloy matrix has a porous structure, and the fragrance is loaded within the porous structure by immersion, enabling the fragrance-releasing porous titanium alloy to continuously release fragrance in an open environment at room temperature.

10. The fragrance-releasing porous titanium alloy according to any one of claims 8 or 9, characterized in that, The fragrance-releasing porous titanium alloy has an average pore size of 60~90 μm, a density of 55%~70%, and a fragrance loading of 0.50~0.80 g / cm³.