A spherical low-sodium aluminum hydroxide powder, its preparation method, and its applications
By controlling the pH and temperature of the urea-aluminum sulfate mixed solution, combined with gradient slow cooling temperature control and low shear force stirring, spherical low-sodium aluminum hydroxide powder was prepared in situ, solving the problems of irregular morphology and high sodium oxide content in the existing technology, and improving thermal conductivity and insulation performance.
Patent Information
- Application Number
- CN202611321039.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies make it difficult to prepare near-spherical low-sodium aluminum hydroxide powder in situ, resulting in irregular particle morphology, low stacking efficiency, difficulty in constructing thermally conductive networks, and high sodium oxide content affecting insulation and processing performance.
By controlling the pH and temperature with a urea-aluminum sulfate mixed solution, combined with gradient slow cooling temperature control and low shear force stirring, spherical low-sodium aluminum hydroxide powder was prepared in situ through steps such as cyclone classification, solid-liquid separation, washing and drying.
In-situ growth of near-spherical low-sodium aluminum hydroxide powder was achieved, which improved stacking efficiency and thermal conductivity, reduced sodium oxide content, and enhanced insulation and processing performance.
Smart Images

Figure CN123061982A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of inorganic non-metallic materials technology, and in particular to a spherical low-sodium aluminum hydroxide powder, its preparation method, and its application. Background Technology
[0002] With the rapid development of the Internet of Things, artificial intelligence, and new energy vehicle power battery technology, the integration and power density of electronic components continue to increase, making thermally conductive and heat-dissipating materials crucial for solving thermal management problems. Composite materials with polymer matrix and thermally conductive powder as filler phase have become the mainstream thermally conductive and heat-dissipating solution due to their ease of processing and structural designability. Among inorganic non-metallic thermally conductive fillers, aluminum hydroxide is widely used in low-wattage thermally conductive material systems due to its advantages of flame retardancy, insulation, thermal conductivity, and low cost.
[0003] However, existing technologies for preparing aluminum hydroxide powder have significant limitations in application: First, irregular particle morphology and prominent edges lead to low packing efficiency and difficulty in continuously constructing thermally conductive networks, thus limiting the improvement of the thermal conductivity of composite materials. Second, irregular morphology increases system viscosity and degrades processing performance, failing to meet high-filling requirements. Third, high sodium oxide content reduces high-temperature insulation performance and triggers alkali corrosion. Fourth, excessive oil absorption increases resin consumption and degrades interfacial bonding. Although post-processing methods such as mechanical rounding, melt granulation, and spray molding can improve sphericity to some extent, these methods are all post-particle shaping processes, which easily cause grain breakage, increased lattice defects, sodium content rebound, and decreased purity. Moreover, the processes are lengthy and costly, making it difficult to achieve in-situ controllable synthesis of thermally conductive aluminum hydroxide powder with near-spherical morphology, low sodium content, low oil absorption, and high filler compatibility. Currently, there is a significant gap in the core technology for in-situ growth and molding of near-spherical low-sodium aluminum hydroxide powder. Summary of the Invention
[0004] This application provides a spherical low-sodium aluminum hydroxide powder, its preparation method, and its application, to solve the following technical problem: how to prepare spherical low-sodium aluminum hydroxide powder in situ without the need for a post-particle shaping process.
[0005] In a first aspect, embodiments of this application provide a method for preparing spherical low-sodium aluminum hydroxide powder, comprising the following steps: Urea solution is added to aluminum sulfate solution and mixed to obtain urea-aluminum sulfate mixed solution; At a temperature of 40℃~60℃, refined sodium aluminate solution is added to the urea-aluminum sulfate mixed solution until the pH value of the urea-aluminum sulfate mixed solution is 7~10; The urea-aluminum sulfate mixed solution with a pH of 7-10 is chemically reacted at a temperature of 80-90°C for 2-4 hours to obtain a spherical aluminum hydroxide microcrystalline slurry. The spherical aluminum hydroxide microcrystalline slurry was added as a seed crystal to a refined sodium aluminate solution for seed crystal decomposition to obtain aluminum hydroxide slurry. The seed crystal decomposition adopted a gradient slow cooling temperature control method, with an initial decomposition temperature of 65℃~80℃ and a decomposition termination temperature of 53℃~55℃. The seed crystal decomposition adopted a low shear force stirring method. The aluminum hydroxide slurry is subjected to hydrocyclone classification to obtain coarse-particle aluminum hydroxide slurry and fine-particle aluminum hydroxide slurry. The coarse-particle-size aluminum hydroxide slurry is subjected to solid-liquid separation to obtain aluminum hydroxide filter cake; The aluminum hydroxide filter cake is washed and dried; the washing is carried out in a hot water synergistic ammonium salt system for deep sodium removal; The dried aluminum hydroxide filter cake is subjected to dry classification to remove large particles and obtain spherical low-sodium aluminum hydroxide powder.
[0006] Optionally, the concentration of the urea solution is 40 g / L to 70 g / L, and the concentration of the aluminum sulfate solution is 40 g / L to 70 g / L.
[0007] Optionally, the urea in the urea solution and the Al in the aluminum sulfate solution... 3+ The molar ratio is 10:1 to 12:1.
[0008] Optionally, the refined sodium aluminate solution is prepared from industrial aluminum hydroxide or bauxite through alkali dissolution, lime slurry purification, deep filtration, and impurity removal and desilication processes; The alumina concentration of the refined sodium aluminate solution is 70 g / L to 140 g / L, and the caustic ratio αK is 1.4 to 2.5.
[0009] Optionally, the initial seed ratio for the seed crystal decomposition is 5%, the decomposition time is 48h to 72h, and the decomposition solid content is 200g / L to 500g / L.
[0010] Optionally, the stirring speed of the low shear force stirring method is not higher than 250 r / min.
[0011] Optionally, the ammonium salt in the hot water-assisted ammonium salt deep desodiumning process is at least one of ammonium acetate, ammonium chloride, and ammonium sulfate, and the amount of the ammonium salt used is 100 ppm to 300 ppm.
[0012] Optionally, the dry classification adopts an airflow classification process; The fine-particle aluminum hydroxide obtained by dry classification is packaged as a thermally conductive, spherical, low-sodium aluminum hydroxide product, while the coarse-particle aluminum hydroxide obtained by dry classification is used for catalysis.
[0013] Secondly, embodiments of this application provide a spherical low-sodium aluminum hydroxide powder, which is prepared by the preparation method described in any one of the first aspects; The spherical low-sodium aluminum hydroxide powder has an in-situ grown spherical particle morphology. The spherical low-sodium aluminum hydroxide powder has a sodium oxide mass fraction of no more than 0.1 wt%, a median particle size D50 of 40 μm to 75 μm, and an oil absorption rate of no more than 22 mL / 100 g.
[0014] Thirdly, embodiments of this application provide an application of the spherical low-sodium aluminum hydroxide powder described in the second aspect as a thermally conductive filler, characterized in that the spherical low-sodium aluminum hydroxide powder is used as an inorganic thermally conductive and insulating filler in thermally conductive silicone, epoxy thermally conductive potting compound, thermally conductive modified plastic, and heat dissipation polymer composite material for power batteries of new energy vehicles.
[0015] The technical solutions provided in this application have the following advantages compared with the prior art: Urea solution is added to aluminum sulfate solution and mixed to obtain urea-aluminum sulfate mixed solution. This urea-aluminum sulfate mixed solution provides a uniform ionic environment for the subsequent preparation of spherical aluminum hydroxide microcrystalline slurry, thereby ensuring that the reaction between aluminate ions and aluminum ions in the solution proceeds uniformly after the addition of refined sodium aluminate solution.
[0016] At a temperature of 40℃ to 60℃, a refined sodium aluminate solution is added to the urea-aluminum sulfate mixed solution until the pH value of the urea-aluminum sulfate mixed solution is 7 to 10. This temperature range and pH range synergistically control the nucleation rate and morphological orientation of aluminum hydroxide microcrystals, so that aluminum hydroxide microcrystals are uniformly precipitated in the urea-aluminum sulfate mixed solution and form quasi-spherical initial crystal nuclei, thereby obtaining a suspension system containing quasi-spherical initial crystal nuclei.
[0017] The urea-aluminum sulfate mixed solution with a pH of 7-10 is chemically reacted at 80-90°C for 2-4 hours. This heating process promotes the crystallization and surface reconstruction of the spherical initial crystal nuclei, making the surface of the microcrystalline particles in the spherical aluminum hydroxide microcrystalline slurry smooth, the edges blunted, and the crystals complete, thus obtaining a spherical aluminum hydroxide microcrystalline slurry that can be used as a template for subsequent crystal seed decomposition.
[0018] Spherical aluminum hydroxide microcrystalline slurry was added as seed crystals to a refined sodium aluminate solution for seed crystal decomposition. This seed crystal decomposition adopted a gradient slow cooling temperature control method, with an initial decomposition temperature of 65℃~80℃ and a decomposition termination temperature of 53℃~55℃. This gradient slow cooling temperature control method allows the supersaturation of the sodium aluminate solution to be released steadily and slowly, avoiding explosive nucleation that would cause lattice defects to be encapsulated by sodium ions. At the same time, it allows the newly formed aluminum hydroxide to be uniformly deposited, directionally grown, and have its edges blunted on the surface of the microcrystals in the spherical aluminum hydroxide microcrystalline slurry, thus obtaining an aluminum hydroxide slurry with morphology that inherits the spherical characteristics of the seed crystals and has a controlled sodium content.
[0019] The seed crystal decomposition adopts a low-shear stirring method, which reduces the fluid shear force and prevents the crystals in the aluminum hydroxide slurry from breaking, being scratched at the edges, and generating secondary fine powder due to strong shear, thereby ensuring the integrity and spherical regularity of the particles in the aluminum hydroxide slurry.
[0020] Aluminum hydroxide slurry is subjected to cyclone classification to obtain coarse-particle-size aluminum hydroxide slurry and fine-particle-size aluminum hydroxide slurry. This cyclone classification process classifies the aluminum hydroxide slurry according to the particle size difference to ensure particle size uniformity, thereby obtaining a coarse-particle-size aluminum hydroxide slurry with a concentrated particle size distribution.
[0021] A coarse-particle-size aluminum hydroxide slurry is subjected to solid-liquid separation to obtain an aluminum hydroxide filter cake. This solid-liquid separation separates the solid phase of aluminum hydroxide from the liquid phase in the coarse-particle-size aluminum hydroxide slurry, thereby obtaining an aluminum hydroxide filter cake to be washed.
[0022] The aluminum hydroxide filter cake is washed and dried. The washing process involves deep sodium removal in a hot water-assisted ammonium salt system. This system relies on hot water to activate the pores of aluminum hydroxide to release the coated alkali or lattice alkali, and then replaces the sodium ions on the surface or inside the aluminum hydroxide filter cake through ammonium ion exchange, thereby obtaining a dry aluminum hydroxide filter cake with a sodium oxide content of no more than 0.1 wt%.
[0023] The dried aluminum hydroxide filter cake is subjected to dry classification to remove large particles. This dry classification adopts an air classifier process, which separates particles according to particle size based on aerodynamic principles, thereby obtaining spherical low-sodium aluminum hydroxide powder with controllable particle size and regular morphology. Attached Figure Description
[0024] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.
[0025] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0026] Figure 1 This is a scanning electron microscope image of the microcrystalline particles in the spherical aluminum hydroxide microcrystalline slurry in the embodiments of this application; Figure 2 Scanning electron microscope image of the spherical low-sodium aluminum hydroxide powder prepared by the method described in the embodiments of this application; Figure 3 This is a scanning electron microscope image of thermally conductive aluminum hydroxide powder in the prior art. Detailed Implementation
[0027] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0028] The range descriptions used herein, such as numerical ranges and proportional ranges, include all possible sub-ranges and single numerical values within that range. For example, the range descriptions of "1 to 5" or "1~5" cover all sub-ranges (such as 1 to 3, 2 to 4, etc.) and single numbers (such as 1, 2, 3, 4, 4, 5) between 1 and 5. Unless otherwise specified, the terms "including" and "contains" as used herein mean "including but not limited to"; relational terms such as "first" and "second" are used only to distinguish different entities or operations and do not imply an actual order or relationship; "and / or" indicates that multiple situations can exist individually or simultaneously; expressions such as "at least one," "multiple," and "at least one" refer to any combination of the corresponding objects, including combinations of single or multiple objects. The proportional relationships mentioned herein, such as mass ratios and molar ratios, should be understood as the correspondence between the first and second terms of a proportional formula, according to the order of description. The raw materials, reagents, instruments, and equipment used herein can all be obtained through commercial purchase or prepared using existing methods.
[0029] In a first aspect, embodiments of this application provide a method for preparing spherical low-sodium aluminum hydroxide powder, comprising the following steps: Urea solution is added to aluminum sulfate solution and mixed to obtain urea-aluminum sulfate mixed solution; At a temperature of 40℃~60℃, refined sodium aluminate solution is added to the urea-aluminum sulfate mixed solution until the pH value of the urea-aluminum sulfate mixed solution is 7~10; The urea-aluminum sulfate mixed solution with a pH of 7-10 is chemically reacted at a temperature of 80-90°C for 2-4 hours to obtain a spherical aluminum hydroxide microcrystalline slurry. The spherical aluminum hydroxide microcrystalline slurry was added as a seed crystal to a refined sodium aluminate solution for seed crystal decomposition to obtain aluminum hydroxide slurry. The seed crystal decomposition adopted a gradient slow cooling temperature control method, with an initial decomposition temperature of 65℃~80℃ and a decomposition termination temperature of 53℃~55℃. The seed crystal decomposition adopted a low shear force stirring method. The aluminum hydroxide slurry is subjected to hydrocyclone classification to obtain coarse-particle aluminum hydroxide slurry and fine-particle aluminum hydroxide slurry. The coarse-particle-size aluminum hydroxide slurry is subjected to solid-liquid separation to obtain aluminum hydroxide filter cake; The aluminum hydroxide filter cake is washed and dried; the washing is carried out in a hot water synergistic ammonium salt system for deep sodium removal; The dried aluminum hydroxide filter cake is subjected to dry classification to remove large particles and obtain spherical low-sodium aluminum hydroxide powder.
[0030] Spherical aluminum hydroxide microcrystalline slurry: refers to a suspension system containing spherical aluminum hydroxide microcrystalline particles. Refined sodium aluminate solution: refers to an aqueous solution of sodium aluminate prepared from industrial aluminum hydroxide or bauxite through alkali dissolution, lime slurry purification, deep filtration, and impurity removal and desilication processes. Gradient slow cooling temperature control: refers to a temperature control method that uses uniform, stepwise slow cooling and stable release of supersaturation throughout the entire seed crystal decomposition process. Low shear force stirring method: refers to a stirring method that uses a low-speed, low-disturbance axial flow gentle stirring mode throughout the entire aluminum hydroxide crystal growth stage to reduce fluid shear force. Hot water synergistic ammonium salt system: refers to a system that uses high-temperature hot water combined with an ammonium salt compound system to soak, wash, and remove sodium from the graded powder during the washing process. Dry classification: refers to the process of particle size classification of dried aluminum hydroxide filter cake using an airflow classification process. Large particles: refers to coarse aluminum hydroxide particles that exceed the upper limit of the controllable particle size range (75μm) of the finished product, which are spherical low-sodium aluminum hydroxide for thermal conductivity, during the dry classification process.
[0031] Temperature parameters (40℃~60℃): If the temperature is below 40℃, the reactivity between urea and aluminum sulfate is insufficient, the nucleation rate of microcrystals in the spherical aluminum hydroxide microcrystalline slurry is too slow, resulting in insufficient seed crystals. The template effect of directional deposition of aluminum hydroxide is weakened during the subsequent seed crystal decomposition process, and the sphericity of the spherical low-sodium aluminum hydroxide powder decreases. If the temperature is above 60℃, the nucleation rate is too fast, the microcrystal size distribution in the spherical aluminum hydroxide microcrystalline slurry becomes wider, the regularity of the seed crystal morphology decreases, the edge passivation effect is worse during the subsequent seed crystal decomposition process, and the morphological uniformity of the spherical low-sodium aluminum hydroxide powder deteriorates.
[0032] pH value parameter (7-10): If the pH value is below 7, the urea-aluminum sulfate mixed solution is acidic, and the aluminate ions in the sodium aluminate solution exist in the form of soluble ions, which cannot effectively precipitate aluminum hydroxide microcrystals, resulting in insufficient seed yield in the spherical aluminum hydroxide microcrystal slurry; if the pH value is above 10, the urea-aluminum sulfate mixed solution is too alkaline, the nucleation and growth of aluminum hydroxide microcrystals lose controllability, the microcrystals in the spherical aluminum hydroxide microcrystal slurry are severely agglomerated, and the template effect fails in the subsequent seed decomposition process.
[0033] Reaction temperature parameters (80℃~90℃): If the reaction temperature is below 80℃, the crystallization degree of the microcrystals in the spherical aluminum hydroxide microcrystalline slurry is insufficient, the surface defects of the seed crystals increase, and the interface quality of the directional deposition of aluminum hydroxide decreases during the subsequent seed crystal decomposition process; if the reaction temperature is above 90℃, the microcrystals in the spherical aluminum hydroxide microcrystalline slurry undergo Ostwald ripening, the seed crystal size is too large, the specific surface area decreases during the subsequent seed crystal decomposition process, and the number of seed crystals is insufficient.
[0034] Reaction time parameters (2h~4h): If the reaction time is less than 2h, the crystallization integrity of the microcrystals in the spherical aluminum hydroxide microcrystalline slurry is insufficient, the distribution of active sites on the seed surface is uneven, and the uniformity of directional deposition of aluminum hydroxide decreases during the subsequent seed decomposition process; if the reaction time exceeds 4h, the microcrystals in the spherical aluminum hydroxide microcrystalline slurry grow excessively, the seed particle size exceeds the controllable range, and the particle size control precision decreases during the subsequent seed decomposition process.
[0035] Initial decomposition temperature parameters (65℃~80℃): If the initial decomposition temperature is below 65℃, the supersaturation of the sodium aluminate solution during seed crystal decomposition will be too high, increasing the risk of explosive nucleation, increasing the fine powder content in the aluminum hydroxide slurry, and decreasing the particle size uniformity of the spherical low-sodium aluminum hydroxide powder; if the initial decomposition temperature is above 80℃, the supersaturation of the sodium aluminate solution during seed crystal decomposition will be too low, the decomposition rate will be too slow, the seed crystals in the aluminum hydroxide slurry will not agglomerate sufficiently, and the sphericity of the spherical low-sodium aluminum hydroxide powder will decrease.
[0036] Decomposition termination temperature parameter (53℃~55℃): If the decomposition termination temperature is below 53℃, the viscosity of the sodium aluminate solution at the end of the seed crystal decomposition will increase, the crystal growth in the aluminum hydroxide slurry will be limited, and the proportion of fine powder will increase; if the decomposition termination temperature is above 55℃, the stability of the sodium aluminate solution at the end of the seed crystal decomposition will be too high, the decomposition will be incomplete, the residual alumina content in the aluminum hydroxide slurry will increase, and the yield of spherical low-sodium aluminum hydroxide powder will decrease.
[0037] Examples of temperatures between 40℃ and 60℃ include, but are not limited to: 40℃, 45℃, 50℃, 55℃, and 60℃. Examples of pH values between 7 and 10 include, but are not limited to: 7, 7.5, 8, 8.5, 9, 9.5, and 10. Examples of temperatures between 80℃ and 90℃ include, but are not limited to: 80℃, 82℃, 85℃, 88℃, and 90℃. Examples of time periods between 2 hours and 4 hours include, but are not limited to: 2 hours, 2.5 hours, 3 hours, 3.5 hours, and 4 hours. Examples of initial decomposition temperatures between 65℃ and 80℃ include, but are not limited to: 65℃, 68℃, 70℃, 73℃, 75℃, 78℃, and 80℃. Examples of decomposition termination temperatures between 53℃ and 55℃ include, but are not limited to: 53℃, 53.5℃, 54℃, 54.5℃, and 55℃.
[0038] This application relates to the field of inorganic non-metallic materials technology, and in particular to a near-spherical low-sodium aluminum hydroxide powder, its preparation method, and its applications. Existing technologies rely on post-particle shaping processes such as mechanical rounding, melt granulation, or spray molding to improve the morphology of aluminum hydroxide powder. These post-shaping processes are all non-in-situ treatments, resulting in problems such as grain breakage, increased lattice defects, sodium content rebound, and lengthy process flows. The embodiments of this application utilize an integrated synergistic strategy of in-situ preparation of near-spherical aluminum hydroxide microcrystalline slurry and directional growth of seed crystals. This eliminates the need for post-particle shaping processes, allowing for controlled nucleation and growth of aluminum hydroxide, directly synthesizing near-spherical low-sodium aluminum hydroxide powder in situ. This overcomes the technical bottleneck of existing technologies that rely on post-processing modification.
[0039] In some embodiments, the concentration of the urea solution is 40 g / L to 70 g / L, and the concentration of the aluminum sulfate solution is 40 g / L to 70 g / L.
[0040] The concentrations of the urea solution and the aluminum sulfate solution are controlled within the range of 40 g / L to 70 g / L. This concentration range ensures that the molar ratio of urea molecules to aluminum ions in the urea-aluminum sulfate mixed solution is within a controllable range. This allows the concentration of the morphology regulator and the aluminum source supply to be matched in a coordinated manner during the preparation of the spherical aluminum hydroxide microcrystalline slurry, thereby ensuring that the nucleation density and sphericity induction effect of the microcrystals in the spherical aluminum hydroxide microcrystalline slurry are within the optimized range.
[0041] This concentration synergistic control ensures that the microcrystalline particles in the near-spherical aluminum hydroxide microcrystalline slurry have smooth surfaces, uniform particle sizes, and complete crystallization. This ensures that when the microcrystalline slurry is added as a seed crystal to a refined sodium aluminate solution for seed crystal decomposition, the newly formed aluminum hydroxide is uniformly deposited, directionally grown, and has its edges blunted on the microcrystalline surface. Consequently, the particles in the aluminum hydroxide slurry obtained from seed crystal decomposition inherit the near-spherical morphology characteristics.
[0042] After being subjected to hydrocyclone classification, solid-liquid separation, washing and drying, and dry classification, the aluminum hydroxide slurry yields spherical low-sodium aluminum hydroxide powder. This allows for the in-situ preparation of spherical low-sodium aluminum hydroxide powder without the need for post-granulation shaping.
[0043] Examples of urea solution concentrations of 40 g / L to 70 g / L include, but are not limited to: 40 g / L, 45 g / L, 50 g / L, 55 g / L, 60 g / L, 65 g / L, and 70 g / L. Examples of aluminum sulfate solution concentrations of 40 g / L to 70 g / L include, but are not limited to: 40 g / L, 45 g / L, 50 g / L, 55 g / L, 60 g / L, 65 g / L, and 70 g / L.
[0044] In some embodiments, the urea in the urea solution and the Al in the aluminum sulfate solution 3+ The molar ratio is 10:1 to 12:1.
[0045] Controlling the Al content in urea solution and aluminum sulfate solution 3+ The molar ratio is 10:1 to 12:1. This molar ratio ensures that the stoichiometric ratio of the morphology modifier and the aluminum source in the urea-aluminum sulfate mixed solution is within the optimal range. This allows the spherical induction effect of urea molecules and the nucleation supply of aluminum ions to be synergistically matched during the preparation of spherical aluminum hydroxide microcrystalline slurry, thereby ensuring the sphericity and particle size uniformity of the microcrystals in the spherical aluminum hydroxide microcrystalline slurry.
[0046] This molar ratio control ensures that the microcrystalline particles in the near-spherical aluminum hydroxide microcrystalline slurry have rounded surfaces, fewer defects, and complete crystallization. This ensures that when the microcrystalline slurry is added as a seed crystal to a refined sodium aluminate solution for seed crystal decomposition, the newly formed aluminum hydroxide is uniformly deposited, directionally grown, and has its edges blunted on the microcrystalline surface. Consequently, the particles in the aluminum hydroxide slurry obtained from seed crystal decomposition inherit the near-spherical morphology characteristics.
[0047] After being subjected to hydrocyclone classification, solid-liquid separation, washing and drying, and dry classification, the aluminum hydroxide slurry yields spherical low-sodium aluminum hydroxide powder. This allows for the in-situ preparation of spherical low-sodium aluminum hydroxide powder without the need for post-granulation shaping.
[0048] Urea and Al 3+Examples of molar ratios of 10:1 to 12:1 include, but are not limited to: 10:1, 10.5:1, 11:1, 11.5:1, and 12:1.
[0049] In some embodiments, the refined sodium aluminate solution is prepared from industrial aluminum hydroxide or bauxite through alkali dissolution, lime slurry purification, deep filtration, and impurity removal and desilication processes; The alumina concentration of the refined sodium aluminate solution is 70 g / L to 140 g / L, and the caustic ratio αK is 1.4 to 2.5.
[0050] The alumina concentration of the refined sodium aluminate solution is limited to 70 g / L to 140 g / L and the caustic ratio αK is 1.4 to 2.5. This alumina concentration range ensures sufficient aluminum source supply and controllable solution viscosity during seed crystal decomposition. This caustic ratio αK range ensures that the stability and supersaturation of the refined sodium aluminate solution are in optimal balance, thereby ensuring that the deposition rate of aluminum hydroxide and the crystal growth quality are controllable in tandem during seed crystal decomposition.
[0051] The synergistic limitation of the alumina concentration and the caustic ratio αK enables the uniform deposition, directional growth, and edge blunting of aluminum hydroxide on the microcrystalline surface of the near-spherical aluminum hydroxide microcrystalline slurry during the seed crystal decomposition process, thereby obtaining an aluminum hydroxide slurry with morphology that inherits near-spherical characteristics and complete crystallization.
[0052] After being subjected to hydrocyclone classification, solid-liquid separation, washing and drying, and dry classification, the aluminum hydroxide slurry yields spherical low-sodium aluminum hydroxide powder. This allows for the in-situ preparation of spherical low-sodium aluminum hydroxide powder without the need for post-granulation shaping.
[0053] Examples of alumina concentrations from 70 g / L to 140 g / L include, but are not limited to: 70 g / L, 80 g / L, 90 g / L, 100 g / L, 110 g / L, 120 g / L, 130 g / L, and 140 g / L. Examples of caustic ratios αK from 1.4 to 2.5 include, but are not limited to: 1.4, 1.5, 1.6, 1.8, 2.0, 2.2, and 2.5.
[0054] In some embodiments, the initial seed ratio for seed decomposition is 5%, the decomposition time is 48h to 72h, and the decomposition solid content is 200g / L to 500g / L.
[0055] The initial seed ratio for seed decomposition is limited to 5%. This initial seed ratio ensures that the number of seed crystals and the ratio of aluminum source in sodium aluminate solution are within the optimal range during the seed decomposition process. This allows newly formed aluminum hydroxide in the aluminum hydroxide slurry to be efficiently deposited on the surface of microcrystals in the near-spherical aluminum hydroxide microcrystal slurry, while avoiding excessive competition between seed crystals. This ensures the concentrated particle size distribution and spherical regularity of the particles in the aluminum hydroxide slurry.
[0056] The decomposition time is limited to 48h to 72h. This decomposition time range ensures that the seed crystal decomposition process is fully carried out, so that the alumina in the aluminum hydroxide slurry is completely decomposed and the crystals grow fully, thereby ensuring the yield and particle size controllability of the spherical low-sodium aluminum hydroxide powder.
[0057] The decomposition solid content is limited to 200 g / L to 500 g / L. This range ensures that the solid concentration and slurry flowability are matched in a coordinated manner during the seed decomposition process, thereby optimizing the contact efficiency between the seed crystals and the solution in the aluminum hydroxide slurry and making the stirring energy consumption controllable. This ensures the growth quality and morphological regularity of the particles in the aluminum hydroxide slurry.
[0058] The synergistic constraints of the initial seed ratio, decomposition time, and decomposition solids content enable aluminum hydroxide to be uniformly deposited, directionally grown, and have its edges blunted on the microcrystalline surface of the near-spherical aluminum hydroxide microcrystalline slurry during the seed decomposition process, thereby obtaining an aluminum hydroxide slurry with morphology inheriting near-spherical characteristics and sufficient yield.
[0059] After being subjected to hydrocyclone classification, solid-liquid separation, washing and drying, and dry classification, the aluminum hydroxide slurry yields spherical low-sodium aluminum hydroxide powder. This allows for the in-situ preparation of spherical low-sodium aluminum hydroxide powder without the need for post-granulation shaping.
[0060] Examples of decomposition times of 48h to 72h include, but are not limited to: 48h, 50h, 55h, 60h, 65h, 70h, and 72h. Examples of decomposition solids content of 200g / L to 500g / L include, but are not limited to: 200g / L, 250g / L, 300g / L, 350g / L, 400g / L, 450g / L, and 500g / L.
[0061] In some embodiments, the stirring speed of the low-shear stirring method is no higher than 250 r / min.
[0062] The stirring speed of the low-shear stirring method is limited to no more than 250 r / min. This upper limit of stirring speed ensures that the fluid shear force during the seed decomposition process is within a controllable range, preventing the crystals in the aluminum hydroxide slurry from breaking, being scratched at the edges and corners, and generating secondary fine powder due to strong shear, thereby ensuring the integrity and spherical regularity of the particles in the aluminum hydroxide slurry.
[0063] This low-shear stirring method enables aluminum hydroxide to be uniformly deposited, directionally grown, and have its edges blunted on the microcrystalline surface of the near-spherical aluminum hydroxide microcrystalline slurry during the seed crystal decomposition process, thereby obtaining an aluminum hydroxide slurry with morphological characteristics that inherits near-spherical shape and has few defects.
[0064] After being subjected to hydrocyclone classification, solid-liquid separation, washing and drying, and dry classification, the aluminum hydroxide slurry yields spherical low-sodium aluminum hydroxide powder. This allows for the in-situ preparation of spherical low-sodium aluminum hydroxide powder without the need for post-granulation shaping.
[0065] Examples of stirring speeds not exceeding 250 r / min include, but are not limited to: 100 r / min, 120 r / min, 150 r / min, 180 r / min, 200 r / min, 220 r / min, and 250 r / min.
[0066] In some embodiments, the ammonium salt in the hot water-assisted ammonium salt deep desodiumning is at least one of ammonium acetate, ammonium chloride, and ammonium sulfate, and the amount of the ammonium salt is 100 ppm to 300 ppm.
[0067] The ammonium salt in the hot water co-processed ammonium salt deep sodium removal is limited to at least one of ammonium acetate, ammonium chloride, and ammonium sulfate. This limitation of the ammonium salt type ensures a stable and reliable source of ammonium ions in the hot water co-processed ammonium salt system, enabling ammonium ions to effectively exchange sodium ions on the surface or inside the aluminum hydroxide filter cake in hot water.
[0068] The dosage of ammonium salt is limited to 100ppm to 300ppm. This dosage range ensures that the concentration of ammonium ions in the hot water co-processed ammonium salt system is matched with the exchange efficiency of sodium ions in the aluminum hydroxide filter cake. This allows the hot water to activate the pores of aluminum hydroxide and release the coating alkali or lattice alkali while the ammonium ions efficiently replace sodium ions, thereby obtaining a dry aluminum hydroxide filter cake with a sodium oxide content of no more than 0.1wt%.
[0069] After dry classification, the dried aluminum hydroxide filter cake yields spherical low-sodium aluminum hydroxide powder with a sodium oxide mass fraction of no more than 0.1 wt%, thus enabling the in-situ preparation of spherical low-sodium aluminum hydroxide powder without the need for post-granulation shaping.
[0070] Examples of ammonium salt dosages of 100ppm to 300ppm include, but are not limited to: 100ppm, 120ppm, 150ppm, 180ppm, 200ppm, 220ppm, 250ppm, 280ppm, and 300ppm.
[0071] In some embodiments, the dry classification employs an airflow classification process; The fine-particle aluminum hydroxide obtained by dry classification is packaged as a thermally conductive, spherical, low-sodium aluminum hydroxide product, while the coarse-particle aluminum hydroxide obtained by dry classification is used for catalysis.
[0072] The dry classification process employs an airflow classification technology, which separates the dried aluminum hydroxide filter cake according to particle size based on aerodynamic principles. This effectively removes large particles from the aluminum hydroxide filter cake, resulting in a fine-particle-size product with controllable particle size.
[0073] The fine-particle aluminum hydroxide obtained by dry classification is packaged as a spherical low-sodium aluminum hydroxide product for thermal conductivity. The particle size of this fine-particle aluminum hydroxide meets the requirements for thermal conductivity filling, thereby ensuring the high filling adaptability of the spherical low-sodium aluminum hydroxide powder in thermal conductivity applications.
[0074] The coarse-grained aluminum hydroxide obtained by dry classification is used for catalysis. The particle size of this coarse-grained product meets the particle size requirements of the catalyst, thereby ensuring the full utilization of resources across all particle sizes.
[0075] This dry grading process removes large particles from the dried aluminum hydroxide filter cake, resulting in fine-sized aluminum hydroxide with regular morphology and controllable particle size. This allows for the production of spherical low-sodium aluminum hydroxide powder suitable for thermal conductivity without the need for post-particle shaping.
[0076] Secondly, embodiments of this application provide a spherical low-sodium aluminum hydroxide powder, which is prepared by the preparation method described in any one of the first aspects; The spherical low-sodium aluminum hydroxide powder has an in-situ grown spherical particle morphology. The spherical low-sodium aluminum hydroxide powder has a sodium oxide mass fraction of no more than 0.1 wt%, a median particle size D50 of 40 μm to 75 μm, and an oil absorption rate of no more than 22 mL / 100 g.
[0077] This type of spherical low-sodium aluminum hydroxide has an in-situ grown spherical particle morphology. This spherical particle morphology increases the contact area between particles when the spherical low-sodium aluminum hydroxide powder is stacked, and the contact mode is mainly surface contact, thereby constructing a continuous heat conduction network channel.
[0078] The sodium oxide mass fraction of this type of spherical low-sodium aluminum hydroxide is no more than 0.1 wt%. This low sodium content ensures that the insulating properties of the spherical low-sodium aluminum hydroxide powder are stable under high-temperature conditions, thereby avoiding the degradation of the reliability of thermally conductive composite materials by alkali corrosion.
[0079] The median particle size D50 of this type of spherical low-sodium aluminum hydroxide is 40μm to 75μm. This particle size range enables the spherical low-sodium aluminum hydroxide powder to achieve a high proportion of filling in thermally conductive composite materials while maintaining controllable system viscosity, thereby meeting the processing requirements of high filling and low viscosity.
[0080] The oil absorption rate of this type of spherical low-sodium aluminum hydroxide is no more than 22mL / 100g. This low oil absorption rate optimizes the interfacial bonding between the spherical low-sodium aluminum hydroxide powder and the resin matrix and reduces resin consumption, thereby improving the processing fluidity and interfacial bonding of the thermally conductive composite material.
[0081] When this type of spherical low-sodium aluminum hydroxide powder is used as an inorganic thermally conductive and insulating filler in thermally conductive silicone, epoxy thermally conductive potting compound, thermally conductive modified plastic, and heat dissipation polymer composite material for power batteries of new energy vehicles, the synergistic effect of its spherical particle morphology, low sodium content, controllable particle size, and low oil absorption rate enables the thermally conductive composite material to achieve integrated performance of high filling, low viscosity, high thermal conductivity, and high insulation. This solves the technical problem that the irregular morphology, high sodium content, and high oil absorption rate of aluminum hydroxide powder in the prior art limit the performance of thermally conductive composite materials.
[0082] Existing technologies produce aluminum hydroxide powders with irregular morphology, prominent edges, high sodium content, and high oil absorption, which cannot simultaneously meet the comprehensive requirements of thermally conductive composite materials for high filling capacity, low viscosity, high thermal conductivity, and high insulation. The near-spherical low-sodium aluminum hydroxide provided in this application has a near-spherical particle morphology formed by in-situ growth, a sodium oxide mass fraction of no more than 0.1 wt%, a median particle size D50 of 40 μm to 75 μm, and an oil absorption rate of no more than 22 mL / 100 g, thereby optimizing the integrated performance of the product and breaking through the bottleneck of the inability to simultaneously achieve the desired performance of aluminum hydroxide powder in existing technologies.
[0083] Examples of median particle size D50 of 40μm to 75μm include, but are not limited to: 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, and 75μm.
[0084] Thirdly, embodiments of this application provide an application of the spherical low-sodium aluminum hydroxide powder described in the second aspect as a thermally conductive filler, characterized in that the spherical low-sodium aluminum hydroxide powder is used as an inorganic thermally conductive and insulating filler in thermally conductive silicone, epoxy thermally conductive potting compound, thermally conductive modified plastic, and heat dissipation polymer composite material for power batteries of new energy vehicles.
[0085] Limited spherical low-sodium aluminum hydroxide is used as an inorganic thermally conductive and insulating filler in thermally conductive silicone, epoxy thermally conductive potting compound, thermally conductive modified plastic, and heat dissipation polymer composite material for power batteries of new energy vehicles. The spherical particle morphology of this type of spherical low-sodium aluminum hydroxide, which is grown in situ, enables it to achieve a high proportion of filling in the above-mentioned thermally conductive composite materials, and the particles form a continuous thermally conductive network through surface contact, thereby improving the thermal conductivity of the thermally conductive composite material.
[0086] The sodium oxide mass fraction of this type of spherical low-sodium aluminum hydroxide is no more than 0.1 wt%. This low sodium content enables this type of spherical low-sodium aluminum hydroxide to maintain high-temperature insulation reliability in the above-mentioned thermally conductive composite materials, thereby avoiding damage to electronic components and power battery systems caused by alkali corrosion.
[0087] The median particle size D50 of this type of spherical low-sodium aluminum hydroxide is 40μm to 75μm. This controllable particle size enables the spherical low-sodium aluminum hydroxide to achieve synergistic adaptation between particle size and matrix viscosity in the above-mentioned thermally conductive composite material, thereby ensuring the high filler processability of the thermally conductive composite material.
[0088] The oil absorption rate of this type of spherical low-sodium aluminum hydroxide is no more than 22 mL / 100 g. This low oil absorption rate reduces resin consumption and optimizes interfacial bonding in the above-mentioned thermally conductive composite materials, thereby improving the processing fluidity and mechanical reliability of the thermally conductive composite materials.
[0089] When this type of spherical low-sodium aluminum hydroxide is used as an inorganic thermally conductive and insulating filler in thermally conductive silicone, epoxy thermally conductive potting compound, thermally conductive modified plastic, and heat dissipation polymer composite material for power batteries of new energy vehicles, the synergistic effect of the spherical particle morphology, low sodium content, controllable particle size and low oil absorption rate enables the above-mentioned thermally conductive composite materials to achieve integrated performance of high filling, low viscosity, high thermal conductivity, high insulation and easy processing. This solves the technical problem that the overall performance of thermally conductive composite materials is limited by the irregular morphology, high sodium content and high oil absorption rate of aluminum hydroxide powder as a thermally conductive filler in the prior art.
[0090] In some embodiments, the fine-particle-size aluminum hydroxide slurry obtained from the cyclone classification process is used as a seed crystal for a new round of seed crystal decomposition.
[0091] In some embodiments, the preparation method does not employ post-particle shaping processes such as mechanical grinding, melt granulation, and spray molding.
[0092] In some embodiments, the spherical low-sodium aluminum hydroxide powder has a smooth and dense particle surface, no sharp edges, and very few lattice defects.
[0093] The present application is further illustrated below with reference to specific embodiments. Experimental methods in the following embodiments that do not specify specific conditions are generally determined according to national standards / standards / disclosures herein; if no corresponding national standards / standards / disclosures exist, they are performed according to generally accepted international standards, conventional conditions, or conditions recommended by the manufacturer.
[0094] Example 1 Example 1 provides a method for preparing spherical low-sodium aluminum hydroxide, comprising the following steps: Step 1: Add a urea solution with a concentration of 50 g / L to an aluminum sulfate solution with a concentration of 50 g / L and mix to obtain a urea-aluminum sulfate mixed solution.
[0095] Step 2: At 40°C, a refined sodium aluminate solution with an alumina concentration of 135 g / L and a caustic ratio αK of 1.41 is added to the urea-aluminum sulfate mixed solution until the pH of the urea-aluminum sulfate mixed solution is 8-10.
[0096] Step 3: The urea-aluminum sulfate mixed solution with a pH of 8-10 is chemically reacted at 85°C for 2 hours to obtain spherical aluminum hydroxide microcrystalline slurry.
[0097] Step 4: The spherical aluminum hydroxide microcrystalline slurry is added as a seed crystal to a refined sodium aluminate solution with an alumina concentration of 135 g / L and a caustic ratio αK of 1.41 for seed crystal decomposition to obtain aluminum hydroxide slurry. The seed crystal decomposition adopts a gradient slow cooling temperature control method, with an initial decomposition temperature of 80℃ and a decomposition termination temperature of 55℃. The seed crystal decomposition adopts a low shear force stirring method, with a stirring speed not exceeding 250 r / min. The initial seed ratio of the seed crystal decomposition is 5%, the decomposition time is 70 h, and the decomposition solid content is 200 g / L to 500 g / L.
[0098] Step 5: Perform hydrocyclone classification on the aluminum hydroxide slurry to obtain coarse-particle-size aluminum hydroxide slurry and fine-particle-size aluminum hydroxide slurry.
[0099] Step 6: Perform solid-liquid separation on the coarse-particle-size aluminum hydroxide slurry to obtain aluminum hydroxide filter cake.
[0100] Step 7: Wash and dry the aluminum hydroxide filter cake; the washing is carried out in a hot water synergistic ammonium salt system for deep sodium removal; the ammonium salt in the hot water synergistic ammonium salt deep sodium removal is ammonium acetate, and the amount of ammonium salt is 100ppm to 300ppm.
[0101] Step 8: Dry classification is performed on the dried aluminum hydroxide filter cake to remove large particles and obtain spherical low-sodium aluminum hydroxide powder; the dry classification adopts an air classifier process.
[0102] Example 2 Example 2 provides a method for preparing spherical low-sodium aluminum hydroxide, comprising the following steps: Step 1: Add a urea solution with a concentration of 40 g / L to an aluminum sulfate solution with a concentration of 70 g / L and mix to obtain a urea-aluminum sulfate mixed solution.
[0103] Step 2: At 50°C, a refined sodium aluminate solution with an alumina concentration of 135 g / L and a caustic ratio αK of 1.41 is added to the urea-aluminum sulfate mixed solution until the pH of the urea-aluminum sulfate mixed solution is 8-10.
[0104] Step 3: The urea-aluminum sulfate mixed solution with a pH of 8-10 is chemically reacted at 90°C for 2 hours to obtain spherical aluminum hydroxide microcrystalline slurry.
[0105] Step 4: The spherical aluminum hydroxide microcrystalline slurry is added as a seed crystal to a refined sodium aluminate solution with an alumina concentration of 135 g / L and a caustic ratio αK of 1.41 for seed crystal decomposition to obtain aluminum hydroxide slurry. The seed crystal decomposition adopts a gradient slow cooling temperature control method, with an initial decomposition temperature of 75℃ and a decomposition termination temperature of 55℃. The seed crystal decomposition adopts a low shear force stirring method, with a stirring speed not exceeding 250 r / min. The initial seed ratio of the seed crystal decomposition is 5%, the decomposition time is 70 h, and the decomposition solid content is 200 g / L to 500 g / L.
[0106] Step 5: Perform hydrocyclone classification on the aluminum hydroxide slurry to obtain coarse-particle-size aluminum hydroxide slurry and fine-particle-size aluminum hydroxide slurry.
[0107] Step 6: Perform solid-liquid separation on the coarse-particle-size aluminum hydroxide slurry to obtain aluminum hydroxide filter cake.
[0108] Step 7: Wash and dry the aluminum hydroxide filter cake; the washing is carried out in a hot water synergistic ammonium salt system for deep sodium removal; the ammonium salt in the hot water synergistic ammonium salt deep sodium removal is ammonium acetate, and the amount of ammonium salt is 100ppm to 300ppm.
[0109] Step 8: Dry classification is performed on the dried aluminum hydroxide filter cake to remove large particles and obtain spherical low-sodium aluminum hydroxide powder; the dry classification adopts an air classifier process.
[0110] Example 3 Example 3 provides a method for preparing spherical low-sodium aluminum hydroxide, comprising the following steps: Step 1: Add a 70 g / L urea solution to a 70 g / L aluminum sulfate solution and mix to obtain a urea-aluminum sulfate mixed solution.
[0111] Step 2: At 50°C, a refined sodium aluminate solution with an alumina concentration of 135 g / L and a caustic ratio αK of 1.41 is added to the urea-aluminum sulfate mixed solution until the pH of the urea-aluminum sulfate mixed solution is 8-10.
[0112] Step 3: The urea-aluminum sulfate mixed solution with a pH of 8-10 is chemically reacted at 90°C for 2 hours to obtain spherical aluminum hydroxide microcrystalline slurry.
[0113] Step 4: The spherical aluminum hydroxide microcrystalline slurry is added as a seed crystal to a refined sodium aluminate solution with an alumina concentration of 135 g / L and a caustic ratio αK of 1.41 for seed crystal decomposition to obtain aluminum hydroxide slurry. The seed crystal decomposition adopts a gradient slow cooling temperature control method, with an initial decomposition temperature of 75℃ and a decomposition termination temperature of 55℃. The seed crystal decomposition adopts a low shear force stirring method, with a stirring speed not exceeding 250 r / min. The initial seed ratio of the seed crystal decomposition is 5%, the decomposition time is 70 h, and the decomposition solid content is 200 g / L to 500 g / L.
[0114] Step 5: Perform hydrocyclone classification on the aluminum hydroxide slurry to obtain coarse-particle-size aluminum hydroxide slurry and fine-particle-size aluminum hydroxide slurry.
[0115] Step 6: Perform solid-liquid separation on the coarse-particle-size aluminum hydroxide slurry to obtain aluminum hydroxide filter cake.
[0116] Step 7: Wash and dry the aluminum hydroxide filter cake; the washing is carried out in a hot water synergistic ammonium salt system for deep sodium removal; the ammonium salt in the hot water synergistic ammonium salt deep sodium removal is ammonium acetate, and the amount of ammonium salt is 100ppm to 300ppm.
[0117] Step 8: Dry classification is performed on the dried aluminum hydroxide filter cake to remove large particles and obtain spherical low-sodium aluminum hydroxide powder; the dry classification adopts an air classifier process.
[0118] Example 4 Example 4 provides a method for preparing spherical low-sodium aluminum hydroxide, comprising the following steps: Step 1: Add a 60 g / L urea solution to a 55 g / L aluminum sulfate solution and mix to obtain a urea-aluminum sulfate mixed solution.
[0119] Step 2: At 45°C, a refined sodium aluminate solution with an alumina concentration of 120 g / L and a caustic ratio αK of 1.6 is added to the urea-aluminum sulfate mixed solution until the pH of the urea-aluminum sulfate mixed solution is 8-10.
[0120] Step 3: The urea-aluminum sulfate mixed solution with a pH of 8-10 is chemically reacted at 88°C for 3 hours to obtain spherical aluminum hydroxide microcrystalline slurry.
[0121] Step 4: The spherical aluminum hydroxide microcrystalline slurry is added as a seed crystal to a refined sodium aluminate solution with an alumina concentration of 120 g / L and a caustic ratio αK of 1.6 for seed crystal decomposition to obtain aluminum hydroxide slurry. The seed crystal decomposition adopts a gradient slow cooling temperature control method, with an initial decomposition temperature of 70℃ and a decomposition termination temperature of 54℃. The seed crystal decomposition adopts a low shear force stirring method, with a stirring speed not exceeding 250 r / min. The initial seed ratio of the seed crystal decomposition is 5%, the decomposition time is 60 h, and the decomposition solid content is 200 g / L to 500 g / L.
[0122] Step 5: Perform hydrocyclone classification on the aluminum hydroxide slurry to obtain coarse-particle-size aluminum hydroxide slurry and fine-particle-size aluminum hydroxide slurry.
[0123] Step 6: Perform solid-liquid separation on the coarse-particle-size aluminum hydroxide slurry to obtain aluminum hydroxide filter cake.
[0124] Step 7: Wash and dry the aluminum hydroxide filter cake; the washing is carried out in a hot water synergistic ammonium salt system for deep sodium removal; the ammonium salt in the hot water synergistic ammonium salt deep sodium removal is ammonium acetate, and the amount of ammonium salt is 100ppm to 300ppm.
[0125] Step 8: Dry classification is performed on the dried aluminum hydroxide filter cake to remove large particles and obtain spherical low-sodium aluminum hydroxide powder; the dry classification adopts an air classifier process.
[0126] Example 5 Example 5 provides a method for preparing spherical low-sodium aluminum hydroxide, comprising the following steps: Step 1: Add a urea solution with a concentration of 45 g / L to an aluminum sulfate solution with a concentration of 60 g / L and mix to obtain a urea-aluminum sulfate mixed solution.
[0127] Step 2: At 55°C, a refined sodium aluminate solution with an alumina concentration of 100 g / L and a caustic ratio αK of 1.8 is added to the urea-aluminum sulfate mixed solution until the pH of the urea-aluminum sulfate mixed solution is 8-10.
[0128] Step 3: The urea-aluminum sulfate mixed solution with a pH of 8-10 is chemically reacted at 82°C for 3.5 hours to obtain spherical aluminum hydroxide microcrystalline slurry.
[0129] Step 4: The spherical aluminum hydroxide microcrystalline slurry is added as a seed crystal to a refined sodium aluminate solution with an alumina concentration of 100 g / L and a caustic ratio αK of 1.8 for seed crystal decomposition to obtain aluminum hydroxide slurry. The seed crystal decomposition adopts a gradient slow cooling temperature control method, with an initial decomposition temperature of 68℃ and a decomposition termination temperature of 53.5℃. The seed crystal decomposition adopts a low shear force stirring method, with a stirring speed not exceeding 250 r / min. The initial seed ratio of the seed crystal decomposition is 5%, the decomposition time is 55 h, and the decomposition solid content is 200 g / L to 500 g / L.
[0130] Step 5: Perform hydrocyclone classification on the aluminum hydroxide slurry to obtain coarse-particle-size aluminum hydroxide slurry and fine-particle-size aluminum hydroxide slurry.
[0131] Step 6: Perform solid-liquid separation on the coarse-particle-size aluminum hydroxide slurry to obtain aluminum hydroxide filter cake.
[0132] Step 7: Wash and dry the aluminum hydroxide filter cake; the washing is carried out in a hot water synergistic ammonium salt system for deep sodium removal; the ammonium salt in the hot water synergistic ammonium salt deep sodium removal is ammonium acetate, and the amount of ammonium salt is 100ppm to 300ppm.
[0133] Step 8: Dry classification is performed on the dried aluminum hydroxide filter cake to remove large particles and obtain spherical low-sodium aluminum hydroxide powder; the dry classification adopts an air classifier process.
[0134] Example 6 Example 6 provides a method for preparing spherical low-sodium aluminum hydroxide, comprising the following steps: Step 1: Add a urea solution with a concentration of 55 g / L to an aluminum sulfate solution with a concentration of 65 g / L and mix to obtain a urea-aluminum sulfate mixed solution.
[0135] Step 2: At 42°C, a refined sodium aluminate solution with an alumina concentration of 110 g / L and a caustic ratio αK of 1.5 is added to the urea-aluminum sulfate mixed solution until the pH of the urea-aluminum sulfate mixed solution is 8-10.
[0136] Step 3: The urea-aluminum sulfate mixed solution with a pH of 8-10 is chemically reacted at 86°C for 2.5 hours to obtain spherical aluminum hydroxide microcrystalline slurry.
[0137] Step 4: The spherical aluminum hydroxide microcrystalline slurry is added as a seed crystal to a refined sodium aluminate solution with an alumina concentration of 110 g / L and a caustic ratio αK of 1.5 for seed crystal decomposition to obtain aluminum hydroxide slurry. The seed crystal decomposition adopts a gradient slow cooling temperature control method, with an initial decomposition temperature of 72℃ and a decomposition termination temperature of 54.5℃. The seed crystal decomposition adopts a low shear force stirring method, with a stirring speed not exceeding 250 r / min. The initial seed ratio of the seed crystal decomposition is 5%, the decomposition time is 65 h, and the decomposition solid content is 200 g / L to 500 g / L.
[0138] Step 5: Perform hydrocyclone classification on the aluminum hydroxide slurry to obtain coarse-particle-size aluminum hydroxide slurry and fine-particle-size aluminum hydroxide slurry.
[0139] Step 6: Perform solid-liquid separation on the coarse-particle-size aluminum hydroxide slurry to obtain aluminum hydroxide filter cake.
[0140] Step 7: Wash and dry the aluminum hydroxide filter cake; the washing is carried out in a hot water synergistic ammonium salt system for deep sodium removal; the ammonium salt in the hot water synergistic ammonium salt deep sodium removal is ammonium acetate, and the amount of ammonium salt is 100ppm to 300ppm.
[0141] Step 8: Dry classification is performed on the dried aluminum hydroxide filter cake to remove large particles and obtain spherical low-sodium aluminum hydroxide powder; the dry classification adopts an air classifier process.
[0142] Example 7 Example 7 provides a method for preparing spherical low-sodium aluminum hydroxide, comprising the following steps: Step 1: Add a 65 g / L urea solution to a 45 g / L aluminum sulfate solution and mix to obtain a urea-aluminum sulfate mixed solution.
[0143] Step 2: At 58°C, a refined sodium aluminate solution with an alumina concentration of 90 g / L and a caustic ratio αK of 2.0 is added to the urea-aluminum sulfate mixed solution until the pH of the urea-aluminum sulfate mixed solution is 8-10.
[0144] Step 3: The urea-aluminum sulfate mixed solution with a pH of 8-10 is chemically reacted at 89°C for 2.5 hours to obtain spherical aluminum hydroxide microcrystalline slurry.
[0145] Step 4: The spherical aluminum hydroxide microcrystalline slurry is added as a seed crystal to a refined sodium aluminate solution with an alumina concentration of 90 g / L and a caustic ratio αK of 2.0 for seed crystal decomposition to obtain aluminum hydroxide slurry. The seed crystal decomposition adopts a gradient slow cooling temperature control method, with an initial decomposition temperature of 76℃ and a decomposition termination temperature of 55℃. The seed crystal decomposition adopts a low shear force stirring method, with a stirring speed not exceeding 250 r / min. The initial seed ratio of the seed crystal decomposition is 5%, the decomposition time is 50 h, and the decomposition solid content is 200 g / L to 500 g / L.
[0146] Step 5: Perform hydrocyclone classification on the aluminum hydroxide slurry to obtain coarse-particle-size aluminum hydroxide slurry and fine-particle-size aluminum hydroxide slurry.
[0147] Step 6: Perform solid-liquid separation on the coarse-particle-size aluminum hydroxide slurry to obtain aluminum hydroxide filter cake.
[0148] Step 7: Wash and dry the aluminum hydroxide filter cake; the washing is carried out in a hot water synergistic ammonium salt system for deep sodium removal; the ammonium salt in the hot water synergistic ammonium salt deep sodium removal is ammonium acetate, and the amount of ammonium salt is 100ppm to 300ppm.
[0149] Step 8: Dry classification is performed on the dried aluminum hydroxide filter cake to remove large particles and obtain spherical low-sodium aluminum hydroxide powder; the dry classification adopts an air classifier process.
[0150] Example 8 Example 8 provides a method for preparing spherical low-sodium aluminum hydroxide, comprising the following steps: Step 1: Add a urea solution with a concentration of 50 g / L to an aluminum sulfate solution with a concentration of 50 g / L and mix to obtain a urea-aluminum sulfate mixed solution.
[0151] Step 2: At 48°C, a refined sodium aluminate solution with an alumina concentration of 130 g / L and a caustic ratio αK of 1.45 is added to the urea-aluminum sulfate mixed solution until the pH of the urea-aluminum sulfate mixed solution is 8-10.
[0152] Step 3: The urea-aluminum sulfate mixed solution with a pH of 8-10 is chemically reacted at 85°C for 4 hours to obtain spherical aluminum hydroxide microcrystalline slurry.
[0153] Step 4: The spherical aluminum hydroxide microcrystalline slurry is added as a seed crystal to a refined sodium aluminate solution with an alumina concentration of 130 g / L and a caustic ratio αK of 1.45 for seed crystal decomposition to obtain aluminum hydroxide slurry. The seed crystal decomposition adopts a gradient slow cooling temperature control method, with an initial decomposition temperature of 74℃ and a decomposition termination temperature of 54℃. The seed crystal decomposition adopts a low shear force stirring method, with a stirring speed not exceeding 250 r / min. The initial seed ratio of the seed crystal decomposition is 5%, the decomposition time is 72 h, and the decomposition solid content is 200 g / L to 500 g / L.
[0154] Step 5: Perform hydrocyclone classification on the aluminum hydroxide slurry to obtain coarse-particle-size aluminum hydroxide slurry and fine-particle-size aluminum hydroxide slurry.
[0155] Step 6: Perform solid-liquid separation on the coarse-particle-size aluminum hydroxide slurry to obtain aluminum hydroxide filter cake.
[0156] Step 7: Wash and dry the aluminum hydroxide filter cake; the washing is carried out in a hot water synergistic ammonium salt system for deep sodium removal; the ammonium salt in the hot water synergistic ammonium salt deep sodium removal is ammonium acetate, and the amount of ammonium salt is 100ppm to 300ppm.
[0157] Step 8: Dry classification is performed on the dried aluminum hydroxide filter cake to remove large particles and obtain spherical low-sodium aluminum hydroxide powder; the dry classification adopts an air classifier process.
[0158] Comparative Example 1 Comparative Example 1 provides a method for preparing spherical low-sodium aluminum hydroxide. The difference from Example 1 is that the initial decomposition temperature of the gradient slow cooling temperature control method for seed crystal decomposition is changed from 80°C to 73°C. The remaining steps are the same as in Example 1 and will not be repeated here.
[0159] Comparative Example 2 Comparative Example 2 provides a method for preparing spherical low-sodium aluminum hydroxide. The difference from Example 1 is that the initial decomposition temperature of the gradient slow cooling temperature control method for seed crystal decomposition is changed from 80°C to 65°C. The remaining steps are the same as in Example 1 and will not be repeated here.
[0160] Comparative Example 3 Comparative Example 3 provides a method for preparing spherical low-sodium aluminum hydroxide. The difference from Example 2 is that the caustic ratio αK of the refined sodium aluminate solution is changed from 1.41 to 1.75. The remaining steps are the same as in Example 2 and will not be repeated here.
[0161] Comparative Example 4 Comparative Example 4 provides a method for preparing spherical low-sodium aluminum hydroxide. The difference from Example 2 is that the caustic ratio αK of the refined sodium aluminate solution is changed from 1.41 to 2.0. The remaining steps are the same as in Example 2 and will not be repeated here.
[0162] Comparative Example 5 Comparative Example 5 provides a method for preparing spherical low-sodium aluminum hydroxide, which differs from Example 2 in that the caustic ratio αK of the refined sodium aluminate solution is changed from 1.41 to 2.5. The remaining steps are the same as in Example 2 and will not be repeated here.
[0163] The spherical low-sodium aluminum hydroxide powder prepared by the above method has a median particle size D50 of 57.150 μm and a morphology of spherical shape.
[0164] Comparative Example 6 Comparative Example 6 provides a method for preparing spherical low-sodium aluminum hydroxide, which differs from Example 3 in that the alumina concentration of the refined sodium aluminate solution is changed from 135 g / L to 115 g / L. The remaining steps are the same as in Example 3 and will not be repeated here.
[0165] Comparative Example 7 Comparative Example 7 provides a method for preparing spherical low-sodium aluminum hydroxide, which differs from Example 3 in that the alumina concentration of the refined sodium aluminate solution is changed from 135 g / L to 95 g / L. The remaining steps are the same as in Example 3 and will not be repeated here.
[0166] Comparative Example 8 Comparative Example 8 provides a method for preparing spherical low-sodium aluminum hydroxide, which differs from Example 3 in that the alumina concentration of the refined sodium aluminate solution is changed from 135 g / L to 75 g / L. The remaining steps are the same as in Example 3 and will not be repeated here.
[0167] Experimental methods for evaluating results: I. Determination of SiO2 content The mass fraction of SiO2 in spherical low-sodium aluminum hydroxide powder was determined by X-ray fluorescence spectrometry (XRF) or chemical analysis.
[0168] II. Determination of Fe2O3 content The mass fraction of Fe2O3 in near-spherical low-sodium aluminum hydroxide powder was determined by X-ray fluorescence spectrometry (XRF) or chemical analysis.
[0169] III. Determination of Na2O Content The mass fraction of Na2O in spherical low-sodium aluminum hydroxide powder was determined by flame atomic absorption spectrometry or inductively coupled plasma optical emission spectrometry (ICP-OES).
[0170] IV. Determination of Loss on Ignition In accordance with GB / T 6609.2 "Methods for chemical analysis and determination of physical properties of alumina - Part 2: Determination of mass loss at 300℃ and 1000℃", the percentage of mass loss of spherical low-sodium aluminum hydroxide powder in the temperature range of 300℃ to 1000℃ was determined.
[0171] V. Determination of Alkali Adsorption The content of adsorbed alkali on the surface of spherical low-sodium aluminum hydroxide powder was determined by acid-base titration.
[0172] VI. Decomposition Rate Determination The decomposition rate is calculated based on the change in alumina concentration before and after sodium aluminate decomposition in semen: Decomposition rate = (alumina concentration before decomposition - alumina concentration after decomposition) / alumina concentration before decomposition × 100%.
[0173] VII. Determination of median particle size at D50 The particle size distribution of near-spherical low-sodium aluminum hydroxide powder was determined using a laser particle size analyzer, and the median particle size D50 value was recorded.
[0174] VIII. Oil Absorption Rate Determination In accordance with the provisions of ASTM D281 or GB / T 5211.15 "Determination of Oil Absorption of Pigments", the oil absorption rate of spherical low-sodium aluminum hydroxide powder was determined by linseed oil or dibutyl phthalate (DBP) absorption method.
[0175] IX. Morphological Observation The particle morphology of near-spherical low-sodium aluminum hydroxide powder was observed using scanning electron microscopy (SEM).
[0176] Table of Experimental Data on the Effects of Each Embodiment and Comparative Example
[0177] By comparing the effect data of each embodiment and each comparative example, we can conclude that: I. Comparing Example 1, Comparative Example 1, and Comparative Example 2, the initial decomposition temperature of the gradient slow cooling temperature control method for seed crystal decomposition in Example 1 was 80°C, the initial decomposition temperature of Comparative Example 1 was 73°C, and the initial decomposition temperature of Comparative Example 2 was 65°C. The Na₂O content of the spherical low-sodium aluminum hydroxide powder in Example 1 was 0.085%, the Na₂O content of Comparative Example 1 was 0.094%, and the Na₂O content of Comparative Example 2 was 0.102%. The D₅₀ of the spherical low-sodium aluminum hydroxide powder in Example 1 was 63.306 μm, the D₅₀ of Comparative Example 1 was 58.458 μm, and the D₅₀ of Comparative Example 2 was 55.832 μm. The decomposition rate of Example 1 was 42.12%, the decomposition rate of Comparative Example 1 was 48.43%, and the decomposition rate of Comparative Example 2 was 50.68%.
[0178] This indicates that when the initial decomposition temperature of the gradient cooling temperature control method for seed crystal decomposition decreases, the supersaturation of the refined sodium aluminate solution increases, the decomposition rate accelerates during seed crystal decomposition, and the decomposition rate increases. However, the accelerated crystal growth rate during seed crystal decomposition leads to a decrease in grain packing density, an increase in internal porosity, an increase in the amount of alkali solution coated in the refined sodium aluminate solution, and weakened molecular thermal motion, which is conducive to sodium ion adsorption. Therefore, the Na2O content of the spherical low-sodium aluminum hydroxide powder increases. Appropriately increasing the initial decomposition temperature of the gradient cooling temperature control method for seed crystal decomposition is beneficial to seed crystal aggregation and growth, but the decomposition rate decreases.
[0179] 2. Comparing Examples 2, 3, 4, and 5, the caustic ratio αK of the purified sodium aluminate solution in Example 2 was 1.41, in Comparative Example 3 it was 1.75, in Comparative Example 4 it was 2.0, and in Comparative Example 5 it was 2.5. The decomposition rate of Example 2 was 48.42%, in Comparative Example 3 it was 39.21%, in Comparative Example 4 it was 31.66%, and in Comparative Example 5 it was 21.22%. The D50 of Example 2 was 53.672 μm, in Comparative Example 3 it was 61.693 μm, in Comparative Example 4 it was 62.183 μm, and in Comparative Example 5 it was 57.150 μm.
[0180] This indicates that as the caustic ratio αK of the refined sodium aluminate solution increases, the stability of the refined sodium aluminate solution improves, the decomposition rate during the seed crystal decomposition process decreases, the particle size of the near-spherical low-sodium aluminum hydroxide powder tends to increase, and the Na2O content tends to decrease. This is because the caustic ratio αK of the refined sodium aluminate solution relates to the supersaturation of the decomposition solution and is the most important factor affecting the seed crystal decomposition rate, alumina yield, and particle size of the near-spherical low-sodium aluminum hydroxide powder.
[0181] 3. Comparing Examples 3, 6, 7, and 8, the alumina concentration of the refined sodium aluminate solution in Example 3 was 135 g / L, in Comparative Example 6 it was 115 g / L, in Comparative Example 7 it was 95 g / L, and in Comparative Example 8 it was 75 g / L. The decomposition rate was 48.21% in Example 3, 49.31% in Comparative Example 6, 49.88% in Comparative Example 7, and 49.75% in Comparative Example 8. The D50 was 43.282 μm in Example 3, 45.484 μm in Comparative Example 6, 48.061 μm in Comparative Example 7, and 49.779 μm in Comparative Example 8.
[0182] This indicates that as the alumina concentration in the refined sodium aluminate solution decreases, the decomposition rate during the seed crystal decomposition process tends to increase, and the particle size of the near-spherical low-sodium aluminum hydroxide powder tends to increase. This is because the alumina concentration in the refined sodium aluminate solution is related to the supersaturation of the decomposition solution. Under the same conditions, a decrease in the alumina concentration of the refined sodium aluminate solution leads to an increase in the decomposition rate, and the particle size of the near-spherical low-sodium aluminum hydroxide powder tends to increase.
[0183] In summary, the comparison of the effect data of the above embodiments and comparative examples shows that the preparation method of spherical low-sodium aluminum hydroxide powder is formed under the combined effect of various parameters, and none of them can be omitted. The morphology of the spherical aluminum hydroxide microcrystalline slurry has a significant impact on the morphology of the spherical low-sodium aluminum hydroxide powder. This is because the decomposition of sodium aluminate crystals is a heterogeneous nucleation and directional growth process. The newly formed aluminum hydroxide preferentially deposits at the active sites on the surface of the crystal and grows epitaxially along the original crystal plane direction of the crystal. The shape of the crystal is the prototype of the product growth. Therefore, the shape of the crystal, the exposure of the crystal plane, the integrity of the crystal, and the agglomeration state directly determine the crystal morphology, particle structure, particle size, density, and stacking mode of the product. The spherical aluminum hydroxide microcrystalline slurry prepared by the spherical induced crystal in-situ growth technology is relatively rounded. When the product morphology is decomposed using this spherical aluminum hydroxide microcrystalline slurry as a template, it is a continuation and evolution of the crystal morphology. Therefore, the spherical low-sodium aluminum hydroxide powder has a spherical morphology.
[0184] Detailed explanation of the attached diagram: Figure 1 The image shows the scanning electron microscope morphology of microcrystalline particles in a spherical aluminum hydroxide microcrystalline slurry. From... Figure 1It can be seen that the microcrystalline particles in the near-spherical aluminum hydroxide microcrystalline slurry exhibit a near-spherical morphology, with smooth surfaces, blunted edges, uniform particle size, and low agglomeration. When these microcrystalline particles are added to a refined sodium aluminate solution as seed crystals for seed decomposition, the newly formed aluminum hydroxide preferentially deposits at active sites on the seed crystal surface and grows epitaxially along the original crystal plane of the seed crystal. The shape of the seed crystal is the prototype of the product growth. Therefore, the shape of the seed crystal, the exposure of the crystal plane, the integrity of crystallization, and the agglomeration state directly determine the crystal morphology, particle structure, particle size, density, and packing mode of the product. Figure 1 The rounded morphology of the medium-sized spherical aluminum hydroxide microcrystalline slurry lays the foundation for the inheritance of the spherical morphology of the spherical low-sodium aluminum hydroxide powder during the subsequent seed crystal decomposition process.
[0185] Figure 2 The image shows the scanning electron microscope morphology of the spherical low-sodium aluminum hydroxide powder prepared using the method of this invention. From... Figure 2 It can be seen that the near-spherical low-sodium aluminum hydroxide powder exhibits a near-spherical morphology, with smooth and dense particle surfaces, no sharp edges, few lattice defects, and tight packing with a concentrated particle size distribution. This morphological characteristic verifies the effectiveness of the complete process for preparing the powder in this invention, which employs near-spherical induced in-situ seed growth, gradient slow cooling temperature-controlled seed decomposition, low-shear force controlled crystal growth, cyclone classification shaping, hot water-ammonium salt synergistic deep sodium removal, and dry fine classification to remove coarse particles. The near-spherical particle morphology of the near-spherical low-sodium aluminum hydroxide powder ensures that the particles are mainly in surface contact during packing, thereby constructing a continuous thermally conductive network channel, while reducing the system viscosity and meeting the requirements of high-filling, low-viscosity processing.
[0186] Figure 3 The image shows the scanning electron microscope morphology of commercially available thermally conductive aluminum hydroxide powder. From... Figure 3 It can be seen that the existing thermally conductive aluminum hydroxide powders on the market have irregular particle morphology, prominent edges and corners, rough surfaces, and severe agglomeration. Some particles exhibit obvious polygonal or plate-like structures. This irregular morphology causes the existing thermally conductive aluminum hydroxide powders on the market to have mainly point contact when stacked, making it difficult to build a continuous thermally conductive network and limiting the improvement of the thermal conductivity of the composite material. At the same time, the irregular morphology increases the viscosity of the system and worsens the processability, making it unable to meet the requirements for high filling. Figure 3 A comparison of the morphology of thermally conductive aluminum hydroxide powder with that of commercial products shows that the spherical low-sodium aluminum hydroxide powder prepared by this invention is significantly superior to existing products in terms of morphological regularity, surface smoothness, degree of edge blunting, and particle uniformity. This verifies the technical effect of this invention in preparing spherical low-sodium aluminum hydroxide powder in situ without the need for a post-particle shaping process.
[0187] In summary, in comparison Figure 1 , Figure 2 and Figure 3It can be concluded that the spherical aluminum hydroxide microcrystalline slurry prepared by the in-situ growth technology of spherical induced crystal seeds in this invention ( Figure 1 It has a rounded, smooth, and uniform spherical morphology, which is effectively inherited and evolved during subsequent seed crystal decomposition. Figure 2 The final product is a spherical low-sodium aluminum hydroxide powder. Figure 2 ) and existing thermally conductive aluminum hydroxide powders on the market ( Figure 3 Compared to other materials, it exhibits significant advantages in terms of particle morphology regularity, surface smoothness, edge blunting, and packing method. These morphological differences directly correspond to the high filler compatibility, low viscosity processability, high thermal conductivity network construction ability, and high interfacial bonding strength of near-spherical low-sodium aluminum hydroxide powder in thermally conductive composites. This solves the technical problem in existing technologies where the irregular morphology and protruding edges of aluminum hydroxide powder limit the performance of thermally conductive composites.
[0188] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for preparing spherical low-sodium aluminum hydroxide powder, characterized in that, Includes the following steps: Urea solution is added to aluminum sulfate solution and mixed to obtain urea-aluminum sulfate mixed solution; At a temperature of 40℃~60℃, refined sodium aluminate solution is added to the urea-aluminum sulfate mixed solution until the pH value of the urea-aluminum sulfate mixed solution is 7~10; The urea-aluminum sulfate mixed solution with a pH of 7-10 is chemically reacted at a temperature of 80-90°C for 2-4 hours to obtain a spherical aluminum hydroxide microcrystalline slurry. The spherical aluminum hydroxide microcrystalline slurry was added as a seed crystal to a refined sodium aluminate solution for seed crystal decomposition to obtain aluminum hydroxide slurry. The seed crystal decomposition adopted a gradient slow cooling temperature control method, with an initial decomposition temperature of 65℃~80℃ and a decomposition termination temperature of 53℃~55℃. The seed crystal decomposition adopted a low shear force stirring method. The aluminum hydroxide slurry is subjected to hydrocyclone classification to obtain coarse-particle aluminum hydroxide slurry and fine-particle aluminum hydroxide slurry. The coarse-particle-size aluminum hydroxide slurry is subjected to solid-liquid separation to obtain aluminum hydroxide filter cake; The aluminum hydroxide filter cake is washed and dried; The washing process involves deep sodium removal in a hot water-assisted ammonium salt system. The dried aluminum hydroxide filter cake is subjected to dry classification to remove large particles and obtain spherical low-sodium aluminum hydroxide powder.
2. The preparation method according to claim 1, characterized in that, The concentration of the urea solution is 40 g / L to 70 g / L, and the concentration of the aluminum sulfate solution is 40 g / L to 70 g / L.
3. The preparation method according to claim 2, characterized in that, The urea in the urea solution and the Al in the aluminum sulfate solution 3+ The molar ratio is 10:1 to 12:
1.
4. The preparation method according to claim 1, characterized in that, The refined sodium aluminate solution is prepared from industrial aluminum hydroxide or bauxite through alkaline dissolution, lime milk purification, deep filtration and impurity removal and desilication processes. The alumina concentration of the refined sodium aluminate solution is 70 g / L to 140 g / L, and the caustic ratio αK is 1.4 to 2.
5.
5. The preparation method according to claim 1, characterized in that, The initial seed ratio for the decomposition of the crystals is 5%, the decomposition time is 48h to 72h, and the solid content of the decomposition is 200g / L to 500g / L.
6. The preparation method according to claim 1, characterized in that, The stirring speed of the low shear force stirring method shall not exceed 250 r / min.
7. The preparation method according to claim 1, characterized in that, The ammonium salt used in the hot water-assisted ammonium salt deep desodium removal is at least one of ammonium acetate, ammonium chloride, and ammonium sulfate, and the amount of the ammonium salt used is 100ppm to 300ppm.
8. The preparation method according to claim 1, characterized in that, The dry classification method employs an airflow classification process. The fine-particle aluminum hydroxide obtained by dry classification is packaged as a thermally conductive, spherical, low-sodium aluminum hydroxide product, while the coarse-particle aluminum hydroxide obtained by dry classification is used for catalysis.
9. A spherical low-sodium aluminum hydroxide powder, characterized in that, Prepared by the preparation method according to any one of claims 1 to 8; The spherical low-sodium aluminum hydroxide powder has an in-situ grown spherical particle morphology. The spherical low-sodium aluminum hydroxide powder has a sodium oxide mass fraction of no more than 0.1 wt%, a median particle size D50 of 40 μm to 75 μm, and an oil absorption rate of no more than 22 mL / 100 g.
10. The application of the near-spherical low-sodium aluminum hydroxide powder of claim 9 as a thermally conductive filler, characterized in that, The spherical low-sodium aluminum hydroxide powder is used as an inorganic thermally conductive and insulating filler in thermally conductive silicone, epoxy thermally conductive potting compound, thermally conductive modified plastic, and heat dissipation polymer composite material for power batteries of new energy vehicles.