A composite graphitic carbon nitride gas-sensitive material, its preparation method and application
By preparing a composite material of ZrO2 and graphitic carbon nitride (g-C3N4), the problem of insufficient sensitivity of composite graphitic carbon nitride gas-sensitive materials for NO2 detection was solved, achieving high sensitivity and stability of NO2 detection, suitable for room temperature detection.
Patent Information
- Application Number
- CN202611006599.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-07
- Publication Date
- 2026-11-10
AI Technical Summary
Existing composite graphitic carbon nitride (g-C3N4) gas-sensitive materials have insufficient sensitivity and stability for NO2 detection, making it difficult to meet practical detection needs.
ZrO2 was obtained by hydrothermal synthesis of UiO-66 metal-organic framework material and calcination. ZrO2 was then combined with graphitic carbon nitride (g-C3N4) to prepare a composite graphitic carbon nitride gas-sensitive material. The synergistic effect of ZrO2 and g-C3N4 formed a heterojunction interface, which enhanced the gas adsorption and carrier transport efficiency.
The detection performance of the gas-sensitive material for NO2 has been improved, with the detection limit reduced to 10 ppb, short response time, and significantly improved sensitivity and stability, making it suitable for room temperature detection.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of gas-sensitive materials technology, specifically relating to a composite graphite carbon nitride gas-sensitive material, its preparation method, and its application. Background Technology
[0002] In the context of industrialization, nitrogen dioxide (NO2), a typical toxic gas released during fuel combustion, poses a significant threat to both the ecological environment and human health. This reddish-brown gas with a pungent odor is not only a major contributor to environmental problems such as acid rain and photochemical smog, but also a direct factor endangering human health. Even at low concentrations, NO2 can irritate the throat and respiratory system, and long-term exposure can lead to a range of serious health problems, including irreversible lung damage. Therefore, developing sensors capable of detecting low concentrations of NO2 with high sensitivity and selectivity at room temperature is crucial.
[0003] Metal-organic frameworks (MOFs) are a class of crystalline porous materials with periodic network structures, formed through the self-assembly and interconnection of metal centers and bridging organic ligands. Their high porosity and extremely large specific surface area make them widely used in catalysis, gas storage, drug delivery, and sensing. Metal oxides prepared using MOFs as precursors not only retain the advantages of MOFs but also exhibit higher stability. Porous and hollow structures obtained through MOF pyrolysis have become highly attractive gas sensing materials. Metal oxide semiconductors (MOS), such as zinc oxide, tungsten trioxide, and copper oxide, play a crucial role in detecting toxic gases. These materials are favored due to their simple synthesis, excellent stability, rapid response, and low cost. UiO-66 possesses a highly ordered crystal structure, and its conversion product, zirconium dioxide, retains a certain degree of order. This ordered structure helps improve the material's stability and performance. Zirconium dioxide derived from UiO-66 not only retains the porosity characteristics of the original structure but also benefits from its high specific surface area and porosity, significantly enhancing gas adsorption capacity and sensing efficiency.
[0004] Graphitic carbon nitride (g-C3N4) is a two-dimensional layered carbon-nitrogen material with a graphene-like structure and a tunable band gap (ranging from 2.5 to 2.8 eV). This material consists of graphene-like hexagonal rings composed of alternating carbon and nitrogen atoms, forming a stable planar structure with a large specific surface area, abundant nitrogen functional groups, and excellent chemical stability. These properties make g-C3N4 a promising candidate for applications in photocatalysis, electrochemistry, and gas sensing. Its high specific surface area significantly enhances gas adsorption capacity, thereby improving the sensitivity and response speed of sensors; simultaneously, its good chemical stability ensures stable performance under various conditions.
[0005] However, the detection sensitivity of composite graphitic carbon nitride (g-C3N4) gas-sensitive materials for NO2 still needs further improvement, and their stability in practical detection applications is insufficient to meet actual needs. Therefore, the overall detection performance of composite graphitic carbon nitride (g-C3N4) gas-sensitive materials requires further research and improvement. Summary of the Invention
[0006] To address the aforementioned problems, this invention provides a composite graphitic carbon nitride gas-sensitive material, which is obtained by combining ZrO2 obtained from hydrothermally synthesized UiO-66 metal-organic framework material with graphitic carbon nitride (g-C3N4) after calcination. This composite graphitic carbon nitride gas-sensitive material not only exhibits improved stability and a reduced detection limit to 10 ppb, but also demonstrates a short response time, significantly enhancing its overall NO2 detection performance to meet the needs of practical detection applications.
[0007] The purpose of this invention is to provide a composite graphitic carbon nitride gas-sensitive material, which is prepared by heating and reacting raw materials including ZrO2 and graphitic carbon nitride (g-C3N4) in solvent B.
[0008] The ZrO2 is obtained by calcining UiO-66 metal-organic framework material. The calcination temperature is 300-600℃, preferably 350-550℃, and more preferably 400-500℃. The calcination time is 2-5h, preferably 2.5-4.5h, and more preferably 3-4h.
[0009] The graphitic carbon nitride is obtained by solvothermal reaction of raw materials including melamine and phosphoric acid to obtain a graphitic carbon nitride precursor, which is then heated under solvent conditions, and the resulting product is calcined.
[0010] The present invention also aims to provide a method for preparing the composite graphitic carbon nitride gas-sensitive material, wherein the method involves reacting raw materials including ZrO2 and graphitic carbon nitride (g-C3N4) in solvent B by heating.
[0011] The method specifically includes the following steps:
[0012] Step 1: Obtain ZrO2;
[0013] Step 2: Obtain graphite carbon nitride;
[0014] Step 3: Add ZrO2 and graphite carbon nitride to solvent B, heat to react, and after the reaction is complete, separate the product, wash and dry it to obtain composite graphite carbon nitride gas-sensitive material.
[0015] The third aspect of this invention aims to provide the use of the composite graphitic carbon nitride gas-sensitive material for preparing a gas-sensitive element for detecting nitrogen dioxide.
[0016] The fourth aspect of this invention aims to provide a gas-sensitive element for detecting nitrogen dioxide. Its detection limit for nitrogen dioxide is 0.01 ppm, and at a concentration of 0.01 ppm, the response time is within 60 seconds.
[0017] The present invention has the following beneficial effects:
[0018] (1) The composite graphitic carbon nitride gas-sensitive material has excellent nitrogen dioxide detection performance. It has oxygen vacancy enrichment, reasonable pore structure design and synergistic effect of heterojunction. These factors together enhance the gas adsorption / activation process and carrier transport efficiency, effectively overcome the limitations of traditional sensing technology, and open up new avenues for the development of new high-performance gas sensors.
[0019] (2) This invention successfully achieved uniform dispersion of ZrO2 on the surface of ultrathin porous g-C3N4 nanomaterials through hydroxyl-induced self-assembly design. In the prepared composite graphitic carbon nitride gas-sensitive material, the calcined ZrO2 not only retains the three-dimensional porous framework of UiO-66 nanomaterials, but also significantly improves the gas-sensing performance by utilizing the high specific surface area and abundant pores of g-C3N4.
[0020] (3) Experimental data show that the composite graphite carbon nitride gas-sensitive material has excellent gas-sensing properties for NO2 at room temperature. Its high specific surface area provides abundant gas adsorption and reactive active sites; its excellent pore structure, ideal pore size distribution and pore volume characteristics establish efficient channels for the rapid diffusion of gas molecules; at the same time, the heterojunction interface formed by g-C3N4 and ZrO2 significantly improves the carrier transport efficiency. The synergistic effect of the above multiple factors makes the NO2 gas-sensing performance of the composite graphite carbon nitride gas-sensitive material significantly enhanced.
[0021] (4) The gas sensing element made from the composite graphite carbon nitride gas sensing material provided by the present invention exhibits excellent sensing performance for NO2 at room temperature: the sensitivity to 100 ppm NO2 reaches 62, the response and recovery times are 3.1 seconds and 13.2 seconds, respectively, and the detection limit is as low as 10 ppb. Attached Figure Description
[0022] Figure 1 The X-ray diffraction pattern of the composite graphitic carbon nitride gas-sensitive material I prepared in Example 1 is shown;
[0023] Figure 2 The image shows a scanning electron microscope (SEM) image of the composite graphitic carbon nitride gas-sensitive material I prepared in Example 1.
[0024] Figure 3 The image shown is a transmission electron microscope (TEM) image of the composite graphitic carbon nitride gas-sensitive material I prepared in Example 1.
[0025] Figure 4 This shows a high-resolution transmission electron microscope image of the composite graphitic carbon nitride gas-sensitive material I prepared in Example 1;
[0026] Figure 5 The accompanying diagram shows the NO2 adsorption and desorption of the composite graphite carbon nitride gas-sensitive material I prepared in Example 1;
[0027] Figure 6 The Mott-Schottky curves of the UiO-66, g-C3N4, ZrO2, and ZC materials prepared in Example 1 are shown.
[0028] Figure 7 The graph shows the response curve of the gas-sensitive element I prepared in Example 1 to the nitrogen dioxide gas gradient.
[0029] Figure 8 The sensitivity comparison diagram of the gas-sensitive element I prepared in Example 1 for detecting nitrogen dioxide under different relative humidities is shown.
[0030] Figure 9 The sensitivity change of the gas-sensitive element I prepared in Example 1 is shown in the test results over 1-12 weeks;
[0031] Figure 10 The diagram shows a comparison of the response properties of the gas-sensitive element I of the present invention at a detection temperature of 25 °C and a detection humidity of 25% (relative humidity) to the detection of 100 ppm NO2 (This work in the figure) with those of a previously disclosed NO2 detection gas-sensitive material. Detailed Implementation
[0032] The present invention will now be described in detail through specific embodiments, and the features and advantages of the present invention will become clearer and more explicit with these descriptions.
[0033] This invention provides a composite graphitic carbon nitride gas-sensitive material, which is prepared by heating and reacting raw materials including ZrO2 and graphitic carbon nitride (g-C3N4) in solvent B.
[0034] The ZrO2 is obtained by calcining UiO-66 metal-organic framework material. The calcination temperature is 300-600℃, preferably 350-550℃, and more preferably 400-500℃. The calcination time is 2-5h, preferably 2.5-4.5h, and more preferably 3-4h.
[0035] The graphitic carbon nitride is obtained by solvothermal reaction of raw materials including melamine and phosphoric acid to obtain a graphitic carbon nitride precursor, which is then heated under solvent conditions, and the resulting product is calcined.
[0036] The present invention also provides a method for preparing the composite graphitic carbon nitride gas-sensitive material, wherein the method comprises ZrO2 and graphitic carbon nitride (g-C3N4) as raw materials, which are heated and reacted in solvent B.
[0037] The method specifically includes the following steps:
[0038] Step 1: Prepare ZrO2.
[0039] The ZrO2 is obtained by calcining UiO-66 metal-organic framework material. The calcination temperature is 300-600℃, preferably 350-550℃, and more preferably 400-500℃. The calcination time is 2-5h, preferably 2.5-4.5h, and more preferably 3-4h. The calcination atmosphere is an oxygen-containing atmosphere, such as air. The above-mentioned calcination temperature affects key parameters such as the ZrO2 phase, particle size, specific surface area, and defect concentration. If the temperature is too low, organic ligands may not be completely removed, resulting in poor ZrO2 crystallinity, high specific surface area but unstable structure, and weak electron transport capacity, which is not conducive to gas-sensitive reactions. If the temperature is too high, ZrO2 grains grow significantly and agglomerate, and the specific surface area and porosity decrease sharply, leading to a reduction in gas adsorption and reactive active sites. At the same time, a suitable temperature helps to form a stable phase and retain appropriate structural defects (such as oxygen vacancies), which can serve as active centers for gas adsorption and improve response sensitivity.
[0040] The UiO-66 metal-organic framework material is obtained by adding terephthalic acid solution to zirconium salt solution, heating the reaction in a sealed reactor, and then post-processing.
[0041] The solvent for the terephthalic acid solution is one or more of alcohol solvents and amide solvents, preferably one or more of ethanol, ethylene glycol, N,N-dimethylformamide and N,N-dimethylacetamide, more preferably N,N-dimethylformamide and / or N,N-dimethylacetamide, such as N,N-dimethylformamide.
[0042] The terephthalic acid solution has a terephthalic acid concentration of 0.01-0.07 mol / L, preferably 0.02-0.06 mol / L, and more preferably 0.03-0.05 mol / L.
[0043] The solvent for the zirconium salt solution is one or more of alcohols and amides, preferably one or more of N,N-dimethylformamide and / or N,N-dimethylacetamide, more preferably N,N-dimethylformamide. The solvent mainly affects the crystallinity, morphology, and size of UiO-66 by influencing the solubility, coordination environment, and reaction rate of the reactants. N,N-dimethylformamide (DMF) has a high boiling point and good coordination ability, which is more conducive to the formation of a highly crystalline framework under solvothermal conditions. If alcohols (such as ethanol) are used as substitutes or mixtures, the crystal growth rate may change due to differences in coordination ability and boiling point, resulting in products with smaller particle sizes or different morphologies. This will affect the particle size and agglomeration degree of ZrO2 after calcination. In gas-sensitive applications, ZrO2 with uniform size and good dispersibility is beneficial for uniformly compounding with g-C3N4 to form a stable heterogeneous interface, which is crucial for improving sensitivity and stability.
[0044] The zirconium salt is selected from one or more of zirconium chloride, zirconium bromide, zirconium sulfate, zirconium nitrate and zirconium oxychloride octahydrate, preferably one or more of zirconium chloride, zirconium bromide and zirconium nitrate, and more preferably zirconium chloride.
[0045] Preferably, the zirconium salt solution contains a carboxylic acid regulator B, selected from one or more monocarboxylic and dicarboxylic acids, preferably one or two of formic acid, acetic acid, and benzoic acid, and more preferably acetic acid. In the synthesis of UiO-66, it can compete with zirconium clusters for coordination, regulating crystal nucleation and growth rates through a "coordination regulation" mechanism. This effectively controls crystal size and morphology and introduces structural defects (such as missing linker defects), which is beneficial for enhancing interfacial interactions and electron transfer efficiency during subsequent complexation with g-C3N4, ultimately improving gas-sensing performance. The carboxylic acid regulator B, acting as a "modulator," competes with terephthalic acid for coordination sites of zirconium clusters, slowing down the nucleation and growth rate of the framework, thereby effectively controlling crystal size, reducing agglomeration, and making the crystal morphology more regular. More importantly, it can induce "missing linker" type defects, increasing the proportion of mesoporous sites and unsaturated coordinated zirconium sites within the framework. These sites contribute to the formation of ZrO2 with higher specific surface area and more active oxygen species during calcination. Acetic acid has an even better effect. Optimizing the dosage of carboxylic acid regulator B is key to balancing crystallinity and defect concentration, directly affecting the final gas adsorption and catalytic activity of ZrO2, thereby improving the sensing performance of the composite material.
[0046] The zirconium salt concentration in the zirconium salt solution is 0.016-0.04 mol / L, preferably 0.02-0.036 mol / L, and more preferably 0.024-0.032 mol / L.
[0047] The volume molar ratio of the carboxylic acid regulator B to the zirconium salt is (5-7) mL:(0.65-1.40) mmol, preferably (5-7) mL:(0.75-1.20) mmol, and more preferably (5-7) mL:(0.85-1.00) mmol.
[0048] Preferably, the terephthalic acid solution is added to the zirconium salt solution dropwise. Stirring is continued for 30-90 minutes, preferably 40-80 minutes, and more preferably 50-70 minutes.
[0049] The high-pressure heating reaction is preferably carried out in a high-pressure reactor lined with polytetrafluoroethylene. The reaction temperature is 105-135℃, preferably 110-130℃, and more preferably 115-125℃. The reaction time is 4-14h, preferably 5-12h, and more preferably 6-10h. The reaction temperature and time affect the core parameters of UiO-66 crystal nucleation, growth rate, final crystallinity, particle size, and morphology. At lower temperatures or shorter times, crystal growth is incomplete, and the product may have low crystallinity, low yield, or even contain unreacted precursors. As the temperature increases and the time prolongs, the crystals gradually grow and the crystallinity improves, but excessively high temperatures or excessively long times may lead to excessive grain growth, agglomeration, and a decrease in specific surface area. This directly determines the particle size, specific surface area, and porosity characteristics of the calcined ZrO2. Optimizing this step to obtain UiO-66 with high specific surface area, small particle size, and abundant mesopores is a prerequisite for finally obtaining high-performance ZrO2 gas-sensitive materials.
[0050] Step 2: Obtain graphite carbon nitride.
[0051] The graphitic carbon nitride is obtained by solvothermal reaction of raw materials including melamine and phosphoric acid to obtain a graphitic carbon nitride precursor, which is then heated under solvent conditions, and the resulting product is calcined.
[0052] Melamine and phosphoric acid are added to water and stirred at 65-95°C for 0.5-3 hours, preferably at 70-90°C for 0.5-2.5 hours, and more preferably at 75-85°C for 1-2 hours. The mixture is then transferred to a high-pressure reactor for a solvothermal reaction at a temperature of 165-195°C, preferably 170-190°C, and more preferably 175-185°C for 7-15 hours, preferably 8-13 hours, and more preferably 9-11 hours. The solvothermal reaction temperature and time directly affect the assembly structure and chemical composition of the melamine-phosphoric acid supramolecular precursor. Suitable temperature and time facilitate the orderly self-assembly of melamine and phosphoric acid through hydrogen bonds and other forces, forming a supramolecular precursor with a specific two-dimensional morphology. This process also involves partial hydrolysis or condensation of melamine. Too low a temperature or too short a time results in insufficient assembly or incomplete reaction, affecting the precursor structure; too high a temperature or too long a time may lead to excessive condensation or structural collapse of the precursor. The structure of the precursor directly determines the morphology (such as whether ultrathin nanosheets can be obtained), specific surface area, defect degree and degree of polymerization of g-C3N4 obtained by subsequent calcination, which in turn affects its composite effect with ZrO2 and the final gas-sensing performance.
[0053] The mass ratio of melamine to phosphoric acid is 1:(1-2.4), preferably 1:(1-2.0), and more preferably 1:(1-1.6). The concentration of phosphoric acid is 70-85 wt%, preferably 75-85 wt%, and more preferably 80-85 wt%. The ratio of melamine to phosphoric acid affects the composition and structural stability of the supramolecular precursor. Phosphoric acid acts as a "dopant" and "structure directing agent," and its content affects the layered assembly structure and hydrogen bond network of the precursor. A suitable ratio helps to form a stable layered supramolecular structure, and after heat treatment and exfoliation, thinner g-C3N4 nanosheets with a larger specific surface area can be obtained. If the proportion of phosphoric acid is too low, the layered structure of g-C3N4 may not be effectively exfoliated; if the proportion is too high, too much phosphorus-containing impurity may be introduced during calcination or the basic structural units of g-C3N4 may be destroyed, affecting its semiconductor properties.
[0054] The water is preferably deionized water or distilled water, more preferably deionized water.
[0055] The mass-to-volume ratio of melamine to water is 1 g:(40-150) mL, preferably 1 g:(50-130) mL, and more preferably 1 g:(60-110) mL. Water serves as the reaction medium, and its amount affects the solubility and concentration of the reactants, thus influencing the nucleation and growth kinetics of the supramolecular precursor. Insufficient water may result in incomplete dissolution and uniform mixing of melamine and phosphoric acid, affecting the homogeneity of the precursor; excessive water will reduce the reactant concentration, potentially leading to a decrease in yield or requiring a longer reaction time. Within a suitable range, the amount of water primarily affects the mass transfer efficiency of the reaction system and the particle size distribution of the final product, thereby affecting the performance of the composite material.
[0056] After the reaction is complete, the product is separated, washed with deionized water until neutral, and dried, preferably at 60-80℃ for 6-12 hours, to obtain the graphitic carbon nitride precursor.
[0057] The graphitic carbon nitride precursor is uniformly dispersed in solvent A, heated to react, and then centrifuged and dried. Solvent A is one or more alcohol solvents, preferably one or more of liquid monohydric alcohols, liquid dihydric alcohols, and liquid trihydric alcohols, more preferably a mixture of glycerol and ethanol. The volume ratio of glycerol to ethanol is 1:(1-7), preferably 1:(1-6), more preferably 1:(2-5). The mixture of glycerol and ethanol is commonly used for the exfoliation and dispersion of g-C3N4. Ethanol helps wet and disperse the precursor, while glycerol, as a high-boiling-point solvent, provides a mild liquid-phase exfoliation environment under reflux conditions and may form hydrogen bonds with the precursor surface through its hydroxyl groups, assisting in the exfoliation to obtain thinner nanosheets, thereby facilitating gas adsorption and improving the gas-sensitive properties of the composite material.
[0058] The mass ratio of the graphite carbon nitride precursor to solvent A is 0.6:(9-40), preferably 0.6:(12-35), and more preferably 0.6:(15-30).
[0059] The heating reaction temperature is 75-105℃, preferably 80-100℃, more preferably 85-95℃, and the reaction time is 1-4h, preferably 1.5-3.5h, more preferably 2-3h. The drying temperature is 60-100℃, preferably 65-95℃, more preferably 70-90℃, and the drying time is 4-16h, preferably 5-14h, more preferably 6-12h. By optimizing the reaction temperature and time, the exfoliation state and specific surface area of the nanosheets can be maintained to the maximum extent, ensuring that the final g-C3N4 product has a highly active surface, thereby forming a high-quality heterogeneous interface with ZrO2 during composite formation and improving gas-sensing performance.
[0060] The calcination temperature is 300-600℃, preferably 350-550℃, and more preferably 400-500℃; the calcination time is 1-5h, preferably 1.5-4h, and more preferably 2-3h. Calcination is a key step in the thermal polymerization to form g-C3N4. Temperature determines the degree of condensation of the precursor and the degree of polymerization of the product. If the calcination temperature is too low, condensation will be insufficient, and the product may contain a large number of unpolymerized intermediates and have poor crystallinity; if the temperature is too high, the g-C3N4 structure may partially decompose, carbonization will be intensified, and its electronic structure and band structure will be affected. Time affects the completion of the condensation reaction; if the time is too short, the product will be impure, and if the time is too long, it may cause excessive condensation and structural degradation. Optimizing the calcination conditions can obtain g-C3N4 nanosheets with suitable specific surface area, good crystallinity, and stable band structure, which is crucial for the sensitivity and selectivity of subsequent composite materials.
[0061] Step 3: Add ZrO2 and graphite carbon nitride to solvent B, heat to react, and after the reaction is complete, separate the product, wash and dry it to obtain composite graphite carbon nitride gas-sensitive material.
[0062] The mass ratio of graphitic carbon nitride to ZrO2 is 1:(1.1-3.1), preferably 1:(1.2-2.8), and more preferably 1:(1.3-2.5). This ratio directly determines the number and distribution of heterojunctions in the composite material, significantly affecting gas-sensing performance. When the graphitic carbon nitride content is too low, the active sites on the ZrO2 surface are excessively covered, or the conductive pathways provided by graphitic carbon nitride are insufficient, resulting in excessively high resistance and a weak response signal. When the graphitic carbon nitride content is too high, the relative proportion of ZrO2 as the main gas-sensing reaction center decreases, and the insulation or low conductivity of graphitic carbon nitride may also hinder carrier transport, similarly reducing sensitivity. The optimal ratio aims to construct an optimal "reaction-conduction" synergistic interface, where ZrO2 provides gas adsorption and reactive active centers, and g-C3N4 provides electron transfer channels and a heterojunction interface, jointly improving sensitivity and response speed.
[0063] Solvent B is selected from one or more alcohol solvents, preferably one or more of methanol, ethanol, propanol, and butanol, and more preferably ethanol. As a dispersion medium, the alcohol solvent helps to achieve uniform dispersion of ZrO2 and g-C3N4 nanoparticles, facilitating close contact and assembly between the two through interactions such as hydroxyl groups.
[0064] The heating reaction temperature is 50-90℃, preferably 55-85℃, more preferably 60-80℃, and the time is 0.5-4h, preferably 0.8-3.5h, more preferably 1-3h. The purpose of heating is to provide sufficient thermal energy to the ZrO2 and g-C3N4 nanosheets to promote hydroxyl condensation or other chemical bonding between their interfaces, enhance the interfacial bonding strength, and form a stable heterostructure. If the temperature is too low (e.g., room temperature), the interfacial bonding mainly relies on physical adsorption, which is weak and unstable, affecting the stability of the device; if the temperature is too high, it may introduce unnecessary side reactions or cause the nanosheets to recombine. If the time is too short, the recombination is insufficient; if it is too long, there is no additional benefit. Optimizing this step aims to construct a robust and efficient ZrO2 / g-C3N4 heterointerface, which is crucial for achieving a rapid and stable gas-sensitive response.
[0065] The drying temperature is 50-90℃, preferably 55-85℃, more preferably 60-80℃, and the drying time is 4-16h, preferably 6-14h, more preferably 8-12h.
[0066] This invention also provides the use of the composite graphitic carbon nitride gas-sensitive material for preparing a gas-sensitive element for detecting nitrogen dioxide. A suspension of the composite graphitic carbon nitride gas-sensitive material is coated onto an Au interdigitated electrode, and after drying, a gas-sensitive element for detecting nitrogen dioxide is obtained.
[0067] The present invention also provides a gas-sensitive element for detecting nitrogen dioxide, which is obtained by coating a suspension of the composite graphite carbon nitride gas-sensitive material onto an Au interdigitated electrode and then drying it.
[0068] The gas-sensitive element used for detecting nitrogen dioxide has a detection limit of 0.01 ppm. At a concentration of 0.01 ppm, the response time is within 60 seconds.
[0069] Example
[0070] Example 1
[0071] 0.23 g of zirconium tetrachloride was dissolved in 25 ml of N,N-dimethylformamide and stirred until mixed. Then, 6 ml of acetic acid was added and stirred for 15 min to obtain mixture 1. Separately, 0.17 g of terephthalic acid was dissolved in 25 ml of N,N-dimethylformamide and stirred until homogeneous to obtain mixture 2. After both solutions were completely dissolved, mixture 2 was added dropwise to mixture 1 at a uniform rate and stirring was continued for 60 min. The thoroughly mixed solution was then transferred to a reaction vessel (a closed polytetrafluoroethylene reaction vessel) and heated at 120 °C for 24 h. The resulting liquid was ultrasonically washed with N,N-dimethylformamide and then dried in a vacuum oven at 80 °C for 12 h to obtain UiO-66 metal-organic framework material I.
[0072] The UiO-66 metal-organic framework material obtained above was placed in a muffle furnace and calcined at 450 °C for 4 h to obtain pure phase ZrO2Ⅰ.
[0073] 1.0 g of melamine and 1.2 g of phosphoric acid (85 wt%) were added to 100 ml of deionized water and stirred at 80 °C for 1 h to dissolve. The solution was then transferred to a reaction vessel (a closed polytetrafluoroethylene reaction vessel) and reacted at 180 °C for 10 h. After the reaction, the solution was washed with deionized water until neutral and then dried in an oven at 60 °C for 12 h to obtain the supramolecular layer g-C3N4 precursor. 0.6 g of the supramolecular layer g-C3N4 precursor was dispersed in a mixture of 5 ml glycerol and 15 ml ethanol. After sonication for 30 min, the solution was reacted in an oil bath at 90 °C for 3 h. The resulting solution was then added to an appropriate amount of anhydrous ethanol, centrifuged and washed, and dried in a vacuum drying oven at 60 °C for 6 h. The product was calcined in a muffle furnace at 500 °C for 2 h to obtain g-C3N4 nanosheets I (denoted as CNI).
[0074] 1.2 g CNⅠ and 1.8 g ZrO2Ⅰ were added to 60 mL of anhydrous ethanol and sonicated for 30 min to disperse them evenly. Then, the mixture was reacted at 80 ℃ for 2 h under oil bath heating conditions. After the reaction was completed, the mixture was allowed to stand, the supernatant was poured off, and the bottom product was separated. The product was washed with deionized water and dried in a vacuum drying oven at 60 ℃ for 12 h to obtain composite graphite carbon nitride gas-sensitive material Ⅰ.
[0075] Example 2
[0076] 0.22 g of zirconium tetrachloride was dissolved in 25 ml of N,N-dimethylformamide and stirred until mixed. Then, 6 ml of acetic acid was added, and the mixture was stirred for 20 min to obtain mixture 1. Separately, 0.17 g of terephthalic acid was dissolved in 26 ml of N,N-dimethylformamide and stirred until homogeneous to obtain mixture 2. After both solutions were completely dissolved, mixture 2 was added dropwise to mixture 1 at a uniform rate, and the mixture was stirred for another 60 min. The thoroughly mixed solution was then transferred to a reaction vessel (a closed polytetrafluoroethylene reaction vessel) and heated at 120 °C for 12 h. The resulting liquid was ultrasonically washed with N,N-dimethylformamide and then dried in a vacuum oven at 80 °C for 6 h to obtain UiO-66 metal-organic framework material II.
[0077] The UiO-66 metal-organic framework material II obtained above was placed in a muffle furnace and calcined at 450 °C for 4 h to obtain pure phase ZrO2II.
[0078] 1 g of melamine and 1.3 g of phosphoric acid (85 wt%) were added to 80 ml of deionized water and stirred at 80 °C for 1 h to dissolve them. The solution was then transferred to a reaction vessel (a closed polytetrafluoroethylene reaction vessel) and reacted at 180 °C for 10 h. After the reaction, the solution was washed with deionized water until neutral and dried in an oven at 60 °C for 12 h to obtain supramolecular layered g-C3N4 precursor II. 0.6 g of supramolecular layered g-C3N4 precursor II was dispersed in a mixture of 5 ml glycerol and 10 ml ethanol. After sonication for 30 min, the solution was reacted in an oil bath at 90 °C for 3 h. An appropriate amount of anhydrous ethanol was added to the resulting solution, and after centrifugation and washing, the solution was dried in a vacuum drying oven at 80 °C for 6 h. The product was calcined in a muffle furnace at 500 °C for 2 h to obtain g-C3N4 nanosheets II (denoted as CNII).
[0079] 0.6 g CNⅡ and 1.2 g ZrO2Ⅱ were added to 60 mL of anhydrous ethanol and sonicated for 30 min to disperse them evenly. Then, the mixture was reacted at 80 ℃ for 1 h in an oil bath. After the reaction was completed, the mixture was allowed to stand, the supernatant was poured off, and the bottom product was separated. The product was washed with deionized water and dried in a vacuum drying oven at 60 ℃ for 12 h to obtain composite graphite carbon nitride gas-sensitive material Ⅱ.
[0080] Example 3
[0081] 0.21 g of zirconium tetrachloride was dissolved in 30 ml of N,N-dimethylformamide and stirred until mixed. Then, 5 ml of acetic acid was added, and the mixture was stirred for 20 min to obtain mixture 1. Separately, 0.18 g of terephthalic acid was dissolved in 25 ml of N,N-dimethylformamide and stirred until homogeneous to obtain mixture 2. After both solutions were completely dissolved, mixture 2 was added dropwise to mixture 1 at a uniform rate, and the mixture was stirred for another 60 min. The thoroughly mixed solution was then transferred to a reaction vessel (a closed polytetrafluoroethylene reaction vessel) and heated at 120 °C for 8 h. The resulting liquid was ultrasonically washed with N,N-dimethylformamide and then dried in a vacuum oven at 60 °C for 6 h to obtain UiO-66 metal-organic framework material III.
[0082] The UiO-66 metal-organic framework material III obtained above was placed in a muffle furnace and calcined at 500 °C for 4 h to obtain pure phase ZrO2III.
[0083] 1.2 g of melamine and 1.6 g of phosphoric acid (85 wt%) were added to 80 ml of deionized water and stirred at 80 °C for 1 h to dissolve. The solution was then transferred to a reaction vessel (a closed polytetrafluoroethylene reaction vessel) and reacted at 180 °C for 10 h. After the reaction, the solution was washed with deionized water until neutral and dried in an oven at 60 °C for 12 h to obtain g-C3N4 precursor III. 0.7 g of supramolecular layered g-C3N4 precursor III was dispersed in a mixture of 5 ml glycerol and 20 ml ethanol. After sonication for 30 min, the solution was reacted in an oil bath at 90 °C for 2 h. An appropriate amount of anhydrous ethanol was added to the resulting solution, and after centrifugation and washing, the solution was dried in a vacuum drying oven at 80 °C for 8 h. The product was calcined in a muffle furnace at 500 °C for 3 h to obtain g-C3N4 nanosheets III (denoted as CNⅢ).
[0084] 0.7 g CNⅢ and 1.4 g ZrO2Ⅲ were added to 55 mL of anhydrous ethanol and sonicated for 30 min to disperse them evenly. Then, the mixture was reacted at 80 °C for 2 h in an oil bath. After the reaction was completed, the mixture was allowed to stand, the supernatant was poured off, and the bottom product was separated. The product was washed with deionized water and dried in a vacuum drying oven at 60 °C for 10 h to obtain composite graphite carbon nitride gas-sensitive material Ⅲ.
[0085] Example 4
[0086] 0.23 g of zirconium tetrachloride was dissolved in 30 ml of N,N-dimethylformamide and stirred until mixed. Then, 7 ml of acetic acid was added and stirred for 20 min to obtain mixture 1. Separately, 0.21 g of terephthalic acid was dissolved in 30 ml of N,N-dimethylformamide and stirred until homogeneous to obtain mixture 2. After both solutions were completely dissolved, mixture 2 was added dropwise to mixture 1 at a uniform rate and stirring was continued for 60 min. The thoroughly mixed solution was then transferred to a reaction vessel (a closed polytetrafluoroethylene reaction vessel) and heated at 120 °C for 10 h. The resulting liquid was ultrasonically washed with N,N-dimethylformamide and then dried in a vacuum oven at 100 °C for 6 h to obtain UiO-66 metal-organic framework material IV.
[0087] The UiO-66 metal-organic framework material IV obtained above was placed in a muffle furnace and calcined at 400 °C for 3 h to obtain pure phase ZrO2 IV.
[0088] 0.8 g of melamine and 1.2 g of phosphoric acid (85 wt%) were added to 70 ml of deionized water and stirred at 80 °C for 1 h to dissolve. The solution was then transferred to a reaction vessel (a closed polytetrafluoroethylene reaction vessel) and reacted at 180 °C for 10 h. After the reaction, the solution was washed with deionized water until neutral and dried in an oven at 60 °C for 12 h to obtain supramolecular layered g-C3N4 precursor IV. 0.8 g of supramolecular layered g-C3N4 precursor IV was dispersed in a mixture of 5 ml glycerol and 25 ml ethanol. After sonication for 30 min, the solution was reacted in an oil bath at 90 °C for 3 h. An appropriate amount of anhydrous ethanol was added to the resulting solution, and after centrifugation and washing, the solution was dried in a vacuum drying oven at 80 °C for 12 h. The product was calcined in a muffle furnace at 400 °C for 3 h to obtain g-C3N4 nanosheets IV (denoted as CNⅣ).
[0089] 0.8 g CNⅣ and 1.8 g ZrO2Ⅳ were added to 60 mL of anhydrous ethanol and sonicated for 30 min to disperse them evenly. Then, the mixture was reacted at 60 ℃ for 3 h under oil bath heating conditions. After the reaction was completed, the mixture was allowed to stand, the supernatant was poured off, the bottom product was separated, the product was washed with deionized water, and then dried in a vacuum drying oven at 60 ℃ for 8 h to obtain composite graphite carbon nitride gas-sensitive material Ⅳ.
[0090] Example 5
[0091] Five milligrams of the composite graphite carbon nitride gas-sensitive material I prepared in Example 1 were ultrasonically dispersed in 1.0 mL of anhydrous ethanol to form a uniform suspension. 0.05 mL of this suspension was drop-coated onto the surface of a pre-cleaned gold interdigitated electrode and dried at 80 °C for 6 h to obtain gas-sensitive element I.
[0092] The prepared gas-sensitive element I was subjected to gas-sensitive detection using a static gas mixing method. The specific steps were as follows: First, the gas-sensitive element I was installed in the gas chamber and connected to the information acquisition and analysis equipment. At a detection temperature of 25 ℃ and a detection humidity of 25% (relative humidity), 100 ppm of NO2 was injected. When the gas-sensitive response stabilized according to the feedback from the data acquisition system, the gas was pumped out to desorb the NO2, returning the device to its initial state, thus completing one gas injection cycle. Then, NO2 gas injection cycles were performed sequentially at 50 ppm, 30 ppm, 10 ppm, 5 ppm, 3 ppm, 1 ppm, 0.5 ppm, 0.3 ppm, 0.1 ppm, 0.05 ppm, 0.03 ppm, and 0.01 ppm. After completing the gas injection cycle, the sensitivity curve for detecting nitrogen dioxide at room temperature was obtained. Sensitivity S=R g / R a R a R is the resistance of the sensor in air. gThe resistance of the sensor is given by the NO2 atmosphere. The time required for the resistance to change by 90% during gas adsorption and desorption is the response time.
[0093] Table 1 shows the sensitivity and response time of the gas-sensitive element I under different nitrogen dioxide concentrations. The sensitivity to NO2 at a concentration of 100 ppm is 62.1, and the sensitivity to NO2 at a concentration as low as 0.01 ppm (10 ppb) is 1.3. The material has a fast response speed and good adsorption reversibility.
[0094] Table 1
[0095] <![CDATA[NO2 concentration]]> Sensitivity Response time 100 ppm 62.1 3.1 s 50 ppm 55.6 4.8 s 30 ppm 48.3 7.5 s 10 ppm 40.5 11.8 s 5 ppm 32.7 15.5 s 3 ppm 20.3 21.6 s 1 ppm 15.8 30.8 s 0.5 ppm 13.2 36.7 s 0.3 ppm 10.5 41.2 s 0.1 ppm 8.1 45.9 s 0.05 ppm 4.2 49.8 s 0.03 ppm 2.1 53.6 s 0.01 ppm 1.5 57.8
[0096] Example 6
[0097] The gas-sensitive element I prepared in Example 5 was subjected to gas-sensitive detection using a static gas mixing method. The specific steps were as follows: First, the gas-sensitive element I was installed in the gas chamber and connected to the information acquisition and analysis equipment. At a detection temperature of 30 °C and a detection humidity of 40% (relative humidity), 100 ppm of NO2 was injected. When the gas-sensitive response stabilized according to the feedback from the data acquisition system, the gas was pumped out to desorb the NO2, and the device returned to its initial state, thus completing one gas injection cycle. Then, NO2 was injected sequentially at concentrations of 50 ppm, 30 ppm, 10 ppm, 5 ppm, 3 ppm, 1 ppm, 0.5 ppm, 0.3 ppm, 0.1 ppm, and 0.03 ppm. After the gas injection was completed, the sensitivity curve for detecting nitrogen dioxide by the gas-sensitive element was obtained. Its sensitivity to NO2 concentration of 100 ppm was 20.78, and its sensitivity to NO2 concentration as low as 0.03 ppm was 0.8.
[0098] Comparative Example
[0099] The gas-sensitive element I prepared according to this invention was tested at a detection temperature of 25 °C and a detection humidity of 25% (relative humidity) to detect 100 ppm NO2. Figure 10 This work compares the response properties of this material with those of previously published NO2 detection gas-sensitive materials, specifically as follows: Figure 10 As shown. Figure 10 The preparation methods and experimental results of other gas-sensitive materials are as follows:
[0100] The preparation method and experimental results of ZrO2 / ZnO are from the literature J. Yang, H. Peng, C. Lin, Q. Pan, L. Qi, L. Li, K. Shi, UiO-66 metal–organic framework-derived ZrO2 / ZnOmesoporous materials for high-efficiency detection of NO2 at room temperature, Journal of Materials Chemistry A 11(42) (2023) 22859-22867.
[0101] The preparation method and experimental results of UiO-66@BiOI are from the literature H. Chang, J. Fan, R. Chen, H. Qiu, S. Liu, L. Wang, M. Ikram, C. Wang, X. Chen, UiO-66@BiOI core-shell structures with high concentration of defective oxygen for NO2 gas sensing atroom temperature, Journal of Alloys and Compounds 1010 (2025).
[0102] The preparation method and experimental results of rGO / ZrO2 are from the literature A. FRAIH, N. NAEEMA, F. ABBAS, High-performance NO2 gas sensor based on reduced graphene oxide / ZrO2 hybrids, Journal of Metals, Materials and Minerals, 34 3 (2024) 2038.
[0103] The preparation method and experimental results of BiC-2 are from the literature L. Jiang, J. Gao, J. Fan, F. Qin, H.Lv, M. Khan, J. Wang, Y. Fan, H. Wu, K. Shi, Spirally growing on porous C3N4thin layer with BiOCl nanosheets to enhance NO2 gas sensitivity at room temperature, Journal of Alloys and Compounds 938 938 (2023) 168644.
[0104] The preparation method and experimental results of ZnO / Ag / g-C3N4 are from the literature H. Li, Y. Sun, Q. Zhang, H. Yuan, C. Dong, S. Xu, M. Xu, Facile synthesis of ZnO / Ag / g-C3N4 nanocomposites for multiple applications in photocatalytic degradation and photoactivated NO2 sensing, Applied Surface Science 638 (2023) 15801.
[0105] The preparation method and experimental results of g-C3N4 / NiO are from the literature M. Ullah, H. Lv, Z. Liu, X. Bai, J. Chen, Y. Zhang, J. Wang, B. Sun, L. Li, K. Shi, Rational fabrication of ag-C3N4 / NiO hierarchical nanocomposite with a large surface area for the effective detection of NO2 gas at room temperature, Applied Surface Science 550 (2021) 149368.
[0106] The preparation method and experimental results of Pd-ZIF-67 / g-C3N4 are from the literature (H. Wu, M. Ullah, L. Jiang, J. Wang, B. Sun, J. Gao, H. Lv, Z. Liu, K. Shi, Controllable synthesis of porous 3D Pd loaded ZIF-67 / g-C3N4 hierarchical nanostructure for efficient detection of NO2 gas at room temperature, Colloids and Surfaces A: Physicochemical and Engineering Aspects 666 (2023) 131363).
[0107] The preparation method and experimental results of YSZ-3Y are from the literature R. You, G. Jing, H. Yu, T. Cui, Flexible Mixed-Potential-Type (MPT) NO2 Sensor Based on An Ultra-Thin Ceramic Film, Sensors 17 8 (2017) 174.)
[0108] The preparation method and experimental results of ZrO2@Co3O4 are from the literature JH Fan, XP Wang, SSCong, R. Zhang, WX Lv, L. Li, QJ Pan, X. Bai, KY Shi. Interface-engineered ZrO2@Co3O4 core-shell materials from bimetallic MOFs for enhanced room temperature NO2 sensing, Chemical Engineering Journal 543 (2026) 178268.
[0109] Experimental Example
[0110] Experimental Example 1
[0111] The composite graphite carbon nitride gas-sensitive material I prepared in Example 1 ( Figure 1 X-ray diffraction tests were performed on ZC-2 (Zhong ZC-2), specifically as follows: Figure 1 As shown.
[0112] from Figure 1 As can be seen, the diffraction peak corresponding to the (111) crystal plane of pure ZrO2 appears at 2θ = 32.210, while the peak position of the composite graphitic carbon nitride gas-sensitive material I shifts to a lower angle (30.181–30.048), indicating that the introduction of g-C3N4 may lead to lattice expansion. Furthermore, the characteristic (002) crystal plane diffraction peak of g-C3N4 appears at 2θ = 27.631, while the diffraction peak of the composite graphitic carbon nitride gas-sensitive material I shifts slightly to a higher angle (27.780–27.815), indicating an interfacial interaction between ZrO2 and g-C3N4. These systematic changes in peak positions and interlayer spacing confirm the successful construction of the heterostructure in the composite graphitic carbon nitride gas-sensitive material I.
[0113] Experiment Example 2
[0114] The composite graphite carbon nitride gas-sensitive material I prepared in Example 1 was imaged using a scanning electron microscope (SEM). The SEM image is shown below. Figure 2 As shown.
[0115] from Figure 2 The layered stacked structure and regular block shape can be clearly seen, with the two materials stacked on top of each other.
[0116] Experimental Example 3
[0117] Transmission electron microscopy (TEM) was performed on the composite graphite carbon nitride gas-sensitive material I prepared in Example 1. The TEM image is shown below. Figure 3 As shown, high-resolution TEM Figure 4 As shown.
[0118] from Figure 3 It can be clearly seen that nano-ZrO2 is dispersed on the surface of g-C3N4 nanosheets. There is a clear and well-defined heterojunction interface between ZrO2 and g-C3N4. Figure 4 The lattice stripes of the two materials can be seen. The lattice stripes of 2.96 nm and 2.62 nm correspond to the (111) and (002) crystal planes of ZrO2, respectively. ZrO2 and g-C3N4 are tightly bonded to form a contact surface, which is the heterojunction interface.
[0119] Experiment Example 4
[0120] The NO2 adsorption and desorption tests were performed on the composite graphite carbon nitride gas-sensitive material I prepared in Example 1. The NO2 adsorption and desorption results are shown in the attached figures. Figure 5 As shown.
[0121] The adsorption and desorption curves of composite graphitic carbon nitride gas-sensitive material I exhibit typical type IV isotherm characteristics, accompanied by an H3 type adsorption hysteresis loop, indicating that its pore size distribution is concentrated in the mesoporous range (2-50 nm), providing a structural basis for the effective diffusion of gas molecules. The specific surface area is 54.3 m² / g. This demonstrates that composite graphitic carbon nitride gas-sensitive material I possesses abundant mesoporous structure and a large specific surface area, providing more active adsorption sites for gases. This not only facilitates the rapid adsorption and desorption of target gases such as NO2 but also accelerates the diffusion rate of gas molecules within the material, thereby significantly improving gas sensing performance.
[0122] Experimental Example 5
[0123] Mott-Schottky (MS) analysis was performed on UiO-66, g-C3N4, and ZrO2 obtained in Example 1 using a three-electrode system in 0.1 M KOH solution. The working electrode was the prepared sample-coated glassy carbon electrode (GCE), the counter electrode was a platinum (Pt) plate electrode, and the reference electrode was a saturated calomel electrode. Electrochemical impedance spectroscopy (EIS) measurements were performed in laboratory air and nitrogen dioxide environments, respectively. A low voltage amplitude of 0.2 V was used during the experiments, and the frequency range was set from 1 to 10. 6 Hz. The experiment employed a four-electrode system including a working electrode, counter electrode, reference electrode, and auxiliary electrode, and measurements were conducted under low bias and high current conditions. The electrical properties of each sample were evaluated using a gold-inserted electrode substrate covered with a thin-film coating. Carrier density was calculated using the classical Mott-Schottky equation: N d = (2 / eεε0) (d(1 / C 2 ) / dv) -1 Where e is the elementary charge, ε0 is the permittivity of air, ε is the relative permittivity, and N is the relative permittivity. d Where C represents the doping concentration, C represents the capacitance, and v represents the voltage. The results show that ZC-2 exhibits the smallest slope in its Mott-Schottky curve, corresponding to a carrier density as high as 2.15 × 10⁻⁶. 18 ·cm -3 The values are higher than those of UiO-66 (3.48×10). 14 cm -3 ), g-C3N4 (7.69×10 16 cm -3 ZrO2 (2.58×10) 15 ·cm -3 ), specifically as Figure 6As shown, the carrier concentration of the composite graphitic carbon nitride gas-sensitive material is significantly increased, which is attributed to its unique composite structure that effectively promotes charge separation and migration. The high carrier density enables the composite graphitic carbon nitride gas-sensitive material to achieve more efficient electron transfer during NO2 adsorption, thereby enhancing the gas sensing response signal and providing a theoretical basis for its excellent NO2 sensing performance.
[0124] Experimental Example 6
[0125] Under conditions of 25°C and 25% relative humidity, the resistance of the gas-sensitive element I prepared in Example 1 was observed to change at NO2 concentrations of 100 ppm, 50 ppm, 30 ppm, 10 ppm, 5 ppm, 3 ppm, 1 ppm, 0.5 ppm, 0.3 ppm, 0.1 ppm, 0.05 ppm, 0.03 ppm, and 0.01 ppm. The specific changes are as follows: Figure 7 As shown. During the test, 100 ppm of NO2 was initially injected. When the gas-sensitive response stabilized according to the feedback from the data acquisition system, the gas was pumped out to desorb the NO2, and the device under test returned to its initial state, thus completing the 100 ppm test. Then, NO2 was injected sequentially at concentrations of 50 ppm, 30 ppm, 10 ppm, 5 ppm, 3 ppm, 1 ppm, 0.5 ppm, 0.3 ppm, 0.1 ppm, 0.05 ppm, 0.03 ppm, and 0.01 ppm.
[0126] Gas-sensitive element I exhibits excellent linearity in its response-recovery curves within the concentration range of 0.01–100 ppm, with a sensitivity of 62.1, a response time of 3.1 seconds, and a recovery time of 13.2 seconds. This superior gas sensing performance is primarily attributed to the synergistic effect of the material system. The composite graphitic carbon nitride gas-sensitive material I not only possesses a high specific surface area and abundant pore structure to enhance adsorption capacity, but the introduction of g-C3N4 significantly improves overall conductivity and accelerates charge transfer.
[0127] Experimental Example 7
[0128] The sensitivity change of the gas-sensitive element I prepared in Example 1 at a NO2 concentration of 100 ppm was observed at 25°C and relative humidity of 25%, 45%, 60%, and 80%, as detailed below. Figure 8 As shown.
[0129] from Figure 8It can be seen that the sensitivity of gas-sensitive element I decreases with increasing ambient humidity. This is mainly because there is a competitive adsorption effect between water molecules and NO2 at the active sites on the material surface. Water molecules occupy the active sites, hindering the effective adsorption of NO2, thus reducing the gas sensing response performance. It is noteworthy that the composite graphite carbon nitride gas-sensitive material I of this invention maintains excellent response performance even under humidity interference conditions.
[0130] Experimental Example 8
[0131] At 25°C and 25% relative humidity, the sensitivity change of the gas-sensitive element I prepared in Example 5 at a NO2 concentration of 100 ppm over 1-12 weeks (1 week is 7 days) is shown in the following figures. Figure 8 As shown.
[0132] Gas-sensitive element I exhibited excellent long-term stability during the 12-week testing period. The response value showed no decay or drift, indicating that its material structure, interfacial properties, and electrical response behavior underwent almost no degradation under environmental conditions. Compared with previously reported similar materials, the stability of composite graphite carbon nitride gas-sensitive material I is at a leading level.
[0133] The present invention has been described in detail above with reference to specific embodiments and / or exemplary examples, as well as the accompanying drawings. However, these descriptions should not be construed as limiting the present invention. Those skilled in the art will understand that various equivalent substitutions, modifications, or improvements can be made to the technical solutions and embodiments of the present invention without departing from the spirit and scope of the invention, and all such modifications and improvements fall within the scope of the present invention. The scope of protection of the present invention is defined by the appended claims.
Claims
1. A composite graphitic carbon nitride gas-sensitive material, prepared by heating a reaction of raw materials including ZrO2 and graphitic carbon nitride in solvent B. The ZrO2 was obtained by calcining UiO-66 metal-organic framework material.
2. A method for preparing the composite graphite carbon nitride gas-sensitive material according to claim 1, characterized in that, The method describes the preparation of the product by heating a reaction of raw materials comprising ZrO2 and graphitic carbon nitride in solvent B. Preferably, the method specifically includes the following steps: Step 1: Obtain ZrO2; Step 2: Obtain graphite carbon nitride; Step 3: Add ZrO2 and graphite carbon nitride to solvent B, heat to react, and after the reaction is complete, separate the product, wash and dry it to obtain composite graphite carbon nitride gas-sensitive material.
3. The preparation method of the composite graphite carbon nitride gas-sensitive material according to claim 2, characterized in that, In step 1, The ZrO2 was obtained by calcining UiO-66 metal-organic framework material at a temperature of 300-600℃ for 2-5 hours.
4. The preparation method of the composite graphite carbon nitride gas-sensitive material according to claim 3, characterized in that, In step 1, the UiO-66 metal-organic framework material is obtained by adding terephthalic acid solution to zirconium salt solution, reacting the solution in a sealed reactor under heating, and then undergoing post-processing. The solvent for the terephthalic acid solution is one or more of alcohols and amides, preferably one or more of ethanol, ethylene glycol, N,N-dimethylformamide, and N,N-dimethylacetamide. The solvent for the zirconium salt solution is one or more of alcohols and amides, preferably one or more of N,N-dimethylformamide and / or N,N-dimethylacetamide. The zirconium salt is selected from one or more of zirconium chloride, zirconium bromide, zirconium sulfate, zirconium nitrate, and zirconium oxychloride octahydrate. Preferably, the zirconium salt solution contains a carboxylic acid regulator B, selected from one or more monocarboxylic acids and dicarboxylic acids, and preferably one or two of formic acid, acetic acid and benzoic acid.
5. The method for preparing the composite graphite carbon nitride gas-sensitive material according to claim 2, characterized in that, In step 2, the graphite carbon nitride is obtained by solvothermal reaction of raw materials including melamine and phosphoric acid to obtain a graphite carbon nitride precursor, which is then heated under solvent conditions to obtain the product after calcination.
6. The method for preparing the composite graphite carbon nitride gas-sensitive material according to claim 5, characterized in that, In step 2, melamine and phosphoric acid are added to water and stirred at 65-95°C for 0.5-3 hours. The mass ratio of melamine to phosphoric acid is 1:(1-2.4), preferably 1:(1-2.0), and more preferably 1:(1-1.6). The mixture is then transferred to a high-pressure reactor for a solvothermal reaction at a temperature of 165-195°C, preferably 170-190°C, more preferably 175-185°C, for a reaction time of 7-15 hours, preferably 8-13 hours, more preferably 9-11 hours.
7. The method for preparing the composite graphite carbon nitride gas-sensitive material according to claim 6, characterized in that, In step 2, the graphite carbon nitride precursor is uniformly dispersed in solvent A, heated to react, then centrifuged and dried. Solvent A is one or more alcohol solvents, preferably one or more of liquid monohydric alcohols, liquid dihydric alcohols, and liquid trihydric alcohols, and more preferably a mixed solvent of glycerol and ethanol. The heating reaction temperature is 75-105℃, and the reaction time is 1-4 hours. The calcination temperature is 300-600℃, preferably 350-550℃, and more preferably 400-500℃; the calcination time is 1-5h, preferably 1.5-4h, and more preferably 2-3h.
8. The method for preparing the composite graphite carbon nitride gas-sensitive material according to claim 2, characterized in that, In step 3, The mass ratio of graphitic carbon nitride to ZrO2 is 1:(1.1-3.1), preferably 1:(1.2-2.8), and more preferably 1:(1.3-2.5). Solvent B is selected from one or more alcohol solvents, preferably one or more of methanol, ethanol, propanol, and butanol. The heating reaction temperature is 50-90℃, preferably 55-85℃, more preferably 60-80℃, and the time is 0.5-4h, preferably 0.8-3.5h, more preferably 1-3h.
9. The use of the composite graphite carbon nitride gas-sensitive material according to claim 1, characterized in that, To prepare a gas-sensitive element for detecting nitrogen dioxide, a suspension of composite graphite carbon nitride gas-sensitive material is coated onto an Au interdigitated electrode, and after drying, a gas-sensitive element for detecting nitrogen dioxide is obtained.
10. A gas-sensitive element for detecting nitrogen dioxide, characterized in that, It is obtained by coating a suspension of the composite graphite carbon nitride gas-sensitive material as described in claim 1 onto an Au interdigitated electrode, followed by drying. The gas-sensitive element used for detecting nitrogen dioxide has a detection limit of 0.01 ppm. At a concentration of 0.01 ppm, the response time is within 60 seconds.