Method for preparing ca-mg-fe-p04 type slow-release phosphorus intermediates based on phosphogypsum leachate

The Ca-Mg-Fe-PO4 type LDH was prepared by electrodialysis and in-situ oxidation of iron powder. Combined with polymer encapsulation, the problems of low resource utilization rate of phosphogypsum leachate and high LDH preparation cost were solved. This resulted in a high-purity, structurally stable slow-release phosphorus intermediate suitable for loading and slow-release of agricultural functional substances.

CN123062006APending Publication Date: 2026-11-10CHINA MINMETALS CHANGSHA MINING RES INST +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611069317.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-17
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In existing technologies, the resource utilization rate of phosphogypsum leachate is low, the traditional LDH preparation cost is high, it is easily affected by impurities, and it is difficult to balance the loading of agricultural functional substances and the slow-release function of phosphorus.

Method used

Anions and cations were separated by electrodialysis, and then combined with in-situ oxidation of iron powder and pH control to prepare Ca-Mg-Fe-PO4 type LDH. The core-shell structure was formed by polymer encapsulation to achieve loading and slow release of agricultural functional substances.

Benefits of technology

This approach achieves the harmlessness and resource utilization of phosphogypsum leachate, reduces the cost of LDH preparation, improves product purity and structural stability, and extends the phosphorus release cycle, meeting the needs of green chemical industry and sustainable agricultural development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123062006A_ABST
    Figure CN123062006A_ABST
Patent Text Reader

Abstract

This application provides a method for preparing a Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate based on phosphogypsum leachate, belonging to the technical field of phosphorus chemical wastewater resource utilization and layered double hydroxide preparation. The method includes: pre-treating the phosphogypsum leachate by electrodialysis to obtain a cation concentrate; conditioning the cation concentrate and removing heavy metals to obtain pure Ca... 2+ -Mg 2+ Mixed raw material liquid; add waste iron powder for in-situ oxidation to form Fe 3+ -Ca 2+ -Mg 2+ A multi-metal ion system was developed; phosphate and a precipitant were added, and after reaction and aging, a Ca-Mg-Fe-PO4 type LDH precipitate was obtained; finally, the LDH was dispersed into a slurry, loaded with agricultural functional substances, and polymer-encapsulated to obtain a Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate. This application realizes the harmlessness and resource utilization of phosphogypsum leachate, turning waste into treasure, significantly reducing the cost of LDH preparation, and the obtained intermediate has the dual function of slow-release phosphorus and controlled release of multiple agricultural functional substances, thus broadening its application scenarios.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of resource utilization of phosphorus chemical wastewater and preparation of layered double hydroxides, specifically to a method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediates based on phosphogypsum leachate. Background Technology

[0002] Phosphogypsum is a large-scale industrial solid waste generated during the wet-process phosphoric acid production. The leachate produced during its storage is a typical highly acidic, high-salinity industrial wastewater, with a pH value typically between 2.2 and 2.4. This wastewater is rich in calcium. 2+ Mg 2+ PO4 3- SO4 2- F - Plasma, containing trace amounts of Fe 3+ / Fe 2+ And heavy metal pollutants such as arsenic, copper, and zinc.

[0003] Currently, the treatment of phosphogypsum leachate mainly adopts traditional methods such as neutralization precipitation and dilution discharge. These methods not only fail to realize the resource utilization of valent ions in the wastewater, but also cause ecological and environmental problems such as soil compaction, water eutrophication and heavy metal pollution due to incomplete treatment, resulting in resource waste.

[0004] Layered hydrogen hydroxides (LDHs) have broad application prospects in agricultural slow-release fertilizers and functional substance carriers due to their unique layered structure, ion exchange properties, and slow-release performance. However, traditional processes for preparing Ca-Mg-Fe-PO4 type LDHs mostly rely on pure chemical reagents, which are costly and not combined with industrial wastewater treatment, thus failing to conform to the concept of green recycling.

[0005] In existing technologies, electrodialysis for wastewater desalination is not specifically combined with LDH preparation; iron powder reduction oxidation technology provides an iron source, but there is no mature process for how to synergistically synthesize multifunctional LDH with calcium and magnesium ions in wastewater and achieve agricultural functional material loading. Furthermore, the high concentration of SO4 in the wastewater... 2- It can competitively embed into the LDH interlayer, affecting product purity and structural stability, while heavy metal ions threaten its biosafety. Existing technologies lack effective raw material purification solutions.

[0006] Therefore, there is an urgent need to develop a process that can synergistically achieve the harmless treatment and high-value utilization of phosphogypsum leachate, in order to prepare high-purity, high-performance Ca-Mg-Fe-PO4 type LDH slow-release phosphorus intermediates at low cost. Summary of the Invention

[0007] In view of the technical problems existing in the background art, this application provides a method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate based on phosphogypsum leachate, aiming to solve the technical problems of low resource utilization rate of phosphogypsum leachate, easy pollution, high cost of traditional LDH preparation, easy interference from impurities, and difficulty in taking into account the agricultural functional material loading and phosphorus slow-release function.

[0008] This application provides a method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediates based on phosphogypsum leachate, comprising the following steps: S1, the phosphogypsum leachate is pumped into an electrodialysis device for electrodialysis ion enrichment treatment to obtain cation concentrate, anion concentrate and desalination desalination solution. S2, the cation concentrate is conditioned, and then sodium sulfide or calcium hydroxide is added to adjust the pH of the system to 4.0-5.0, so that Fe... 3+ As 3+ Cu 2+ and Zn 2+ The formation of insoluble hydroxide or sulfide precipitates is observed; after filtration, pure Ca is obtained. 2+ -Mg 2+ Mixed raw material liquid; S3, adjust the Ca 2+ -Mg 2+ The pH of the mixed raw material solution is adjusted to 3.0-4.0, followed by the addition of scrap iron powder. After the scrap iron powder corrodes and dissolves, it undergoes an in-situ oxidation reaction to form Fe. 3+ -Ca 2+ -Mg 2+ Multi-metal ion system; S4, to the Fe 3+ -Ca 2+ -Mg 2+ A Ca-Mg-Fe-PO4 type LDH precipitate was obtained by adding soluble phosphate and precipitant to a multi-metal ion system and then reacting with stirring and aging. S5, the Ca-Mg-Fe-PO4 type LDH precipitate is subjected to solid-liquid separation to obtain filter cake; the filter cake is dispersed into LDH slurry, and agricultural functional substances are loaded using an appropriate loading method, followed by the addition of polymer for encapsulation treatment to obtain Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate.

[0009] Furthermore, when the agricultural functional substance is an anionic agricultural functional substance, it is intercalated and loaded at 40-50℃ for 60-120 min using an ion exchange method; the mass ratio of the anionic agricultural functional substance to LDH is 1:(3-5). When agricultural functional substances are non-ionic or weakly polar, surface adsorption is used for loading.

[0010] Furthermore, the electrodialysis device consists of alternating cation exchange membranes and anion exchange membranes forming a membrane stack structure; in step S1, under the action of a DC electric field, cations migrate through the cation exchange membrane to the cation concentration chamber, and anions migrate through the anion exchange membrane to the anion concentration chamber, forming a desalination solution in the intermediate chamber.

[0011] Furthermore, during the electrodialysis ion enrichment treatment, the electrodialysis operating voltage is 15-30V, and the current density is 20-50mA / cm³. 2 The operation will stop when the conductivity of the desalination solution drops to 1.0-1.5 mS / cm.

[0012] Furthermore, the conditioning treatment refers to low-temperature concentration; after the conditioning treatment, the Ca in the cation concentrate... 2+ Concentration of 10-20 g / L, Mg 2+ The concentration is 5-10 g / L.

[0013] Furthermore, the waste iron powder is cast iron shavings or low-carbon steel shavings, with an Fe content >90% and a particle size of 100-200 mesh; the dosage of the waste iron powder is based on the ratio of Fe to Ca. 2+ and Mg 2+ The ratio of the sum of the molar amounts is 1:(1-2) control.

[0014] Furthermore, the conditions for the in-situ oxidation reaction are: stirring at room temperature for 30-60 min, a gas-liquid ratio of 5:1, an aeration rate of 1.0-1.5 L air / (L solution·min), and the reaction proceeds until the system pH reaches 5.5-6.5 and Fe... 2+ Stop when the concentration is <0.1g / L.

[0015] Further, in step S4, the precipitant is a 1.0-2.0 mol / L NaOH solution, and the dropping rate of the precipitant is 1-2 mL / (L·min); the pH of the system is controlled at 10.5-11.0 during the reaction, and after stirring for 90-120 min, the mixture is aged at 75±5℃ with low stirring at 50-100 rpm for 20-24 h; the PO4 in the soluble phosphate... 3- The molar ratio of the total metal ions in the multi-metal ion system is 1:(2-2.2).

[0016] Further, in step S5, the polymer is pectin, chitosan, or polyacrylate.

[0017] Furthermore, the encapsulation process refers to stirring and reacting at 50-60°C for 30-60 minutes to form a continuous coating layer on the surface of LDH particles, which is then cross-linked and cured to form core-shell type sustained-release particles of LDH-functional component-polymer.

[0018] The beneficial effects of this application are as follows: This application proposes a method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediates based on phosphogypsum leachate. Using phosphogypsum leachate as raw material, this application achieves efficient separation and targeted enrichment of anions and cations through electrodialysis. 2 + Mg 2+ Recovery rate >85%, SO4 2- The transfer rate is >90%, which removes F from the leachate. - It eliminates harmful pollutants such as heavy metals, and uses valuable ions such as calcium and magnesium in wastewater as the core raw materials for LDH synthesis, replacing traditional pure chemical reagents, which greatly reduces the cost of LDH preparation. At the same time, it solves the ecological pollution problem caused by the random discharge of phosphogypsum leachate, realizing "wastewater treatment and waste-to-treasure", and achieving the dual goals of harmlessness and resource utilization of phosphogypsum leachate.

[0019] This application avoids high-concentration SO4 at the source by using electrodialysis for zoned enrichment and low-temperature concentration and conditioning. 2- Competitive intercalation into the LDH interlayer structure; selective precipitation and removal of impurity ions such as Fe, As, Cu, and Zn through precise pH control, while ensuring Ca... 2+ With Mg 2+ While remaining in solution, this process improves the purity and structural stability of subsequent LDH synthesis raw materials; it avoids the impact of heavy metals on the structural stability and biosafety of LDH; and the in-situ oxidation process of iron powder achieves Fe... 3+ A stable supply, combined with precise pH and molar ratio control, enables Ca... 2+ Mg 2+ Fe 2+ With PO4 3- OH - After thorough assembly and Oswald ripening, the crystallinity and structural order of the product are significantly improved, and the prepared Ca-Mg-Fe-PO4 type LDH has high purity and good structural stability.

[0020] This application constructs an integrated process flow of "separation-synthesis-functionalization", organically combining electrodialysis separation, in-situ oxidation of iron powder, LDH-directed synthesis, and agricultural functional material loading and encapsulation. The prepared LDH multi-purpose agricultural slow-release phosphorus intermediate not only possesses interlayer PO4 3- The targeted sustained-release function of the constructed "LDH core-polymer shell" core-shell structure can effectively inhibit the rapid release of functional components in a neutral environment, while in an acidic environment or under conditions containing complexed organic molecules, the polymer shell gradually degrades and promotes the slow dissociation of the LDH interlayer structure, thereby achieving continuous sustained release of functional components and environmentally responsive release.

[0021] The scrap iron powder used in this application is a byproduct of mechanical processing, which is widely available and inexpensive. The electrodialysis operating parameters can be flexibly adjusted according to actual working conditions. Subsequent synthesis and loading steps are conventional chemical operations, requiring no special or expensive equipment. The reaction conditions in each step of the process are mild, and the reaction endpoint determination indicators are clear, making it easy to achieve continuous industrial production and meeting the needs of green chemical industry and sustainable agricultural development. The process of this application is low in cost, simple to operate, and easy to promote industrially.

[0022] This application utilizes all components of phosphogypsum leachate in a graded manner. The cationic concentrate is used for LDH synthesis, and the anionic concentrate can be further utilized by referring to bipolar membrane electrodialysis technology. The desalination solution can be reused in the production process, realizing the recycling of water resources and achieving high resource utilization. No harmful waste is generated throughout the process, and heavy metals are fixed and removed in the form of precipitation, which will not cause secondary pollution and has significant environmental friendliness.

[0023] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description

[0024] To more clearly illustrate the technical solutions of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.

[0025] Figure 1 This is a schematic diagram of the electrodialysis apparatus used for treating phosphogypsum leachate in this application.

[0026] Figure 2 This is a schematic diagram of the microstructure of the Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate obtained in this application.

[0027] Figure 3 The cumulative phosphorus release curves are shown for the Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate samples prepared in Example 1 and Comparative Example 1. Detailed Implementation

[0028] The embodiments of the technical solution of this application will now be described in detail with reference to the accompanying drawings. These embodiments are only used to more clearly illustrate the technical solution of this application and are therefore merely examples, and should not be used to limit the scope of protection of this application.

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the drawings are intended to cover non-exclusive inclusion.

[0030] This application provides a method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediates based on phosphogypsum leachate, comprising the following steps: 1. Electrodialysis zone enrichment treatment: The phosphogypsum leachate is pumped into an electrodialysis unit for zoned enrichment treatment; the electrodialysis unit has a membrane stack of 40-60 pairs of membranes, and the anion exchange membranes are selected with a sheet resistivity of less than 15 Ω·cm. 2 Heterogeneous anion exchange membranes and cation exchange membranes with a sheet resistivity of less than 12 Ω·cm 2 Furthermore, it is a heterogeneous cation exchange membrane with high selectivity for divalent cations.

[0031] During electrodialysis operation, the voltage is controlled at 15-30V and the current density is 20-50mA / cm². 2 The process continues until the conductivity of the desalination solution drops to 1.0-1.5 mS / cm and the Ca concentration in the cation concentrate decreases. 2+ The concentration is 15-25 g / L, and Mg 2+ Stop when the concentration reaches 8-12 g / L, and obtain cation concentrate, anion concentrate and desalination solution.

[0032] Among them, the cation concentrate is used as the core raw material for subsequent LDH synthesis, while the anion concentrate is treated separately to meet the standards before being discharged or utilized as a resource.

[0033] 2. Conditioning and heavy metal removal of cation concentrate: The cation concentrate was subjected to low-temperature concentration and conditioning treatment to improve the Ca content. 2+ Adjust the concentration to 10-20 g / L, Mg 2+ Adjust the concentration to 5-10 g / L; then add sodium sulfide or calcium hydroxide to the system and adjust the pH of the system to 4.0-5.0.

[0034] Under these pH conditions, Fe 3+ As 3+ Cu 2+ and Zn 2+ Impurity ions preferentially form insoluble hydroxide or sulfide precipitates, while Ca... 2+ With Mg 2+ It remains in a dissolved state, thereby achieving selective precipitation and removal of impurity ions.

[0035] After stirring the reaction for 30-60 minutes, the precipitate was separated by plate and frame filtration to obtain Ca. 2+ -Mg 2+ Mix the raw material liquid.

[0036] Due to Ca 2+ With Mg 2+ The corresponding hydroxide has high solubility at pH 4.0-5.0, therefore no significant precipitation occurs; it remains dissolved and retained in solution. It serves as a raw material for the subsequent synthesis of LDH.

[0037] 3. Preparation of a multi-metal ion system by in-situ oxidation of iron powder: Ca 2+ -Mg 2+ The pH of the mixed raw material liquid is adjusted to 3.0-4.0, and waste iron powder is added; wherein the waste iron powder is cast iron shavings or low carbon steel shavings, with an Fe content >90% and a particle size of 100-200 mesh.

[0038] The amount of scrap iron powder added is based on the ratio of Fe to Ca. 2+ and Mg 2+ The molar ratio of the sum of the molar amounts is 1:(1-2) controlled.

[0039] The in-situ oxidation reaction process is as follows: Stir the reaction at room temperature for 30-60 minutes, simultaneously introducing air at a gas-liquid ratio of 5:1, with an aeration rate of 1.0-1.5 L air / (L solution·min), until the system pH reaches 5.5-6.5, and Fe... 2+ Stop when concentration <0.1 g / L, forming Fe 3+ -Ca 2+ -Mg 2+ Multi-metal ion system.

[0040] 4. Phosphate regulation and directed synthesis of Ca-Mg-Fe-PO4 type LDH: To Fe 3+ -Ca 2+ -Mg 2+ Adding soluble phosphates to a multi-metal ion system controls PO4. 3- The molar ratio of the total metal ions in the multi-metal ion system is 1:(2-2.2).

[0041] At a stirring speed of 300-500 r / min, 1.0-2.0 mol / L NaOH solution was slowly added dropwise as a precipitant at a dropping rate of 1-2 mL / (L·min). The pH of the system was precisely adjusted to 10.5-11.0. After stirring for 90-120 min, the mixed slurry was aged at 75±5℃ with low stirring speed of 50-100 rpm for 20-24 h to obtain Ca-Mg-Fe-PO4 type LDH precipitate.

[0042] 5. Preparation of LDH multi-purpose agricultural slow-release phosphorus intermediate by loading agricultural functional substances and polymer encapsulation: The Ca-Mg-Fe-PO4 type LDH precipitate is subjected to solid-liquid separation to obtain a filter cake, which is then dispersed into a slurry with a mass concentration of 5-10%.

[0043] Select the appropriate loading method based on the type of agricultural functional material.

[0044] Specifically, for anionic agricultural functional substances, ion exchange loading is used, with the mass ratio of agricultural functional substances to LDH being 1:(3-5), and the reaction is carried out at 40-50℃ for 60 minutes with stirring. For nonionic agricultural functional substances, surface adsorption loading is used, with an appropriate amount of surfactant added simultaneously.

[0045] After loading is completed, pectin, chitosan or polyacrylate is added as polymer, and the mixture is stirred at 50-60℃ for 30 min for encapsulation to form core-shell type slow-release particles of LDH-functional substance-polymer, thus obtaining Ca-Mg-Fe-PO4 type LDH multipurpose agricultural slow-release phosphorus intermediate.

[0046] This application realizes the harmlessness and resource utilization of phosphogypsum leachate, turning waste into treasure, and significantly reduces the cost of LDH preparation. The resulting Ca-Mg-Fe-PO4 type LDH multipurpose agricultural slow-release phosphorus intermediate has the dual functions of phosphorus slow release and controlled release of various agricultural functional substances, and has a wider range of applications.

[0047] The Ca-Mg-Fe-PO4 type LDH multipurpose agricultural slow-release phosphorus intermediate prepared in this application can be loaded with various agricultural functional substances such as agricultural functional substances, fertilizers, plant growth regulators, and humic acid, and is suitable for various scenarios such as food crops, cash crops, facility agriculture, and soil improvement.

[0048] The following are some specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.

[0049] The phosphogypsum leachate used in this embodiment is a byproduct wastewater from wet-process phosphoric acid production, with a pH of 2.3, containing Ca... 2+ Concentration of 8.5 g / L, Mg 2+ The concentration was 3.2 g / L, SO4 2- The concentration was 25.6 g / L, F - The concentration is 1.8 g / L, containing trace amounts of As. 3+ Cu 2+ Zn 2+ and Fe 3+ / Fe 2+ The surface resistivity of the heterogeneous anion exchange membrane used is 12 Ω·cm. 2 The surface resistivity of the heterogeneous cation exchange membrane is 10 Ω·cm 2 The selectivity coefficient for divalent cations is >1.5; the waste iron powder is cast iron scrap with an Fe content of 92% and a particle size of 150 mesh; the soluble phosphate is disodium hydrogen phosphate, and the polymer is chitosan.

[0050] The prepared LDH core-shell type sustained-release particles have a low release rate under neutral conditions, while under weakly acidic conditions the polymer shell gradually degrades and the LDH interlayer structure slowly dissociates, exhibiting obvious environmentally responsive sustained-release characteristics; the release period of functional components can be adjusted to 80-120 days depending on the polymer type and coating thickness.

[0051] Example 1 Please see Figure 1 As shown, this embodiment provides a method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediates based on phosphogypsum leachate, including the following steps: S1, the phosphogypsum permeate is pumped into an electrodialysis device with 40 pairs of cation exchange membranes and anion exchange membranes arranged alternately to form a membrane stack structure for electrodialysis ion enrichment treatment; wherein, the sheet resistance of the anion exchange membrane is 12 Ω·cm. 2 The sheet resistance of the cation exchange membrane is 10 Ω·cm. 2 It also exhibits high selectivity for divalent cations.

[0052] Under the action of a DC electric field, Ca 2+ Mg 2+ Cations migrate through the cation exchange membrane to the cation concentration chamber, SO4 2- F - Anions migrate through the anion exchange membrane to the anion concentration chamber, where a desalination solution is formed in the intermediate chamber. Figure 1 As shown, the corresponding cation concentrate, anion concentrate, and desalination solution were obtained.

[0053] The electrodialysis operating voltage is controlled at 15V, and the current density is 20mA / cm². 2 The process continued until the conductivity of the desalination solution dropped to 1.0 mS / cm, and the Ca in the cation concentrate... 2+ Concentration of 15 g / L, Mg 2+ Stop when the concentration reaches 8 g / L.

[0054] Based on testing and calculation, the Ca²⁺ content in this step... + and Mg² + The overall recovery rate from the feed solution to the cation concentrate is 85%, meaning that the Ca²⁺ collected in the cation concentrate... + With Mg² + The total molar amount of Ca² in the feed solution + With Mg² + 85% of the total molar amount. SO4 2- The transfer rate from the feed solution to the anion concentrate is 90%, meaning that the SO4 collected in the anion concentrate... 2- The molar amount of SO4 in the feed liquid 2- 90% of the total molar amount.

[0055] S2, the obtained cation concentrate is subjected to low-temperature concentration and conditioning to remove Ca 2+ The concentration was adjusted to 10 g / L, Mg 2+ The concentration was adjusted to 5 g / L. Then, sodium sulfide was added, and the pH was controlled at 4.0 to allow Fe... 3+ As 3+ Cu 2+ and Zn 2+ Impurity ions form sulfide precipitates, while Ca... 2+ With Mg 2+ While still in a dissolved state, after stirring for 30 minutes, plate and frame filtration was used to remove the heavy metal precipitate, yielding pure Ca. 2+ -Mg 2+ Mix the raw material liquid.

[0056] S3, Ca 2+ -Mg 2+ Adjust the pH of the mixed raw material solution to 3.0, add cast iron scrap and waste iron powder, and add them in proportions of Fe and Ca. 2+ +Mg 2+ Molar ratio controlled at 1:1.

[0057] Stir at room temperature for 30 minutes, simultaneously introducing air at a gas-liquid ratio of 5:1 and an aeration rate of 1.0 L air / (L solution·min). Continue the reaction until the system pH reaches 5.5 and Fe... 2+ Stop when the concentration reaches 0.08 g / L, forming Fe. 3+ -Ca 2+ -Mg 2+Multi-metal ion system.

[0058] S4, towards Fe 3+ -Ca 2+ -Mg 2+ Adding disodium hydrogen phosphate to a multi-metal ion system controls PO4. 3- The molar ratio of the total metal ions in the multi-metal ion system is 1:2.

[0059] The stirring speed was 300 r / min, and 1.0 mol / L NaOH solution was added dropwise at a rate of 1 mL / (L·min) to adjust the pH of the system to 10.5. The reaction was stirred for 90 minutes. Subsequently, the mixed slurry was aged at 70℃ with low stirring speed of 50 rpm for 20 hours to obtain Ca-Mg-Fe-PO4 type LDH precipitate.

[0060] S5. The Ca-Mg-Fe-PO4 type LDH precipitate was subjected to solid-liquid separation to obtain a filter cake, which was then dispersed into a slurry with a mass concentration of 5%. An anionic agricultural functional substance (glyphosate) was selected and mixed with LDH at a mass ratio of 1:3. Ion exchange loading was carried out by stirring at 40℃ for 60 minutes. After loading, chitosan was added, and the mixture was encapsulated by stirring at 50℃ for 30 minutes to obtain a Ca-Mg-Fe-PO4 type LDH multi-purpose agricultural slow-release phosphorus intermediate. Its microstructure diagram is shown below. Figure 2 As shown, the intermediate exhibits a core-shell structure: the core is a Ca-Mg-Fe-PO4 type LDH sheet loaded with agricultural functional substances, and the outer shell is a polymer coating layer.

[0061] Under neutral or weakly alkaline conditions, the polymer shell structure is stable and can effectively inhibit the rapid release of functional components. When the system is in an acidic environment or in the presence of complexed organic molecules, the polymer shell gradually swells and degrades, and the external solution gradually penetrates into the LDH interlayer. At the same time, the LDH plates slowly dissociate, thereby achieving the continuous and slow release of functional components.

[0062] Comparative Example 1 Comparative Example 1 provides a Ca-Mg-Fe-PO4 type LDH control material slow-release phosphorus intermediate without polymer encapsulation. Its preparation method is basically the same as that of Example 1, except that chitosan is not added for encapsulation in step S5, as detailed below: S1, the phosphogypsum permeate is pumped into an electrodialysis device consisting of 40 pairs of alternating cation exchange membranes and anion exchange membranes to form a membrane stack structure for electrodialysis ion enrichment treatment; wherein, the surface resistivity of the anion exchange membrane is 12 Ω·cm. 2 The surface resistivity of the cation exchange membrane is 10 Ω·cm 2 It also exhibits high selectivity for divalent cations.

[0063] The electrodialysis operating voltage is controlled at 15V, and the current density is 20mA / cm². 2 The process was stopped when the conductivity of the desalination solution dropped to 1.0 mS / cm, yielding cation concentrate, anion concentrate, and desalination solution. Calculations showed that the Ca²⁺ content in this step... + and Mg² + The overall recovery rate was 85% for SO4. 2- The transfer rate was 90%. The meaning of recovery rate and transfer rate, and their significance for subsequent processes, are the same as in Example 1.

[0064] S2, the obtained cation concentrate is subjected to low-temperature concentration and conditioning treatment to remove Ca²⁺. + Adjust the concentration to 10 g / L, Mg² + The concentration was adjusted to 5 g / L. Sodium sulfide was then added and the pH of the system was adjusted to 4.0, so that Fe³⁺… + As³ + Cu² + and Zn² + Impurity ions form insoluble sulfide precipitates, while Ca²⁺… + With Mg² + It remained in a dissolved state. After stirring for 30 minutes, the precipitate was removed by plate and frame filtration to obtain Ca²⁺. + -Mg² + Mix the raw material liquid.

[0065] S3, Ca² + -Mg² + Adjust the pH of the mixed raw material solution to 3.0, add waste iron powder (cast iron filings) with a particle size of 150 mesh, and mix Fe and Ca². + Mg² + The total molar ratio is 1:1 when adding the product.

[0066] The mixture was stirred for 30 minutes at room temperature while simultaneously aerated, maintaining a gas-liquid ratio of 5:1 and an aeration rate of 1.0 L air / (L solution·min). The reaction continued until the system pH reached 5.5 and Fe²⁺ was reduced. + The reaction stops when the concentration is below 0.08 g / L, forming Fe³⁺. + -Ca 2+ -Mg 2+ Multi-metal ion system.

[0067] S4, towards Fe³ + -Ca 2+ -Mg 2+ Adding disodium hydrogen phosphate to a multi-metal ion system controls PO4. 3- The molar ratio of the total metal ions in the multi-metal ion system is 1:2.

[0068] Subsequently, 1.0 mol / L NaOH solution was added dropwise at a rate of 1 mL / (L·min) to adjust the pH of the system to 10.5. After stirring for 90 min, the resulting slurry was aged at 70 °C and 50 rpm for 20 h to obtain Ca-Mg-Fe-PO4 type LDH precipitate.

[0069] S5, the obtained Ca-Mg-Fe-PO4 type LDH precipitate was subjected to solid-liquid separation to obtain a filter cake, which was then prepared into a slurry with a mass concentration of 5%. Glyphosate was then added as an agricultural functional substance, and mixed at a mass ratio of agricultural functional substance to LDH of 1:3. The mixture was stirred at 40℃ for 60 min to complete ion exchange loading. After loading, the mixture was directly filtered, washed, and dried without chitosan encapsulation, ultimately obtaining a Ca-Mg-Fe-PO4 type LDH slow-release phosphorus intermediate without a polymer shell.

[0070] To evaluate the effect of polymer encapsulation structure on sustained-release performance, 5g of the sample prepared in Example 1 and 5g of the sample prepared in Comparative Example 1 were weighed and placed in 500mL of 0.01mol / L CaCl2 solution (pH=5.5). Release experiments were conducted in a 25℃ constant-temperature shaking incubator. Samples were taken on days 1, 7, 15, 30, 60, 90, and 120 to determine the concentration of orthophosphate (PO42-) in the solution. 3- -P) concentration, and replenished with an equal volume of fresh release medium. The ammonium molybdate spectrophotometric method was used to determine the orthophosphate phosphorus content. The organic phosphorus in glyphosate molecules did not show color under these detection conditions and did not affect the results. The cumulative phosphorus release rate was calculated based on the cumulative release of phosphorus in the release medium. The test results are shown in Table 1.

[0071] Table 1. Cumulative phosphorus release rates of samples prepared in Example 1 and Comparative Example 1 Plot the cumulative phosphorus release curve based on the data in Table 1, as follows: Figure 3 As shown.

[0072] From Table 1 and Figure 3 It can be seen that the cumulative phosphorus release rate of Comparative Example 1 reached 84.6% on day 30 and 94.8% on day 60, basically completing the phosphorus release process and showing a relatively rapid release characteristic.

[0073] The reason is that: Comparative Example 1 did not undergo polymer encapsulation treatment, and the LDH particles were directly exposed to the release medium. External moisture could quickly enter the LDH interlayer structure and react with the interlayer PO4. 3- An ion exchange reaction occurs, resulting in the rapid release of phosphorus.

[0074] In contrast, Example 1 showed a cumulative phosphorus release rate of only 31.7% on day 30, 52.3% on day 60, and 88.4% on day 120, maintaining a continuous release state and extending the phosphorus release cycle to more than 120 days.

[0075] The reason is that Example 1 constructed a dual sustained-release system of "polymer shell-LDH layered structure" by using chitosan to form a continuous polymer coating layer on the surface of LDH particles. During the release process, the polymer coating layer acts as a barrier to external moisture entering the LDH interlayer. External moisture must first penetrate the polymer coating layer and then gradually diffuse into the LDH interlayer structure. 3- The phosphorus is released gradually through diffusion, ion exchange, and slow dissociation of the laminations, thereby significantly reducing the phosphorus release rate.

[0076] The above results show that the core-shell type sustained-release structure constructed in this application can effectively prolong the phosphorus release cycle, improve nutrient utilization efficiency and reduce the risk of phosphorus loss, which fully demonstrates that the polymer encapsulation step is the key technical feature for achieving the technical effect of this application.

[0077] Example 2 This embodiment provides a method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediates based on phosphogypsum leachate, comprising the following steps: S1, the phosphogypsum permeate is pumped into an electrodialysis device with 50 pairs of cation exchange membranes and anion exchange membranes arranged alternately to form a membrane stack structure for electrodialysis ion enrichment treatment, corresponding to the production of cation concentrate, anion concentrate, and desalination solution; wherein, the sheet resistivity of the anion exchange membrane is 13 Ω·cm. 2 The sheet resistance of the cation exchange membrane is 11 Ω·cm. 2 It also exhibits high selectivity for divalent cations.

[0078] The electrodialysis operating voltage is controlled at 22V, and the current density is 35mA / cm². 2 The process continued until the conductivity of the desalination solution dropped to 1.2 mS / cm, and the Ca in the cation concentrate... 2+ Concentration of 20 g / L, Mg 2+ Stop when the concentration reaches 10 g / L.

[0079] Based on testing and calculation, the Ca²⁺ content in this step... + and Mg² + The overall recovery rate was 88%, SO4 2- The transfer rate was 93%. The meaning of recovery rate and transfer rate, and their significance for subsequent processes, are the same as in Example 1.

[0080] S2, the obtained cation concentrate is subjected to low-temperature concentration and conditioning to remove Ca2+ The concentration was adjusted to 15 g / L, Mg 2+ The concentration was adjusted to 7 g / L. Then, calcium hydroxide was added to control the pH at 4.5, allowing Fe... 3+ As 3+ Cu 2+ and Zn 2+ Impurity ions form insoluble hydroxides, while Ca... 2+ With Mg 2+ While still in a dissolved state, after stirring for 40 minutes, plate and frame filtration was used to remove the heavy metal precipitate, yielding pure Ca. 2+ -Mg 2+ Mix the raw material liquid.

[0081] S3, Ca 2+ -Mg 2+ Adjust the pH of the mixed raw material solution to 3.5, add cast iron scrap and waste iron powder, and add them in proportions of Fe and Ca. 2+ +Mg 2+ The molar ratio is controlled at 1:1.5.

[0082] Stir at room temperature for 45 minutes, simultaneously introducing air at a gas-liquid ratio of 5:1 and an aeration rate of 1.2 L air / (L solution·min). Continue the reaction until the system pH reaches 6 and Fe... 2+ The process was stopped at a concentration of 0.07 g / L, resulting in the formation of Fe. 3+ -Ca 2+ -Mg 2+ Multi-metal ion system.

[0083] S4, towards Fe 3+ -Ca 2+ -Mg 2+ Adding disodium hydrogen phosphate to a multi-metal ion system controls PO4. 3- The molar ratio of the total metal ions to the total metal ions is 1:2.1.

[0084] The stirring speed was 400 r / min, and 1.5 mol / L NaOH solution was added dropwise at a rate of 1.5 mL / (L·min) to adjust the pH of the system to 10.8. The reaction was stirred for 105 minutes. Subsequently, the mixed slurry was aged at 75 °C with low stirring speed of 75 rpm for 22 hours to obtain Ca-Mg-Fe-PO4 type LDH precipitate.

[0085] S5, the Ca-Mg-Fe-PO4 type LDH precipitate was subjected to solid-liquid separation to obtain a filter cake, which was then dispersed into a slurry with a mass concentration of 7%. An anionic agricultural functional substance (paraquat) was selected and mixed with LDH at a mass ratio of 1:4, and stirred at 45℃ for 60 minutes for ion exchange loading.

[0086] After loading was completed, chitosan was added, and the mixture was stirred at 55°C for 30 minutes and then encapsulated to obtain a Ca-Mg-Fe-PO4 type LDH multipurpose agricultural slow-release phosphorus intermediate.

[0087] Example 3 This embodiment provides a method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediates based on phosphogypsum leachate, including the following steps: S1, the phosphogypsum permeate is pumped into an electrodialysis device with 60 pairs of cation exchange membranes and anion exchange membranes arranged alternately to form a membrane stack structure for electrodialysis ion enrichment treatment, corresponding to the production of cation concentrate, anion concentrate, and desalination solution; wherein, the sheet resistivity of the anion exchange membrane is 14 Ω·cm. 2 The sheet resistance of the cation exchange membrane is 12 Ω·cm. 2 It also exhibits high selectivity for divalent cations.

[0088] The electrodialysis operating voltage is controlled at 30V, and the current density is 50mA / cm². 2 The process continued until the conductivity of the desalination solution dropped to 1.5 mS / cm, and the Ca in the cation concentrate... 2+ Concentration of 25 g / L, Mg 2+ Stop when the concentration reaches 12 g / L.

[0089] Based on testing and calculation, the Ca²⁺ content in this step... + and Mg² + The overall recovery rate was 90% for SO4. 2- The transfer rate was 95%. The meaning of recovery rate and transfer rate, and their significance for subsequent processes, are the same as in Example 1.

[0090] S2, the obtained cation concentrate is subjected to low-temperature concentration and conditioning to remove Ca 2+ The concentration was adjusted to 20 g / L, Mg 2+ The concentration was adjusted to 10 g / L. Then, sodium sulfide was added, and the pH was controlled to 5.0, so that Fe... 3+ As 3+ Cu 2+ and Zn 2+ Impurity ions form sulfide precipitates, while Ca... 2+ With Mg 2+ While still in a dissolved state, after stirring for 50 minutes, plate and frame filtration was used to remove the heavy metal precipitate, yielding pure Ca. 2 + -Mg 2+ Mix the raw material liquid.

[0091] S3, Ca 2+ -Mg 2+ Adjust the pH of the mixed raw material solution to 4.0, add cast iron scrap and waste iron powder, and add them in proportions of Fe and Ca.2+ +Mg 2+ Molar ratio controlled at 1:2.

[0092] Stirring at room temperature for 60 minutes, with simultaneous air aeration at a gas-liquid ratio of 5:1 and an aeration rate of 1.5 L air / (L solution·min), until the system pH reaches 6.5 and Fe... 2+ The process was stopped at a concentration of 0.06 g / L, resulting in the formation of Fe. 3+ -Ca 2+ -Mg 2+ Multi-metal ion system.

[0093] S4, towards Fe 3+ -Ca 2+ -Mg 2+ Adding disodium hydrogen phosphate to a multi-metal ion system controls PO4. 3- The molar ratio of the total metal ions to the total metal ions is 1:2.2.

[0094] The stirring speed was 500 r / min, and 2 mol / L NaOH solution was added dropwise at a rate of 2 mL / (L·min) to adjust the pH of the system to 11. The reaction was stirred for 120 minutes. Subsequently, the mixed slurry was aged at 80℃ with low stirring speed of 100 rpm for 24 hours to obtain Ca-Mg-Fe-PO4 type LDH precipitate.

[0095] S5, the Ca-Mg-Fe-PO4 type LDH precipitate was subjected to solid-liquid separation to obtain a filter cake, which was then dispersed into a slurry with a mass concentration of 10%. A non-ionic agricultural functional substance (triazolone) was selected, and sodium dodecylbenzenesulfonate was added as a surfactant. The mixture was stirred and loaded for 60 minutes using a surface adsorption method.

[0096] After loading was completed, chitosan was added, and the mixture was stirred at 60°C for 30 minutes and then encapsulated to obtain a Ca-Mg-Fe-PO4 type LDH multipurpose agricultural slow-release phosphorus intermediate.

[0097] It should be noted that the process parameters of this application, such as the number of electrodialysis membranes, operating voltage, iron powder dosage, molar ratio, reaction temperature and time, can be reasonably adjusted according to the actual ion concentration of the phosphogypsum leachate and the product performance requirements, and are all within the protection scope of this application.

[0098] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediates based on phosphogypsum leachate, characterized in that, Includes the following steps: S1, the phosphogypsum leachate is pumped into an electrodialysis device for electrodialysis ion enrichment treatment to obtain cation concentrate, anion concentrate and desalination desalination solution. S2, the cation concentrate is conditioned, and then sodium sulfide or calcium hydroxide is added to adjust the pH of the system to 4.0-5.0, so that Fe... 3+ As 3+ Cu 2+ and Zn 2+ The formation of insoluble hydroxide or sulfide precipitates is observed; after filtration, pure Ca is obtained. 2 + -Mg 2+ Mixed raw material liquid; S3, adjust the Ca 2+ -Mg 2+ The pH of the mixed raw material solution is adjusted to 3.0-4.0, followed by the addition of scrap iron powder. After the scrap iron powder corrodes and dissolves, it undergoes an in-situ oxidation reaction to form Fe. 3+ -Ca 2+ -Mg 2+ Multi-metal ion system; S4, to the Fe 3+ -Ca 2+ -Mg 2+ A Ca-Mg-Fe-PO4 type LDH precipitate was obtained by adding soluble phosphate and precipitant to a multi-metal ion system and then reacting with stirring and aging. S5, the Ca-Mg-Fe-PO4 type LDH precipitate is subjected to solid-liquid separation to obtain filter cake; the filter cake is dispersed into LDH slurry, and agricultural functional substances are loaded using an appropriate loading method, followed by the addition of polymer for encapsulation treatment to obtain Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate.

2. The method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate based on phosphogypsum leachate according to claim 1, characterized in that, When the agricultural functional substance is an anionic agricultural functional substance, it is intercalated and loaded at 40-50℃ for 60-120 min using the ion exchange method; the mass ratio of the anionic agricultural functional substance to LDH is 1:(3-5). When agricultural functional substances are non-ionic or weakly polar, surface adsorption is used for loading.

3. The method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediates based on phosphogypsum leachate according to claim 1, characterized in that, The electrodialysis device consists of alternating cation exchange membranes and anion exchange membranes to form a membrane stack structure. In step S1, under the action of a DC electric field, cations migrate through the cation exchange membrane to the cation concentration chamber, and anions migrate through the anion exchange membrane to the anion concentration chamber, forming a desalination solution in the intermediate chamber.

4. The method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate based on phosphogypsum leachate according to claim 1, characterized in that, During electrodialysis ion enrichment treatment, the operating voltage is 15-30V and the current density is 20-50mA / cm³. 2 The operation will stop when the conductivity of the desalination solution drops to 1.0-1.5 mS / cm.

5. The method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate based on phosphogypsum leachate according to claim 1, characterized in that, The conditioning treatment refers to low-temperature concentration; after conditioning treatment, the Ca in the cation concentrate... 2+ Concentration of 10-20 g / L, Mg 2+ The concentration is 5-10 g / L.

6. The method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate based on phosphogypsum leachate according to claim 1, characterized in that, The scrap iron powder is cast iron shavings or low-carbon steel shavings, with an Fe content >90% and a particle size of 100-200 mesh; the dosage of the scrap iron powder is based on the ratio of Fe to Ca. 2+ and Mg 2+ The ratio of the sum of the molar amounts is 1:(1-2) control.

7. The method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate based on phosphogypsum leachate according to claim 1, characterized in that, The conditions for the in-situ oxidation reaction are: stirring at room temperature for 30-60 min, gas-liquid ratio of 5:1, aeration rate of 1.0-1.5 L air / (L solution·min), and reaction until the system pH is 5.5-6.5 and Fe... 2+ Stop when the concentration is <0.1g / L.

8. The method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate based on phosphogypsum leachate according to claim 1, characterized in that, In step S4, the precipitant is a 1.0-2.0 mol / L NaOH solution, and the dropping rate of the precipitant is 1-2 mL / (L·min). During the reaction, the pH of the system is controlled at 10.5-11.

0. After stirring for 90-120 min, the mixture is aged at 75±5℃ with low stirring at 50-100 rpm for 20-24 h. The soluble phosphate contains PO4 3- The molar ratio of the total metal ions in the multi-metal ion system is 1:(2-2.2).

9. The method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate based on phosphogypsum leachate according to claim 1, characterized in that, In step S5, the polymer is pectin, chitosan, or polyacrylate.

10. The method for preparing Ca-Mg-Fe-PO4 type slow-release phosphorus intermediate based on phosphogypsum leachate according to claim 1, characterized in that, The encapsulation process refers to stirring and reacting at 50-60℃ for 30-60 minutes to form a continuous coating layer on the surface of LDH particles, which is then cross-linked and cured to form core-shell type sustained-release particles of LDH-functional component-polymer.