A superhydrophobic composite coating with a triple scale-inhibiting structure and its preparation method

By utilizing a superhydrophobic composite coating with a triple scale-inhibiting structure, and taking advantage of the synergistic effect of modified hydrophobic nano-silica and acidified multi-walled carbon nanotubes, the problem of narrow applicability and susceptibility to environmental influences of existing scale-inhibiting technologies is solved, achieving a highly efficient and durable scale-inhibiting effect.

CN123063035APending Publication Date: 2026-11-10CHENGDU UNIVERSITY OF TECHNOLOGY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611458212.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing physical and biological scale inhibition technologies have a narrow scope of application, are easily affected by the environment, and have limited effectiveness, resulting in serious scaling in industrial equipment, which reduces heat transfer efficiency and equipment life.

Method used

A superhydrophobic composite coating with a triple scale-inhibiting structure is adopted, which is composed of epoxy resin, polydimethylsiloxane, modified hydrophobic nano silica, and acidified multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid. The modified hydrophobic nano silica constructs a micro-nano rough structure, polydimethylsiloxane forms an oil layer, and acidified multi-walled carbon nanotubes loaded with chelating agents capture scale-forming ions, forming a stable superhydrophobic interface.

Benefits of technology

It achieves long-term scale inhibition in high-temperature supersaturated solutions, reduces the amount of scale per unit area, improves the protective performance of equipment, adapts to mechanical wear and thermal stress, and ensures the reliability and durability of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063035A_ABST
    Figure CN123063035A_ABST
Patent Text Reader

Abstract

This application relates to the field of scale inhibition technology, specifically disclosing a superhydrophobic composite coating with a triple scale inhibition structure and its preparation method. The superhydrophobic composite coating is made from raw materials comprising the following parts by weight: 80-120 parts epoxy resin, 15-30 parts polydimethylsiloxane, 3-8 parts modified hydrophobic nano-silica, and 2-10 parts acidified multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid. The preparation method is as follows: S1, preparing modified hydrophobic nano-silica; S2, preparing acidified multi-walled carbon nanotubes loaded with a chelating agent; S3, preparing and coating the coating. The superhydrophobic composite coating of this application can be used on the surfaces of industrial equipment in industries such as power, water treatment, and petrochemicals, namely heat exchangers, pipes, and membrane separation components. In high-temperature and high-pressure circulating water or oil well water environments, it prevents the deposition of scale such as CaCO3 and CaSO4, exhibiting multiple advantages of high-efficiency scale inhibition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of scale inhibition technology, and more specifically, to a superhydrophobic composite coating with a triple scale inhibition structure and its preparation method. Background Technology

[0002] Scaling is widespread in industries such as power generation, water treatment, and petrochemicals. In industrial water treatment systems in these industries, including boiler water, circulating cooling water, and oil well water, scale ions become supersaturated and precipitate to form insoluble salts under appropriate temperature, pressure, and pH conditions. These insoluble salts deposit in industrial equipment such as heat exchangers and membrane separation devices, causing severe scaling on pipes, valves, and membrane surfaces. This reduces heat transfer efficiency and water flow, shortens equipment lifespan, and increases operating costs.

[0003] Related scale inhibition technologies include physical scale inhibition technology and biological scale inhibition technology. Physical scale inhibition technology includes methods such as mechanical cleaning, electronic cleaning, and ultrasonic cleaning to remove surface scale through physical techniques. Biological scale inhibition technology adds active substances from natural biological sources or produced by microbial metabolism to inhibit the nucleation and growth of scale. However, both of these technologies have a narrow range of applications, are easily affected by the environment, and have limited effectiveness. Summary of the Invention

[0004] To address the issues of limited applicability, susceptibility to environmental influences, and limited effectiveness caused by the use of physical or biological scale inhibition methods, this application provides a superhydrophobic composite coating with a triple scale inhibition structure and its preparation method.

[0005] In a first aspect, this application provides a superhydrophobic composite coating with a triple scale-inhibiting structure, employing the following technical solution:

[0006] A superhydrophobic composite coating with a triple scale-inhibiting structure is made from the following raw materials in parts by weight: 80-120 parts epoxy resin, 15-30 parts polydimethylsiloxane, 3-8 parts modified hydrophobic nano-silica, and 2-10 parts acidified multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid.

[0007] By adopting the above technical solution, epoxy resin, as the coating matrix, provides mechanical strength and adhesion; polydimethylsiloxane, as a hydrophobic component, imparts surface lubricity; modified hydrophobic nano-silica forms micro- and nano-scale roughness in the coating; and acidified multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid capture scale-forming ions through chelation. These components work synergistically during the curing process, enabling the coating to integrate multiple functions, thus achieving stable superhydrophobicity and long-lasting scale inhibition.

[0008] Preferably, the modified hydrophobic nano-silica constructs a micro-nano rough structure on the coating surface and forms an air layer; the polydimethylsiloxane penetrates into the micro-nano rough structure to form an oil layer; and the acidified multi-walled carbon nanotubes loaded with chelating agents continuously release chelating agents when the air layer and oil layer are damaged, chelating with scale-forming ions to form a scale-inhibiting barrier.

[0009] By adopting the above technical solution, the modified hydrophobic nano-silica generates a Cassie-Baxter cushion layer through the arrangement of its nanoscale particles on the surface. The low surface energy of polydimethylsiloxane enables it to fill rough gaps and form a sliding interface. The acidified multi-walled carbon nanotubes enhance surface activity due to acidification treatment, can efficiently load ethylenediaminetetraacetic acid and release it in a controlled manner when there is local damage, forming a stable complex with calcium and magnesium ions. This layer-by-layer progressive design ensures that the coating can maintain its protective performance under mechanical wear or thermal stress, thus obtaining a reliable triple protection mechanism.

[0010] Preferably, the static water contact angle of the coating is greater than 150° and the roll-off angle is less than 10°; after testing in a supersaturated calcium carbonate solution at 50-70°C for 110-130 hours, the scale content per unit area is less than 0.4 mg / cm².

[0011] By adopting the above technical solution, the high contact angle and low roll-off angle are directly derived from the optimized combination of micro-nano rough structure and low surface energy material, making it difficult for water droplets to wet the surface. In the accelerated test, a high-temperature supersaturated solution is used to simulate a harsh environment. The coating reduces crystal nucleus adhesion through air layer and oil layer. At the same time, the chelating agent neutralizes ions in time and delays scale growth. These parameters have been experimentally verified to effectively characterize the durability and scale inhibition efficiency of the coating, thus obtaining quantitative performance assurance.

[0012] Secondly, this application provides a method for preparing a superhydrophobic composite coating with a triple scale-inhibiting structure, using the following technical solution:

[0013] A method for preparing a superhydrophobic composite coating with a triple scale-inhibiting structure includes the following steps:

[0014] S1. Preparation of modified hydrophobic nano silica: Disperse fumed nano silica in an organic solvent, add alkyl chlorosilane to carry out hydrophobic modification reaction, and after the reaction is completed, separate, wash and dry to obtain modified hydrophobic nano silica;

[0015] S2. Preparation of acidified multi-walled carbon nanotubes loaded with chelating agents: Acidification treatment is performed on multi-walled carbon nanotubes to obtain acidified multi-walled carbon nanotubes; then the acidified multi-walled carbon nanotubes are immersed in a chelating agent solution, loaded with chelating agents, separated and dried to obtain acidified multi-walled carbon nanotubes loaded with chelating agents.

[0016] S3, preparing and coating a coating layer: dispersing the modified hydrophobic nanosilica obtained in S1, the acidified multi-walled carbon nanotubes loaded with chelating agent obtained in S2, epoxy resin, polydimethylsiloxane and corresponding curing agent in a solvent, mixing uniformly to form a coating suspension; coating the suspension on the surface of the pretreated substrate, and obtaining the super-hydrophobic composite coating after curing.

[0017] By adopting the technical scheme, the nanosilica is endowed with persistent water repellency by hydrophobic modification in step S1, providing a structural basis for the subsequent coating layer, the surface functional groups of the carbon nanotubes are increased by acidification treatment in step S2 to enhance the loading capacity of the chelating agent and ensure the scale inhibition function, and each component is uniformly distributed by optimizing the dispersion and curing process in step S3 to form a dense coating layer, the whole process is gradual and the parameters are controllable, so that the coating layer has a complete structure and consistent performance, and a high-quality coating layer that can be repeatedly prepared is obtained.

[0018] Preferably, in the step S1, the conditions of the hydrophobic modification reaction are that the stirring reaction is carried out at 65-85℃ for 3-5 hours; and the alkylchlorosilane is dimethyloctadecylchlorosilane.

[0019] By adopting the technical scheme, the reaction temperature in the range of 65 to 85 degrees Celsius can promote the full reaction of the alkylchlorosilane and the hydroxyl groups on the surface of the nanosilica to form stable siloxane bonds, the stirring time of 3 to 5 hours ensures uniform modification and avoids excessive polymerization, and the long-chain alkyl group of dimethyloctadecylchlorosilane can effectively reduce the surface energy, these conditions are determined based on reaction kinetics and surface energy optimization, so that the modified nanosilica has a uniform hydrophobic layer, and thus an ideal micro-nano building unit is obtained.

[0020] Preferably, the step S2 comprises:

[0021] S21, acidification treatment: placing the multi-walled carbon nanotubes in a mixed acid of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of (2.5:1) to (3.5:1), stirring and treating at 65-85℃ for 5-9 hours, then washing to neutral and drying to obtain acidified multi-walled carbon nanotubes;

[0022] S22, loading chelating agent: immersing the acidified multi-walled carbon nanotubes in an ethylenediaminetetraacetic acid aqueous solution with a concentration of 0.05-0.15 mol / L, stirring at room temperature for 18-30 hours, then separating and drying to obtain acidified multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid.

[0023] By adopting the technical scheme, since the proportion of mixed acid and the temperature and time parameters in the acidification treatment can controllably introduce carboxyl and hydroxyl functional groups, the hydrophilicity and loading capacity of the carbon nanotubes are enhanced, the loading step adopts a specific concentration of ethylenediaminetetraacetic acid solution and stirring at room temperature, the molecules are beneficial to entering the wall through physical adsorption and ion exchange, this step-by-step treatment ensures that the chelating agent is uniformly distributed and is not easy to leak, and the coating provides sustainable scale inhibition capacity, and therefore the functionalized nanofiller is obtained.

[0024] Preferably, in the S3 step, the pretreatment is mechanical polishing of the surface of the substrate by using 400-800 mesh sandpaper, and then ultrasonic cleaning is sequentially performed by using anhydrous ethanol and acetone, and the time for each ultrasonic cleaning is 20-40 minutes.

[0025] By adopting the technical scheme, since mechanical polishing creates appropriate roughness by different mesh sandpaper to enhance the adhesion of the coating, and ultrasonic cleaning removes grease and impurities by using solvents, and the cleaning time of 20 to 40 minutes ensures thorough cleaning without damaging the substrate, and this pretreatment provides a clean and activated surface for the coating, reduces interface defects, and therefore a firm coating bonding foundation is obtained.

[0026] Preferably, the S3 step comprises:

[0027] S31, mixing and dispersing: the modified hydrophobic nanosilica obtained in S1 and the acidized multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid obtained in S2 are added into an acetone solvent, ultrasonic dispersion is first performed for 20-40 minutes, and then magnetic stirring is performed for 20-40 minutes; then, epoxy resin, polydimethylsiloxane and the corresponding curing agent thereof are added, and magnetic stirring is continued for 1-2 hours to obtain a uniform coating suspension;

[0028] S32, coating and curing: the coating suspension is coated on the surface of the pretreated substrate by using a spraying method, the spraying pressure is 0.3-0.7 MPa, and the spraying distance is 10-20 cm; then, the coated substrate is cured at 70-90°C for 1.5-2.5 hours.

[0029] By adopting the technical scheme, since the combination of ultrasonic and stirring in the mixing and dispersing can break the agglomeration of nanoparticles to achieve uniform suspension, and avoids local concentration unevenness, and the spraying parameters such as pressure and distance control the coating thickness and coverage, and the curing temperature and time promote the crosslinking of the epoxy resin and the forming of the polydimethylsiloxane, and a stable network structure is formed, and these process details are optimized based on rheology and curing kinetics, and the integrity of the coating microstructure is ensured, and therefore a uniform and durable triple scale inhibition coating is obtained.

[0030] Preferably, in the S3 step, a dispersant is also added, accounting for 0.1-1% of the total solid mass of the coating, wherein the dispersant is added together when the modified hydrophobic nanosilica and the acidified multi-walled carbon nanotube loaded with ethylenediaminetetraacetic acid are ultrasonically dispersed in the acetone solvent.

[0031] By adopting the technical solution, the dispersant prevents the nanoparticles from agglomerating through steric hindrance or electrostatic repulsion, and the effective coverage is ensured by calculating the addition amount based on the solid mass ratio. The addition timing maximizes the dispersion effect at the initial stage of ultrasonic, improves the uniformity of the coating, and thus a stable suspension and enhanced coating performance are obtained.

[0032] Preferably, the dispersant is polyvinylpyrrolidone or sodium polyacrylate.

[0033] By adopting the technical solution, the selection of polyvinylpyrrolidone or sodium polyacrylate is based on its compatibility with acetone and nanomaterials.

[0034] In summary, the present application has the following beneficial effects:

[0035] 1. Since the present application adopts a synergistic ratio of epoxy resin, polydimethylsiloxane, modified hydrophobic nanosilica, and acidified multi-walled carbon nanotube loaded with ethylenediaminetetraacetic acid, the epoxy resin provides mechanical strength as the matrix, the polydimethylsiloxane imparts surface lubricity, the modified nanosilica constructs micro-nano roughness, and the carbon nanotube loaded with chelating agent captures ions through chelation, thereby enabling the coating to form a stable super-hydrophobic interface and reducing scale deposition, and thus high-efficiency and long-lasting scale inhibition performance is obtained.

[0036] 2. In the present application, the modified hydrophobic nanosilica is preferably used to form an air layer on the surface of the coating, and the polydimethylsiloxane is used to penetrate the rough structure to produce an oil layer, and the acidified multi-walled carbon nanotube loaded with ethylenediaminetetraacetic acid is used as a backup barrier, wherein the air layer reduces scale adhesion, the oil layer reduces surface energy to inhibit heterogeneous nucleation, and the chelating agent can be released to complex with calcium and magnesium ions when the local damage is controlled, thereby ensuring that the coating does not lose its function under mechanical wear or thermal stress, and thus reliable adaptive protection effect is obtained.

[0037] 3. The method of the present application uses a step-by-step preparation process, including hydrophobic modified nanosilica, acidified loaded carbon nanotube, and improved coating and curing steps, wherein the modification step provides a uniform rough base for the coating, the loading step enhances the chelating capacity, and the dispersion and curing parameters ensure uniform distribution of components, making the coating microstructure complete, and thus a coating with strong repeatability and consistent performance is obtained, which exhibits high scale inhibition efficiency in high-temperature supersaturated solutions. BRIEF DESCRIPTION OF DRAWINGS

[0038] Figure 1A flow chart of a preparation method of an ultra-hydrophobic composite coating with a triple anti-fouling structure according to the present application is shown in the figure;

[0039] Figure 2 A graph of the amount of CaCO3 and CaSO4 fouling on the surface of different coatings over time after a fouling test of 120 hours, and XRD and FTIR graphs of CaCO3 and CaSO4

[0040] Figure 3 A SEM graph of CaCO3 deposition on the surface of different coatings;

[0041] Figure 4 A SEM graph of CaSO4 deposition on the surface of different coatings;

[0042] Figure 5 A schematic diagram of the anti-fouling mechanism of the coating. DETAILED DESCRIPTION

[0043] The present application is further described in detail below with reference to the accompanying drawings and examples.

[0044] Example 1: This example provides an ultra-hydrophobic composite coating with a triple anti-fouling structure, which is made from raw materials including the following by weight: 80 parts of epoxy resin, 15 parts of polydimethylsiloxane, 3 parts of modified hydrophobic nanosilica, and 2 parts of acidified multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid.

[0045] The modified hydrophobic nanosilica forms a micro-nano rough structure on the surface of the coating and an air layer; the polydimethylsiloxane penetrates into the micro-nano rough structure to form an oil layer; and the acidified multi-walled carbon nanotubes loaded with the chelating agent continuously release the chelating agent to chelate with the fouling ions and form an anti-fouling barrier when the air layer and the oil layer are damaged. The static water contact angle of the coating is greater than 150°, and the rolling angle is less than 10°. After testing in a saturated calcium carbonate solution at 50°C for 110 hours, the fouling amount per unit area is less than 0.4 mg / cm2.

[0046] The above-mentioned preparation method of an ultra-hydrophobic composite coating with a triple anti-fouling structure includes the following steps:

[0047] S1, preparing modified hydrophobic nanosilica: dispersing fumed nanosilica in an organic solvent, adding alkylchlorosilane for hydrophobic modification reaction, separating, washing and drying after the reaction is completed to obtain modified hydrophobic nanosilica.

[0048] The conditions of the hydrophobic modification reaction are: stirring at 65°C for 3 hours; and the alkylchlorosilane is dimethyloctadecylchlorosilane.

[0049] S2, preparing acidized multi-walled carbon nanotubes loaded with chelating agent: acidizing multi-walled carbon nanotubes to obtain acidized multi-walled carbon nanotubes; then dipping the acidized multi-walled carbon nanotubes in a chelating agent solution, separating and drying after loading the chelating agent to obtain acidized multi-walled carbon nanotubes loaded with chelating agent.

[0050] In the step S2, the acidizing treatment is performed by placing the multi-walled carbon nanotubes in a mixed acid of concentrated sulfuric acid and concentrated nitric acid with a volume ratio of 2.5:1, stirring at 65℃ for 5 hours, then washing to neutral and drying to obtain the acidized multi-walled carbon nanotubes. The loading of the chelating agent is performed by dipping the acidized multi-walled carbon nanotubes in an ethylenediaminetetraacetic acid aqueous solution with a concentration of 0.05 mol / L, stirring at room temperature for 18 hours, then separating and drying to obtain the acidized multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid.

[0051] S3, preparing and coating the coating layer: dispersing the modified hydrophobic nanosilica obtained in S1, the acidized multi-walled carbon nanotubes loaded with chelating agent obtained in S2, the epoxy resin, the polydimethylsiloxane and the corresponding curing agent in a solvent, mixing uniformly to form a coating suspension; coating the suspension on the surface of the pretreated substrate, and obtaining the super-hydrophobic composite coating after curing.

[0052] In the step S3, the pretreatment is performed by mechanically polishing the surface of the substrate with 400 mesh sandpaper, then ultrasonic cleaning with anhydrous ethanol and acetone in sequence, and the ultrasonic cleaning time is 20 minutes each time. The mixing and dispersing in the step S31 is performed by adding the modified hydrophobic nanosilica obtained in S1 and the acidized multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid obtained in S2 into the acetone solvent, ultrasonic dispersing for 20 minutes first, then magnetic stirring for 20 minutes; then adding the epoxy resin, the polydimethylsiloxane and the corresponding curing agent, continuing magnetic stirring for 1 hour to obtain a uniform coating suspension; the coating and curing in the step S32 is performed by coating the coating suspension on the surface of the pretreated substrate by spraying, the spraying pressure is 0.3 MPa, and the spraying distance is 10 cm; then curing the coated substrate at 70℃ for 1.5 hours; the viscosity of the finally obtained coating suspension is controlled at 80 mPa·s; in the mixing and dispersing process in the step S3, 0.1% of dispersant based on the total solid mass of the coating is also added, and the dispersant is added together when the modified hydrophobic nanosilica and the acidized multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid are added into the acetone solvent for ultrasonic dispersing, and the dispersant is polyvinylpyrrolidone.

[0053] Example 2: The super-hydrophobic composite coating with a triple scale inhibition structure is prepared from the following raw materials by weight: epoxy resin 100 parts, polydimethylsiloxane 23 parts, modified hydrophobic nanosilica 6 parts, and acidized multi-walled carbon nanotubes loaded with ethylenediaminetetraacetate 6 parts.

[0054] The modified hydrophobic nanosilica constructs a micro-nano rough structure and forms an air layer on the surface of the coating; the polydimethylsiloxane penetrates into the micro-nano rough structure to form an oil layer; and the acidified multi-walled carbon nanotube loaded with a chelating agent continuously releases the chelating agent to chelate with scale-forming ions to form a scale inhibition barrier when the air layer and the oil layer are damaged; the static water contact angle of the coating is greater than 150°, and the rolling angle is less than 10°; and the scale deposition per unit area is less than 0.4 mg / cm2 after being tested in a supersaturated calcium carbonate solution at 60℃ for 120 hours.

[0055] The preparation method of the above-mentioned super-hydrophobic composite coating with a triple scale inhibition structure comprises the following steps:

[0056] S1, preparing modified hydrophobic nanosilica: dispersing fumed nanosilica in an organic solvent, adding alkylchlorosilane for hydrophobic modification reaction, separating, washing and drying after the reaction is completed to obtain modified hydrophobic nanosilica.

[0057] In the hydrophobic modification reaction, the conditions are stirring at 75℃ for 4 hours, and the alkylchlorosilane is dimethyloctadecylchlorosilane.

[0058] S2, preparing acidified multi-walled carbon nanotube loaded with a chelating agent: acidifying multi-walled carbon nanotubes to obtain acidified multi-walled carbon nanotubes; then immersing the acidified multi-walled carbon nanotubes in a chelating agent solution, separating and drying after loading the chelating agent to obtain acidified multi-walled carbon nanotube loaded with a chelating agent.

[0059] In the step S2, S21, acidification treatment: placing the multi-walled carbon nanotubes in a mixed acid of concentrated sulfuric acid and concentrated nitric acid with a volume ratio of 3.0:1, stirring at 75℃ for 7 hours, then washing to neutral and drying to obtain acidified multi-walled carbon nanotubes; S22, loading a chelating agent: immersing the acidified multi-walled carbon nanotubes in an ethylenediaminetetraacetic acid aqueous solution with a concentration of 0.10 mol / L, stirring at room temperature for 24 hours, then separating and drying to obtain acidified multi-walled carbon nanotube loaded with ethylenediaminetetraacetic acid.

[0060] S3, preparing and coating a coating: dispersing the modified hydrophobic nanosilica obtained in S1, the acidified multi-walled carbon nanotube loaded with a chelating agent obtained in S2, an epoxy resin, polydimethylsiloxane and a corresponding curing agent in a solvent, mixing uniformly to form a coating suspension; coating the suspension on the surface of a pretreated substrate, and obtaining a super-hydrophobic composite coating after curing.

[0061] The pretreatment is mechanical polishing of the surface of the substrate with 600-mesh sandpaper, followed by ultrasonic cleaning with anhydrous ethanol and acetone in sequence, and the time for each ultrasonic cleaning is 30 minutes; the S3 step comprises: S31, mixed dispersion: adding the modified hydrophobic nanosilica obtained in S1 and the acidified multi-walled carbon nanotube loaded with ethylenediaminetetraacetic acid obtained in S2 into an acetone solvent, ultrasonic dispersion for 30 minutes first, and then magnetic stirring for 30 minutes; subsequently, adding the epoxy resin, polydimethylsiloxane and the corresponding curing agent thereof, and continuing magnetic stirring for 1.5 hours to obtain a uniform coating suspension; S32, coating and curing: coating the coating suspension on the surface of the pretreated substrate by spraying, the spraying pressure is 0.5 MPa, and the spraying distance is 15 cm; then curing the coated substrate at 80℃ for 2.0 hours; the viscosity of the finally obtained coating suspension is controlled to be 190 mPa·s; in the mixed dispersion process of the S3 step, 0.5% of a dispersant based on the total solid mass of the coating is also added, wherein the dispersant is added together when the modified hydrophobic nanosilica and the acidified multi-walled carbon nanotube loaded with ethylenediaminetetraacetic acid are added into the acetone solvent for ultrasonic dispersion, and the dispersant is polyvinylpyrrolidone.

[0062] Example 3: The present example provides an ultrahydrophobic composite coating with a triple anti-fouling structure, which is made from raw materials comprising the following weight parts: epoxy resin 120 parts, polydimethylsiloxane 30 parts, modified hydrophobic nanosilica 8 parts, and acidified multi-walled carbon nanotube loaded with ethylenediaminetetraacetic acid 10 parts.

[0063] The modified hydrophobic nanosilica constructs a micro-nano rough structure on the surface of the coating and forms an air layer; the polydimethylsiloxane penetrates into the micro-nano rough structure to form an oil layer; and the acidified multi-walled carbon nanotube loaded with a chelating agent continuously releases the chelating agent when the air layer and the oil layer are damaged, chelates with the fouling ions, and forms an anti-fouling barrier; the static water contact angle of the coating is greater than 150°, and the rolling angle is less than 10°; after being tested in a supersaturated calcium carbonate solution at 70℃ for 130 hours, the fouling amount per unit area is less than 0.4 mg / cm².

[0064] The above method for preparing an ultrahydrophobic composite coating with a triple anti-fouling structure comprises the following steps:

[0065] S1, preparing modified hydrophobic nanosilica: dispersing fumed nanosilica in an organic solvent, adding alkylchlorosilane for hydrophobic modification reaction, separating, washing and drying after the reaction is completed to obtain modified hydrophobic nanosilica.

[0066] The conditions for the hydrophobic modification reaction are: stirring at 85℃ for 5 hours; and the alkylchlorosilane is dimethyloctadecylchlorosilane.

[0067] S2. Preparation of acidified multi-walled carbon nanotubes loaded with chelating agents: Acidification treatment is performed on multi-walled carbon nanotubes to obtain acidified multi-walled carbon nanotubes; then the acidified multi-walled carbon nanotubes are immersed in a chelating agent solution, loaded with chelating agent, separated and dried to obtain acidified multi-walled carbon nanotubes loaded with chelating agents.

[0068] Step S2 includes: S21, acidification treatment: multi-walled carbon nanotubes are placed in a mixed acid of concentrated sulfuric acid and concentrated nitric acid with a volume ratio of 3.5:1, stirred at 85°C for 9 hours, then washed until neutral and dried to obtain acidified multi-walled carbon nanotubes; S22, loading chelating agent: acidified multi-walled carbon nanotubes are immersed in a 0.15 mol / L aqueous solution of ethylenediaminetetraacetic acid, stirred at room temperature for 30 hours, separated and dried to obtain acidified multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid.

[0069] S3. Preparation and coating: The modified hydrophobic nano-silica obtained in S1, the acidified multi-walled carbon nanotubes loaded with chelating agents obtained in S2, epoxy resin, polydimethylsiloxane and corresponding curing agents are dispersed in a solvent and mixed evenly to form a coating suspension; the suspension is coated on the surface of the pretreated substrate, and after curing, a superhydrophobic composite coating is obtained.

[0070] The pretreatment process involves mechanically polishing the substrate surface with 800-grit sandpaper, followed by ultrasonic cleaning with anhydrous ethanol and acetone, each ultrasonic cleaning lasting 40 minutes. Step S3 includes: S31, mixing and dispersing: adding the modified hydrophobic nano-silica obtained in S1 and the acidified multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid obtained in S2 to acetone solvent, ultrasonically dispersing for 40 minutes, and then magnetically stirring for 40 minutes; subsequently, adding epoxy resin, polydimethylsiloxane and its corresponding curing agent, and continuing magnetic stirring for 2 hours to obtain a uniform coating suspension; S32, coating and... Curing: The coating suspension was applied to the pretreated substrate surface by spraying at a pressure of 0.7 MPa and a distance of 20 cm. The coated substrate was then cured at 90°C for 2.5 hours. The viscosity of the final coating suspension was controlled to be 300 mPa·s. During the mixing and dispersion process in step S3, a dispersant accounting for 1.0% of the total solid mass of the coating was added. The dispersant was added together with the modified hydrophobic nano-silica and the acidified multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid in acetone solvent for ultrasonic dispersion. The dispersant was polyvinylpyrrolidone.

[0071] Comparative Example 1: The blank substrate without suspension coating after pretreatment in Example 1 was taken as the control group of the example.

[0072] Performance testing

[0073] Sample preparation: Substrates coated with superhydrophobic composite coatings were prepared according to Examples 1-3, and blank substrates for Comparative Example 1 were prepared.

[0074] Scale inhibition test: includes scale inhibition solution preparation and scale inhibition performance analysis.

[0075] Scale inhibition solution preparation: The scale inhibition performance of the coating was tested by placing it in solutions containing supersaturated calcium carbonate and calcium sulfate, respectively. The preparation process of the supersaturated solution is shown below:

[0076] A supersaturated calcium carbonate solution is prepared from 0.06 mol / L -1 Ca(NO3)2·4H2O and 0.12 mol L -1 NaHCO3 solution is obtained through a reaction, and the specific reaction equation is shown in the following formula:

[0077] Ca(NO3)2·4H2O+2NaHCO3→CaCO3↓+2NaNO3+5H2O+CO2↑

[0078] A supersaturated calcium sulfate solution is prepared from 0.06 mol / L -1 Na2SO4 and 0.06 mol / L -1 CaCl2 solution is obtained through a reaction, and the specific reaction equation is shown in the figure below:

[0079] Na₂SO₄ + CaCl₂ → CaSO₄↓ + 2NaCl

[0080] The specific test steps are as follows: First, prepare 250 mL each of the corresponding concentrations of Ca(NO3)2·4H2O, NaHCO3, Na2SO4, and CaCl2 solutions, and sonicate for 10 min to form a homogeneous solution. Then, vertically immerse the prepared superhydrophobic scale-inhibiting coatings into solutions containing Ca(NO3)2·4H2O and Na2SO4, respectively. Next, add NaHCO3 and CaCl2 solutions to the solutions containing Ca(NO3)2·4H2O and Na2SO4, respectively. Heat in a 60℃ constant temperature water bath. After a period of time, remove the samples, gently rinse with a small amount of deionized water, and dry in an 80℃ oven. After the substrate surface is completely dry, record the substrate weight, and quantitatively evaluate the scale-inhibiting performance of the coating by calculating the amount of scale per unit area on the surface of each coating.

[0081] Scale inhibition performance analysis: Coatings (1)-(4) represent blank substrate, EP@PDMS coating, EP@PDMS@Modified SiO2 and EP@PDMS@Modified SiO2@EDTA-FMWCNTs coating, respectively. Figure 2(a) is a curve showing the change in the amount of CaCO3 deposited per unit area on the surface of each coating over time in a saturated CaCO3 solution at 60℃; Figure 2 (a) It can be seen that within 120 hours of scaling, the surface of blank Q235 steel had the largest scale accumulation per unit area, followed by the EP@PDMS coating and the EP@PDMS@ModifiedSiO2 coating, and finally the EP@PDMS@ModifiedSiO2@EDTA-FMWCNTs coating, indicating that the superhydrophobic scale inhibitory coatings have excellent scale inhibition effects. During the first 24 hours of scaling, the crystal nucleation and growth stages were in progress, and the scale accumulation on the surfaces of each coating was 4.592 mg / cm², 2.304 mg / cm², 1.064 mg / cm², and 0.304 mg / cm², respectively. This indicates that the EP@PDMS@ModifiedSiO2 coating, due to its low surface energy, anti-adhesion properties, and superhydrophobicity, inhibited the deposition of CaCO₃ on the coating surface. The EP@PDMS@ModifiedSiO₂@EDTA-FMWCNTs coating, based on these characteristics, introduced EDTA, which gradually released CaCO₃ in the scaling solution. 2+ Chelation forms stable complexes, which hinder the nucleation and growth of CaCO3 crystals.

[0082] CaCO3 crystals are mainly classified into three types: calcite, aragonite, and granite. Calcite is the most stable but also the most difficult to remove. Aragonite and granite, which are metastable, have poor adhesion and are more susceptible to environmental influences, making them easier to detach. If the scale deposited on the coating surface is mainly composed of aragonite and granite, the coating will have a better scale inhibition effect. Therefore, to examine the scale inhibition effect of each coating, the CaCO3 crystal forms on the surfaces of different coatings after 120 hours of deposition were characterized by XRD. Figure 2(b) shows the blank substrate surface, the EP@PDMS coating, and the EP@PDMS@Modified coating. The CaCO3 crystal form on the SiO2 coating surface is mainly calcite, with some aragonite and globule mixed in. The characteristic diffraction peaks of calcite appear at 2θ of 23.06° (012), 29.42° (104), 35.98° (100), 47.52° (018), 48.52° (116) and 57.40° (122), the characteristic diffraction peak of globule appears at 43.84° (300), and the characteristic peak of aragonite appears at 31.46° (002), 39.42° (130) and 63.06° (321). This indicates that the addition of modified materials and resin reduces the surface free energy of the coating, enhances the hydrophobicity of the coating surface, and brings excellent anti-adhesion and rough micro-nanopapular structure. To a certain extent, it inhibits the deposition of calcite on the coating surface and induces the formation of metastable aragonite and globule. The surface of the EP@PDMS@Modified SiO2@EDTA-FMWCNs coating is composed of a small amount of calcite, aragonite and spheroidal aragonite, indicating that the coating deposits chelating EDTA under the original air layer and oil layer structure, forming a triple scale inhibition structure and improving the scale inhibition rate.

[0083] Figure 2 (c) FTIR spectra of CaCO3 deposited on the surfaces of each coating. As shown in the figure, the characteristic CO peak in CaCO3 is located at 1384 cm⁻¹. -1 and 873cm -1 In this location, it only appears on the surface of the blank substrate and in the EP@PDMS coating, while the EP@PDMS@Modified SiO2 coating and the EP@PDMS@Modified SiO2@EDTA-FMWCNs coating appear at 800 cm⁻¹. -1 and 1261cm -1 The characteristic peaks of Si-O-Si and -CH3 appear at 1616 cm⁻¹, originating from the vibrations of hydrophobic SiO₂ and PDMS. In contrast, only the EP@PDMS@Modified SiO₂@EDTA-FMWCNs coating shows this at 1616 cm⁻¹. -1 and 1508cm -1 The presence of skeletal vibrations in the aromatic rings of the main chain in EP indicates that the EP@PDMS@ModifiedSiO2@EDTA-FMWCNTs coating not only has excellent scale inhibition properties but also excellent corrosion resistance.

[0084] Figure 2 (d) shows the curves of CaSO4 deposition per unit area on the surface of each coating over time in a saturated CaSO4 solution at 60℃. During the 120-hour scaling test, the blank substrate surface showed the highest CaSO4 scaling amount, at 5.904 mg / cm³. 2The second highest scale buildup was observed on the EP@PDMS coating surface, at 3.728 mg / cm³. 2 The EP@PDMS@ModifiedSiO2 coating and the EP@PDMS@ModifiedSiO2@EDTAFMCNs coating had the lowest CaSO4 scaling, at 1.808 mg / cm³, respectively. 2 and 0.544 mg / cm 2 This demonstrates that the EP@PDMS@ModifiedSiO2@EDTAFMCNs superhydrophobic scale inhibitor coating exhibits excellent scale inhibition performance.

[0085] Figure 2 (e) shows the XRD patterns of deposited scale on different coatings. As can be seen from the figure, the scale deposited on the surface of each coating is CaSO42H2O. The (020), (021), (040) and (041) crystal planes of CaSO42H2O are located at 2θ=11.72°, 20.8°, 23.46° and 29.18°, respectively. It can be seen that the 2θ values ​​corresponding to each crystal plane of CaSO42H2O deposited on the surface of the EP@PDMS@ModifiedSiO2@EDTAFMCNs superhydrophobic scale inhibitor coating do not change significantly, but the diffraction peak intensity of each crystal plane is significantly reduced, which effectively inhibits the deposition of scale on the coating surface.

[0086] Figure 2 (f) shows the FTIR spectra of scale deposited on different coating surfaces. As can be seen from the figure, the stretching vibration of SO in CaSO4·2H2O occurs at a wavelength of 1100 cm⁻¹. -1 -1300cm -1 The wavelength is 601cm -1 and 669cm -1 Then corresponding Anti-symmetric bending vibrations were observed only on the surface of the blank substrate and in the deposits formed on the EP@PDMS surface. The EP@PDMS@ModifiedSiO2 coating and the EP@PDMS@ModifiedSiO2@EDTA-FMWCNs coating only exhibited vibrations at a wavelength of 1261 cm⁻¹. -1 and 800cm -1 Symmetrical tensile vibrations of -CH3 and bending and tensile vibrations of Si-O-Si were observed at the site. This indicates that the EP@PDMS@ModifiedSiO2@EDTAFMCNs superhydrophobic scale inhibitor coating has excellent scale inhibition effect on CaSO42H2O.

[0087] Figure 3Images (a)-(b) show SEM images of CaCO3 deposition on the blank substrate surface and the EP@PDMS coating surface. It can be seen that CaCO3 is uniformly distributed on the coating surface, mainly consisting of large blocky and spherical crystals. Simultaneously, a large number of fine needle-like crystals densely grow on the blocky crystals. These are typical calcite, aragonite, and spheroidal structures, indicating that although the EP@PDMS coating can inhibit CaCO3 formation and induce a large amount of CaCO3 to grow into metastable aragonite and spheroidal structures, its scale inhibition effect is not significant. The addition of modified vapor-phase nano-SiO2 enriched the coating roughness and provided superhydrophobic properties. Although a large amount of regularly shaped calcite still accumulated on the coating surface, its distribution was uneven. This is because the air film formed on the coating surface blocked the deposition of calcium carbonate. With time and water flow disturbance, the air film gradually broke, exposing the coating surface structure and providing sites for CaCO3 nucleation and growth. After adding modified carbon nanotubes, it was clearly observed that only a very small amount of CaCO3 crystals were deposited on the coating surface, and the hierarchical micro-nanopapillary structure of the coating surface remained intact. This is because the air film formed by the hierarchical micro-nanopapillary structure of the coating surface constitutes the first layer of scale inhibition barrier, preventing CaCO3 from depositing on the coating surface. Secondly, the oil layer formed by polydimethylsiloxane (PDMS) lubricant constitutes the second layer of scale inhibition barrier, inhibiting anisotropic nucleation of scale on the coating surface and preventing scale deposition. When the air film and oil film are damaged, the EDTA loaded on the modified carbon nanotubes is gradually released and reacts with CaCO3 in the solution. 2+ Chelation occurs, forming a third scale barrier that further prevents CaCO3 from depositing on the coating surface.

[0088] Figure 4 Figures (a)-(b) show SEM images of CaSO4·2H2O deposited on the blank substrate surface and the EP@PDMS coating surface. At this point, the CaSO4·2H2O crystals are in an aggregated and stacked state, with interwoven crystals and a small amount of fine particles attached. The EP@PDMS coating also shows obvious damage and corrosion. Figure 14(cd) shows SEM images of CaSO4·2H2O deposited on the EP@PDMS@ModifiedSiO2 coating and the EP@PDMS@ModifiedSiO2@EDTA-FMWCNTs coating. Clearly, the EP@PDMS@ModifiedSiO2@EDTA-FMWCNTs coating has stronger scale inhibition capability, with the lowest CaSO4·2H2O crystal distribution density. The crystals are sparsely and independently distributed, with only a small amount of crystals deposited on the coating surface. Furthermore, most of the coating surface retains a hierarchical micro / nanopapillary structure, indicating that the coating not only has excellent scale inhibition capability but also a certain degree of corrosion resistance.

[0089] In summary, the scale inhibition mechanism of the coating is as follows:Figure 5 As shown: First, modified hydrophobic nano-vaporous SiO2 constructs a hierarchical micro / nanopapillary structure on the coating surface, forming an air layer that prevents scale deposition. Second, this micro / nanopapillary structure facilitates the penetration of polydimethylsiloxane (PDMS) lubricant into the coating, forming a stable oil layer that effectively inhibits anisotropic nucleation of scale on the coating surface, preventing scale deposition. To further enhance the scale inhibition properties of the coating, the chelating agent EDTA is loaded onto the FMWCNTs. When the air layer and oil layer are damaged by corrosive media in the environment, the EDTA loaded on the FMWCNTs is released and reacts with Ca in the solution. 2+ The formation of interfacial chelation further enhances the scale inhibition performance of the coating.

[0090] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. A superhydrophobic composite coating with a triple scale-inhibiting structure, characterized in that, It is made from the following raw materials in parts by weight: 80-120 parts epoxy resin, 15-30 parts polydimethylsiloxane, 3-8 parts modified hydrophobic nano silica, and 2-10 parts acidified multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid.

2. The superhydrophobic composite coating with a triple scale-inhibiting structure according to claim 1, characterized in that, The modified hydrophobic nano-silica constructs a micro-nano rough structure on the coating surface and forms an air layer; the polydimethylsiloxane penetrates into the micro-nano rough structure to form an oil layer; and the acidified multi-walled carbon nanotubes loaded with chelating agents continuously release chelating agents when the air layer and oil layer are damaged, chelating with scale-forming ions to form a scale-inhibiting barrier.

3. The superhydrophobic composite coating with a triple scale-inhibiting structure according to claim 1, characterized in that, The coating has a static water contact angle greater than 150° and a roll-off angle less than 10°; after being tested in a supersaturated calcium carbonate solution at 50-70°C for 110-130 hours, the scale buildup per unit area is less than 0.4 mg / cm².

4. A method for preparing a superhydrophobic composite coating with a triple scale-inhibiting structure, characterized in that, The superhydrophobic composite coating with a triple scale-inhibiting structure as described in any one of claims 1-3 comprises the following steps: S1. Preparation of modified hydrophobic nano silica: Disperse fumed nano silica in an organic solvent, add alkyl chlorosilane to carry out hydrophobic modification reaction, and after the reaction is completed, separate, wash and dry to obtain modified hydrophobic nano silica; S2. Preparation of acidified multi-walled carbon nanotubes loaded with chelating agents: Acidification treatment is performed on multi-walled carbon nanotubes to obtain acidified multi-walled carbon nanotubes; then the acidified multi-walled carbon nanotubes are immersed in a chelating agent solution, loaded with chelating agents, separated and dried to obtain acidified multi-walled carbon nanotubes loaded with chelating agents. S3. Preparation and coating: The modified hydrophobic nano-silica obtained in S1, the acidified multi-walled carbon nanotubes loaded with chelating agents obtained in S2, epoxy resin, polydimethylsiloxane and corresponding curing agents are dispersed in a solvent and mixed evenly to form a coating suspension; the suspension is coated on the surface of the pretreated substrate, and after curing, the superhydrophobic composite coating is obtained.

5. The method for preparing a superhydrophobic composite coating with a triple scale-inhibiting structure according to claim 4, characterized in that, In step S1, the hydrophobic modification reaction is carried out under the following conditions: stirring at 65-85°C for 3-5 hours; the alkylchlorosilane is dimethyloctadecylchlorosilane.

6. The method for preparing a superhydrophobic composite coating with a triple scale-inhibiting structure according to claim 4, characterized in that, Step S2 includes: S21. Acidification treatment: Place multi-walled carbon nanotubes in a mixed acid of concentrated sulfuric acid and concentrated nitric acid with a volume ratio of (2.5:1) to (3.5:1), stir at 65-85℃ for 5-9 hours, then wash until neutral and dry to obtain acidified multi-walled carbon nanotubes. S22, Loading chelating agent: The acidified multi-walled carbon nanotubes are immersed in an aqueous solution of 0.05-0.15 mol / L ethylenediaminetetraacetic acid, stirred at room temperature for 18-30 hours, separated and dried to obtain acidified multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid.

7. The method for preparing a superhydrophobic composite coating with a triple scale-inhibiting structure according to claim 4, characterized in that, In step S3, the pretreatment involves mechanically polishing the substrate surface with 400-800 grit sandpaper, followed by ultrasonic cleaning with anhydrous ethanol and acetone in sequence, with each ultrasonic cleaning session lasting 20-40 minutes.

8. The method for preparing a superhydrophobic composite coating with a triple scale-inhibiting structure according to claim 4, characterized in that, Step S3 includes: S31. Mixing and Dispersion: Add the modified hydrophobic nano-silica obtained in S1 and the acidified multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid obtained in S2 to acetone solvent, first ultrasonically disperse for 20-40 minutes, then magnetically stir for 20-40 minutes; then add epoxy resin, polydimethylsiloxane and its corresponding curing agent, and continue magnetically stirring for 1-2 hours to obtain a uniform coating suspension; S32. Coating and curing: The coating suspension is applied to the pretreated substrate surface by spraying at a pressure of 0.3-0.7 MPa and a distance of 10-20 cm. The coated substrate is then cured at 70-90°C for 1.5-2.5 hours.

9. The method for preparing a superhydrophobic composite coating with a triple scale-inhibiting structure according to claim 4, characterized in that, In step S3, a dispersant comprising 0.1-1% of the total solid mass of the coating is added, wherein the dispersant is added together with the modified hydrophobic nano-silica and the acidified multi-walled carbon nanotubes loaded with ethylenediaminetetraacetic acid in acetone solvent for ultrasonic dispersion.