A nanofluid coolant and its preparation method
By using covalent bonds in modified spherical carbon particles and a polysiloxane shell design, the stability and corrosion resistance of nanofluid coolant under high temperature and high shear conditions were solved, achieving efficient heat dissipation for data centers.
Patent Information
- Application Number
- CN202611273105.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-10
AI Technical Summary
Existing nanofluid coolants cannot simultaneously achieve high thermal conductivity, long-term dispersion stability, low viscosity growth, and corrosion resistance under high-temperature, long-term, and high-shear cycling conditions, thus limiting their application in the field of data center liquid cooling.
Modified spherical carbon particles are used as thermally conductive fillers, which are connected by CO-Si, CSC and Si-O-Si covalent bonds to form a stable nanofluid coolant. Carboxylated polysiloxane brushes provide electrostatic repulsion and steric hindrance barriers to inhibit particle agglomeration, and the polysiloxane shell shields against electrochemical corrosion.
Modified nanofluid coolant maintains stable dispersion at high temperatures, extending its service life, preventing microchannel blockage, reducing corrosion risk, and improving coolant reliability.
Abstract
Description
Technical Field
[0001] This invention relates to the field of coolant preparation technology, specifically to a nanofluid coolant and its preparation method. Background Technology
[0002] With the rapid development of cloud computing, big data, and artificial intelligence technologies, the integration and power density of data center servers continue to rise. Currently, the heat flux density of high-end CPU and GPU chips has exceeded 100W / cm², and traditional air cooling methods are approaching their heat transfer limits, failing to meet the heat dissipation requirements of high-power-density servers. Liquid cooling technology, especially direct-contact liquid cooling and cold-plate liquid cooling, has become the inevitable choice for heat dissipation in high-density data centers due to its heat exchange capacity far exceeding that of air cooling.
[0003] Nanofluids refer to colloidal suspensions formed by stably suspending nanoscale solid particles in a base fluid. Adding nanoparticles with high thermal conductivity can significantly improve the equivalent thermal conductivity of the base fluid, thereby enhancing the system's heat dissipation capacity. However, existing nanofluid coolant technologies cannot simultaneously achieve high thermal conductivity, long-term dispersion stability, low viscosity growth, strong corrosion resistance, and anti-clogging properties under the high-temperature, long-cycle, and high-shear cyclic operation conditions required by servers. These performance indicators are sharply contradictory, severely restricting the practical application of nanofluids in data center liquid cooling. Summary of the Invention
[0004] The purpose of this invention is to provide a nanofluid coolant and its preparation method, which solves the problems of easy agglomeration, poor stability, and blockage of microchannels in current carbon-based coolants.
[0005] The objective of this invention can be achieved through the following technical solutions: A method for preparing a nanofluid coolant specifically includes the following steps: Step A1: Dissolve lithium dimethylvinylsilane in tetrahydrofuran, purge with nitrogen, and stir while adding tetramethylcyclotetrasiloxane and hexamethylcyclotrisiloxane at 0°C and a speed of 200-300 r / min. Heat to 25-30°C and react for 6-8 h. Then add trimethylchlorosilane and react for 1-1.5 h to obtain alkenyl polysiloxane. Step A2: Disperse the modified spherical carbon in toluene, purge with nitrogen, and stir while adding alkenyl polysiloxane and 2,2-dimethoxy-2-phenylacetophenone under conditions of 120-150 r / min, 20-25℃, and 365nm ultraviolet light irradiation, to obtain pretreated thermally conductive particles; Step A3: Disperse the pretreated thermally conductive particles in toluene, purge with nitrogen, and stir at a speed of 200-300 r / min and a temperature of 65-75℃, adding acrylic acid, p-hydroxyanisole and castor catalyst, and react for 6-8 hours to obtain modified thermally conductive particles. Step A4: Weigh the following raw materials by weight: 40-60 parts ethylene glycol, 40-60 parts deionized water, 0.1-0.5 parts modified thermally conductive particles and 0.1-0.3 parts benzotriazole. Mix the raw materials evenly and add triethanolamine until the pH value is 8-8.5 to obtain the nanofluid coolant.
[0006] Furthermore, the molar ratio of lithium dimethylvinylsilyl alcohol, tetramethylcyclotetrasiloxane, hexamethylcyclotrisiloxane and trimethylchlorosilane in step A1 is 1:3:3:1.2.
[0007] Furthermore, in step A2, the mass ratio of the modified spherical carbon to the alkenyl polysiloxane is 1:1, and the amount of 2,2-dimethoxy-2-phenylacetophenone used is 1.5% of the mass of the alkenyl polysiloxane.
[0008] Furthermore, in step A3, the molar ratio of Si-H bonds on the pretreated thermally conductive particles to acrylic acid is 1:1.2, the amount of p-hydroxybenzyl is 0.1% of the mass of acrylic acid, and the amount of cassette catalyst is 0.5% of the mass of acrylic acid.
[0009] Furthermore, the modified spherical carbon is prepared by the following steps: Step B1: Dissolve ferric nitrate in deionized water, stir and add nano-alumina at a speed of 600-800 r / min and a temperature of 25-30℃, stir for 1-1.5 h, filter to remove filtrate, place in a muffle furnace, calcine at a temperature of 500-550℃ for 1-1.5 h to obtain catalyst, place catalyst in a tube furnace, and react with methane, hydrogen and argon at a temperature of 900-950℃ for 1.5-2 h to obtain precursor; Step B2: Mix the precursor and dilute hydrochloric acid, and stir for 2-3 hours at a speed of 200-300 r / min and a temperature of 50-60℃. Filter to remove the filtrate, place the substrate in hydrofluoric acid, and stir for 20-24 hours at a speed of 150-200 r / min and a temperature of 20-25℃ to obtain spherical carbon. Mix the spherical carbon, concentrated nitric acid, and concentrated sulfuric acid, and react for 6-8 hours at a speed of 200-300 r / min and a temperature of 90-100℃ to obtain functionalized spherical carbon. Step B3: Mix ethanol and deionized water, stir and add vinyltriethoxysilane at a speed of 150-200 r / min, a temperature of 20-25℃, and a pH of 4.5-5.5, and stir for 30-40 min. Add functionalized spherical carbon, heat to 70-80℃, and react for 2-4 h to obtain double-bonded spherical carbon. Disperse the double-bonded spherical carbon in toluene, purge with nitrogen, and stir and add 3-mercaptopropyltrimethoxysilane and 2,2-dimethoxy-2-phenylacetophenone at a speed of 120-150 r / min, a temperature of 20-25℃, and 365 nm ultraviolet light irradiation to obtain pretreated spherical carbon. Step B4: Disperse the pretreated spherical carbon in ethanol, add tetraethoxysilane, methyltriethoxysilane, mercaptopropylmethyldimethoxysilane and deionized water, purge with nitrogen, and react for 4-6 hours at a rotation speed of 150-200 r / min, a temperature of 60-70℃ and a pH of 4-5. Then let it stand and age for 3-5 hours to obtain modified spherical carbon.
[0010] Furthermore, in step B1, the ratio of ferric nitrate, deionized water, and nano-alumina is 3.6g:30mL:10g, the flow rate of methane is 30sccm, the flow rate of hydrogen is 15sccm, and the flow rate of argon is 150sccm.
[0011] Furthermore, in step B2, the ratio of the precursor, dilute hydrochloric acid, and hydrofluoric acid is 1g:20mL:20mL, and the ratio of spherical carbon, concentrated nitric acid, and concentrated sulfuric acid is 1g:10mL:30mL.
[0012] Furthermore, in step B3, the ratio of ethanol, deionized water, vinyltriethoxysilane, and functionalized spherical carbon is 45 mL:5 mL:2 mL:1 g, the ratio of double-bonded spherical carbon, toluene, and 3-mercaptopropyltrimethoxysilane is 1 g:40 mL:2 mL, and the amount of 2,2-dimethoxy-2-phenylacetophenone is 1% of the mass of 3-mercaptopropyltrimethoxysilane.
[0013] Furthermore, the ratio of the amount of pretreated spherical carbon, ethanol, tetraethoxysilane, methyltriethoxysilane, mercaptopropylmethyldimethoxysilane and deionized water used in step B4 is 1g:100mL:2mL:1.5mL:1mL:3mL.
[0014] The beneficial effects of this invention are as follows: This application discloses a nanofluid coolant comprising the following raw materials: ethylene glycol, deionized water, modified thermally conductive particles, and benzotriazole. The modified thermally conductive particles are formed using dimethylvinylsilane lithium as an initiator and tetramethylcyclotetrasiloxane and hexamethylcyclotrisiloxane as polymer monomers, forming a polysiloxane with a double bond at one end and a lithium silanolate at the other end, and a Si-H bond in the side chain. Trimethylchlorosilane is then added, causing the Si-Cl bond on the trimethylchlorosilane to react with the lithium silanolate to obtain an alkenyl polysiloxane. Modified spherical carbon and alkenyl polysiloxane are reacted by ultraviolet light, causing the mercapto groups on the modified spherical carbon to react with the double bonds on the alkenyl polysiloxane to obtain pretreated thermally conductive particles. The pretreated thermally conductive particles are reacted with acrylic acid, causing the Si-H bonds on the pretreated thermally conductive particles to react with the double bonds on the acrylic acid to obtain modified thermally conductive particles.
[0015] Modified spherical carbon is prepared using ferric nitrate and nano-alumina as raw materials. Ferric nitrate is impregnated onto nano-alumina, then calcined and decomposed into ferric oxide, which is anchored on the alumina surface to obtain a catalyst. Methane undergoes cracking on the surface of iron particles, dissolving carbon atoms into the iron particles. After reaching supersaturation, carbon atoms precipitate from the particle surface in the form of a graphite layer, forming a spherical carbon shell to obtain a precursor. The precursor is dissolved in dilute hydrochloric acid to remove most of the iron catalyst core, leaving a hollow carbon shell. The alumina support is then removed by dissolving in hydrofluoric acid to obtain a pure carbon shell, thus obtaining spherical carbon. The spherical carbon is then treated with concentrated nitric acid and concentrated sulfuric acid. Functionalized spherical carbon is prepared by grafting hydroxyl groups onto its surface. The functionalized spherical carbon is then treated with vinyltriethoxysilane to graft double bonds onto its surface, resulting in double-bonded spherical carbon. The double-bonded spherical carbon is then reacted with 3-mercaptopropyltrimethoxysilane to react the double bonds on the double-bonded spherical carbon with the mercapto groups on the 3-mercaptopropyltrimethoxysilane, resulting in pretreated spherical carbon. The pretreated spherical carbon is then treated with tetraethoxysilane, methyltriethoxysilane, and mercaptopropylmethyldimethoxysilane to coat its surface with a polysiloxane shell containing mercapto groups, resulting in modified spherical carbon.
[0016] The modified thermally conductive particles are connected by stable CO-Si, CSC, and Si-O-Si covalent bonds, which can resist high shear forces and thermal shocks during long-term cycling, thereby extending the service life of the nanofluid coolant. The surface is grafted with carboxyl polysiloxane brushes, and the carboxyl groups ionize into carboxylate ions, providing strong electrostatic repulsion. At the same time, the highly extended polysiloxane segments provide a steric barrier, which can effectively overcome the van der Waals forces between particles, making the modified thermally conductive particles less prone to agglomeration. They can maintain long-term stable dispersion at high temperatures. The dense polysiloxane shell can effectively shield the carbon core from direct contact with metal ions, inhibit possible electrochemical corrosion reactions, and ensure the long-term reliability of the coolant. Detailed Implementation
[0017] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0018] Example 1: A method for preparing a nanofluid coolant, specifically including the following steps: Step A1: Lithium dimethylvinylsilane was dissolved in tetrahydrofuran and protected with nitrogen. Under the conditions of 200 r / min and 0℃, tetramethylcyclotetrasiloxane and hexamethylcyclotrisiloxane were added while stirring. The temperature was raised to 25℃ and the reaction was carried out for 6 h. Then, trimethylchlorosilane was added and the reaction was carried out for 1 h to obtain alkenyl polysiloxane. Step A2: The modified spherical carbon was dispersed in toluene, and nitrogen gas was introduced for protection. Under the conditions of 120 r / min rotation speed, 20℃ temperature and 365nm ultraviolet light irradiation, alkenyl polysiloxane and 2,2-dimethoxy-2-phenylacetophenone were added and stirred for 1 h to obtain pretreated thermally conductive particles. Step A3: Disperse the pretreated thermally conductive particles in toluene, purge with nitrogen, and stir at a speed of 200 r / min and a temperature of 65°C. Add acrylic acid, p-hydroxyanisole and castor catalyst and react for 6 h to obtain modified thermally conductive particles. Step A4: Weigh the following raw materials in parts by weight: 40 parts ethylene glycol, 40 parts deionized water, 0.1 parts modified thermally conductive particles and 0.1 parts benzotriazole. Mix the raw materials evenly and add triethanolamine until the pH value is 8 to obtain the nanofluid coolant.
[0019] The molar ratio of lithium dimethylvinylsilyl alcohol, tetramethylcyclotetrasiloxane, hexamethylcyclotrisiloxane and trimethylchlorosilane in step A1 is 1:3:3:1.2.
[0020] The mass ratio of the modified spherical carbon to the alkenyl polysiloxane in step A2 is 1:1, and the amount of 2,2-dimethoxy-2-phenylacetophenone used is 1.5% of the mass of the alkenyl polysiloxane.
[0021] The molar ratio of Si-H bonds on the pretreated thermally conductive particles described in step A3 to acrylic acid is 1:1.2, the amount of p-hydroxybenzyl is 0.1% of the mass of acrylic acid, and the amount of cassette catalyst is 0.5% of the mass of acrylic acid.
[0022] The modified spherical carbon is prepared by the following steps: Step B1: Dissolve ferric nitrate in deionized water, stir and add nano-alumina at 600 r / min and 25°C, stir for 1 h, filter to remove filtrate, place in a muffle furnace, calcine at 500°C for 1 h to obtain catalyst, place catalyst in a tube furnace, introduce methane, hydrogen and argon at 900°C, react for 1.5 h to obtain precursor; Step B2: Mix the precursor and dilute hydrochloric acid, stir for 2 hours at 200 r / min and 50°C, filter to remove the filtrate, place the substrate in hydrofluoric acid, stir for 20 hours at 150 r / min and 20°C to obtain spherical carbon, mix the spherical carbon, concentrated nitric acid and concentrated sulfuric acid, react for 6 hours at 200 r / min and 90°C to obtain functionalized spherical carbon; Step B3: Ethanol and deionized water were mixed and stirred at 150 r / min, 20 °C, and pH 4.5. Vinyltriethoxysilane was added and stirred for 30 min. Functionalized spherical carbon was added, and the temperature was raised to 70 °C for 2 h to obtain double-bonded spherical carbon. The double-bonded spherical carbon was dispersed in toluene and protected with nitrogen. At 120 r / min, 20 °C, and 365 nm ultraviolet light irradiation, 3-mercaptopropyltrimethoxysilane and 2,2-dimethoxy-2-phenylacetophenone were added and stirred for 1 h to obtain pretreated spherical carbon. Step B4: Disperse the pretreated spherical carbon in ethanol, add tetraethoxysilane, methyltriethoxysilane, mercaptopropylmethyldimethoxysilane and deionized water, purge with nitrogen, and react for 4 hours at a speed of 150 r / min, a temperature of 60℃ and a pH of 4. Then let it stand and age for 3 hours to obtain modified spherical carbon.
[0023] In step B1, the ratio of ferric nitrate, deionized water, and nano-alumina is 3.6g:30mL:10g, the flow rate of methane is 30sccm, the flow rate of hydrogen is 15sccm, and the flow rate of argon is 150sccm.
[0024] The ratio of the precursor, dilute hydrochloric acid, and hydrofluoric acid used in step B2 is 1g:20mL:20mL, and the ratio of spherical carbon, concentrated nitric acid, and concentrated sulfuric acid is 1g:10mL:30mL.
[0025] In step B3, the ratio of ethanol, deionized water, vinyltriethoxysilane, and functionalized spherical carbon is 45 mL:5 mL:2 mL:1 g; the ratio of double-bonded spherical carbon, toluene, and 3-mercaptopropyltrimethoxysilane is 1 g:40 mL:2 mL; and the amount of 2,2-dimethoxy-2-phenylacetophenone is 1% of the mass of 3-mercaptopropyltrimethoxysilane.
[0026] The ratio of the amount of pretreated spherical carbon, ethanol, tetraethoxysilane, methyltriethoxysilane, mercaptopropylmethyldimethoxysilane and deionized water in step B4 is 1g:100mL:2mL:1.5mL:1mL:3mL.
[0027] Example 2, a method for preparing a nanofluid coolant, specifically includes the following steps: Step A1: Lithium dimethylvinylsilane was dissolved in tetrahydrofuran under nitrogen protection. The mixture was stirred at 200 r / min and 0 °C, and tetramethylcyclotetrasiloxane and hexamethylcyclotrisiloxane were added. The mixture was heated to 30 °C and reacted for 7 h. Then trimethylchlorosilane was added and reacted for 1.3 h to obtain alkenyl polysiloxane. Step A2: The modified spherical carbon was dispersed in toluene, and nitrogen gas was introduced for protection. Under the conditions of 120 r / min rotation speed, 25℃ temperature and 365nm ultraviolet light irradiation, alkenyl polysiloxane and 2,2-dimethoxy-2-phenylacetophenone were added and stirred for 1.3 h to obtain pretreated thermally conductive particles. Step A3: Disperse the pretreated thermally conductive particles in toluene, purge with nitrogen, and stir at a speed of 200 r / min and a temperature of 70°C. Add acrylic acid, p-hydroxyanisole and caster catalyst and react for 7 h to obtain modified thermally conductive particles. Step A4: Weigh the following raw materials in parts by weight: 50 parts ethylene glycol, 50 parts deionized water, 0.3 parts modified thermally conductive particles and 0.2 parts benzotriazole. Mix the raw materials evenly and add triethanolamine until the pH value is 8.5 to obtain the nanofluid coolant.
[0028] The molar ratio of lithium dimethylvinylsilyl alcohol, tetramethylcyclotetrasiloxane, hexamethylcyclotrisiloxane and trimethylchlorosilane in step A1 is 1:3:3:1.2.
[0029] The mass ratio of the modified spherical carbon to the alkenyl polysiloxane in step A2 is 1:1, and the amount of 2,2-dimethoxy-2-phenylacetophenone used is 1.5% of the mass of the alkenyl polysiloxane.
[0030] The molar ratio of Si-H bonds on the pretreated thermally conductive particles described in step A3 to acrylic acid is 1:1.2, the amount of p-hydroxybenzyl is 0.1% of the mass of acrylic acid, and the amount of cassette catalyst is 0.5% of the mass of acrylic acid.
[0031] The modified spherical carbon is prepared by the following steps: Step B1: Dissolve ferric nitrate in deionized water, stir and add nano-alumina at 800 r / min and 25℃, stir for 1.3 h, filter to remove filtrate, place in a muffle furnace, calcine at 530℃ for 1.5 h to obtain catalyst, place catalyst in a tube furnace, introduce methane, hydrogen and argon at 930℃, react for 1.8 h to obtain precursor; Step B2: Mix the precursor and dilute hydrochloric acid, stir at 300 r / min and 55°C for 2.5 h, filter to remove the filtrate, place the substrate in hydrofluoric acid, stir at 150 r / min and 25°C for 22 h to obtain spherical carbon, mix the spherical carbon, concentrated nitric acid and concentrated sulfuric acid, react at 300 r / min and 95°C for 7 h to obtain functionalized spherical carbon; Step B3: Ethanol and deionized water were mixed and stirred at 200 r / min, 23 °C, and pH 5. Vinyltriethoxysilane was added and stirred for 35 min. Functionalized spherical carbon was added, and the temperature was raised to 75 °C for 3 h to obtain double-bonded spherical carbon. The double-bonded spherical carbon was dispersed in toluene and protected with nitrogen. Under the conditions of 120 r / min, 25 °C, and 365 nm ultraviolet light irradiation, 3-mercaptopropyltrimethoxysilane and 2,2-dimethoxy-2-phenylacetophenone were added and stirred for 1.3 h to obtain pretreated spherical carbon. Step B4: Disperse the pretreated spherical carbon in ethanol, add tetraethoxysilane, methyltriethoxysilane, mercaptopropylmethyldimethoxysilane and deionized water, purge with nitrogen, and react for 5 hours at a speed of 200 r / min, a temperature of 65℃ and a pH of 4. Then let it stand for 4 hours to obtain modified spherical carbon.
[0032] In step B1, the ratio of ferric nitrate, deionized water, and nano-alumina is 3.6g:30mL:10g, the flow rate of methane is 30sccm, the flow rate of hydrogen is 15sccm, and the flow rate of argon is 150sccm.
[0033] The ratio of the precursor, dilute hydrochloric acid, and hydrofluoric acid used in step B2 is 1g:20mL:20mL, and the ratio of spherical carbon, concentrated nitric acid, and concentrated sulfuric acid is 1g:10mL:30mL.
[0034] In step B3, the ratio of ethanol, deionized water, vinyltriethoxysilane, and functionalized spherical carbon is 45 mL:5 mL:2 mL:1 g; the ratio of double-bonded spherical carbon, toluene, and 3-mercaptopropyltrimethoxysilane is 1 g:40 mL:2 mL; and the amount of 2,2-dimethoxy-2-phenylacetophenone is 1% of the mass of 3-mercaptopropyltrimethoxysilane.
[0035] The ratio of the amount of pretreated spherical carbon, ethanol, tetraethoxysilane, methyltriethoxysilane, mercaptopropylmethyldimethoxysilane and deionized water in step B4 is 1g:100mL:2mL:1.5mL:1mL:3mL.
[0036] Example 3, a method for preparing a nanofluid coolant, specifically includes the following steps: Step A1: Lithium dimethylvinylsilane was dissolved in tetrahydrofuran under nitrogen protection. The mixture was stirred at 300 r / min and 0 °C, and tetramethylcyclotetrasiloxane and hexamethylcyclotrisiloxane were added. The mixture was heated to 30 °C and reacted for 8 h. Then trimethylchlorosilane was added and reacted for 1.5 h to obtain alkenyl polysiloxane. Step A2: The modified spherical carbon was dispersed in toluene, and nitrogen gas was introduced for protection. Under the conditions of 150 r / min rotation speed, 25℃ temperature and 365nm ultraviolet light irradiation, alkenyl polysiloxane and 2,2-dimethoxy-2-phenylacetophenone were added and stirred for 1.5 h to obtain pretreated thermally conductive particles. Step A3: Disperse the pretreated thermally conductive particles in toluene, purge with nitrogen, and stir at 300 r / min and 75°C. Add acrylic acid, p-hydroxyanisole and castor catalyst and react for 8 h to obtain modified thermally conductive particles. Step A4: Weigh the following raw materials in parts by weight: 60 parts ethylene glycol, 60 parts deionized water, 0.5 parts modified thermally conductive particles and 0.3 parts benzotriazole. Mix the raw materials evenly and add triethanolamine until the pH value is 8.5 to obtain the nanofluid coolant.
[0037] The molar ratio of lithium dimethylvinylsilyl alcohol, tetramethylcyclotetrasiloxane, hexamethylcyclotrisiloxane and trimethylchlorosilane in step A1 is 1:3:3:1.2.
[0038] The mass ratio of the modified spherical carbon to the alkenyl polysiloxane in step A2 is 1:1, and the amount of 2,2-dimethoxy-2-phenylacetophenone used is 1.5% of the mass of the alkenyl polysiloxane.
[0039] The molar ratio of Si-H bonds on the pretreated thermally conductive particles described in step A3 to acrylic acid is 1:1.2, the amount of p-hydroxybenzyl is 0.1% of the mass of acrylic acid, and the amount of cassette catalyst is 0.5% of the mass of acrylic acid.
[0040] The modified spherical carbon is prepared by the following steps: Step B1: Dissolve ferric nitrate in deionized water, stir and add nano-alumina at 800 r / min and 30℃, stir for 1.5 h, filter to remove filtrate, place in a muffle furnace, calcine at 550℃ for 1.5 h to obtain catalyst, place catalyst in a tube furnace, introduce methane, hydrogen and argon at 950℃, react for 2 h to obtain precursor; Step B2: Mix the precursor and dilute hydrochloric acid, stir for 3 hours at 300 r / min and 60°C, filter to remove the filtrate, place the substrate in hydrofluoric acid, stir for 24 hours at 200 r / min and 25°C to obtain spherical carbon, mix the spherical carbon, concentrated nitric acid and concentrated sulfuric acid, react for 8 hours at 300 r / min and 100°C to obtain functionalized spherical carbon; Step B3: Ethanol and deionized water were mixed and stirred at 200 r / min, 25 °C, and pH 5.5. Vinyltriethoxysilane was added and stirred for 40 min. Functionalized spherical carbon was added, and the temperature was raised to 80 °C for 4 h to obtain double-bonded spherical carbon. The double-bonded spherical carbon was dispersed in toluene and protected with nitrogen. Under 150 r / min, 25 °C, and 365 nm ultraviolet light irradiation, 3-mercaptopropyltrimethoxysilane and 2,2-dimethoxy-2-phenylacetophenone were added and stirred for 1.5 h to obtain pretreated spherical carbon. Step B4: Disperse the pretreated spherical carbon in ethanol, add tetraethoxysilane, methyltriethoxysilane, mercaptopropylmethyldimethoxysilane and deionized water, purge with nitrogen, and react for 6 hours at a speed of 200 r / min, a temperature of 70℃ and a pH of 5. Then let it stand for 5 hours to obtain modified spherical carbon.
[0041] In step B1, the ratio of ferric nitrate, deionized water, and nano-alumina is 3.6g:30mL:10g, the flow rate of methane is 30sccm, the flow rate of hydrogen is 15sccm, and the flow rate of argon is 150sccm.
[0042] The ratio of the precursor, dilute hydrochloric acid, and hydrofluoric acid used in step B2 is 1g:20mL:20mL, and the ratio of spherical carbon, concentrated nitric acid, and concentrated sulfuric acid is 1g:10mL:30mL.
[0043] In step B3, the ratio of ethanol, deionized water, vinyltriethoxysilane, and functionalized spherical carbon is 45 mL:5 mL:2 mL:1 g; the ratio of double-bonded spherical carbon, toluene, and 3-mercaptopropyltrimethoxysilane is 1 g:40 mL:2 mL; and the amount of 2,2-dimethoxy-2-phenylacetophenone is 1% of the mass of 3-mercaptopropyltrimethoxysilane.
[0044] The ratio of the amount of pretreated spherical carbon, ethanol, tetraethoxysilane, methyltriethoxysilane, mercaptopropylmethyldimethoxysilane and deionized water in step B4 is 1g:100mL:2mL:1.5mL:1mL:3mL.
[0045] Comparative Example 1: Compared with Example 1, this comparative example uses lithium dimethylvinylsilane dissolved in tetrahydrofuran, under nitrogen protection, stirred at 200 r / min and 0°C, and hexamethylcyclotrisiloxane is added. The temperature is raised to 25°C and reacted for 6 hours. Then, trimethylchlorosilane is added and reacted for 1 hour. The product obtained is used as the modified thermally conductive particles instead of the alkenyl polysiloxane particles. The remaining steps are the same.
[0046] Comparative Example 2: This comparative example uses carbon nanotubes instead of spherical carbon, but the other steps are the same as in Example 1.
[0047] Comparative Example 3: Compared with Example 1, this comparative example uses pretreated spherical carbon dispersed in ethanol, with the addition of tetraethoxysilane, methyltriethoxysilane and deionized water, under nitrogen protection, and reacted for 4 hours at a rotation speed of 150 r / min, a temperature of 60 °C and a pH of 4. After standing and aging for 3 hours, the product obtained replaces the modified thermally conductive particles, and the remaining steps are the same.
[0048] The coolant samples prepared in Examples 1-3 and Comparative Examples 1-3 were placed at a constant temperature of 25°C and kept static for 90 days. The initial absorbance and the absorbance after 90 days of static storage were measured, and the concentration retention rate was calculated. The coolant samples were placed in an oven at 80°C and aged continuously for 30 days. The initial absorbance and the absorbance after 30 days of aging were measured, and the concentration retention rate was calculated. Copper and aluminum sheets were respectively immersed in the coolant samples and placed in a constant temperature chamber at 88°C for 14 days. The corrosion rate was calculated. The copper and aluminum sheets were used as working electrodes, the reference electrode was a saturated calomel electrode, and the auxiliary electrode was a platinum sheet. The three electrodes were connected to an electrochemical workstation. When the potential... Fluctuations were less than 2 mV / min. Open circuit potential values were recorded, scanning from -250 mV to +250 mV at a rate of 0.166 mV / s, with one data point collected every 1 mV to detect the chemical corrosion rate. The simulated cold plate, pump, and storage tank were connected in a closed loop using pipelines. Differential pressure sensors and flow meters were installed at the inlet and outlet of the cold plate. The system was first circulated with ethylene glycol-water-based liquid without modified thermal conductive particles for 30 minutes, and the pressure drop at different flow rates was recorded as a baseline. The base liquid was drained, and the nanofluid coolant to be tested was injected at a constant flow rate of 2 L / min. After running for 72 hours, the inside of the microchannels was observed with a microscope. The test results are shown in Table 1 below.
[0049] Table 1 Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Retention rate at room temperature (%) 97.2 96.5 94.8 87.6 26.7 58.5 High temperature concentration retention rate % 94.1 92.3 89.7 83.4 15.3 50.7 Copper corrosion rate (mm / year) 0.05 0.06 0.08 0.12 0.25 0.15 Aluminum corrosion rate (mm / year) 0.08 0.10 0.12 0.18 0.35 0.20 Copper corrosion current density μA / cm² 0.06 0.09 0.11 0.22 0.45 0.35 Aluminum corrosion current density μA / cm² 0.15 0.18 0.22 0.35 0.67 0.55 Congestion No blockage found No blockage found No blockage found Blockage Blockage Blockage As shown in Table 1, this application has good stability while providing cooling effect, and it is not easy to corrode the server and will not cause blockage.
[0050] The above description is merely an example and illustration of the concept of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the concept of the invention or exceed the scope defined in the claims, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing a nanofluid coolant, characterized in that: Specifically, the steps include the following: Step A1: Dissolve lithium dimethylvinylsilane in tetrahydrofuran, purge with nitrogen for protection, stir and add tetramethylcyclotetrasiloxane and hexamethylcyclotrisiloxane, heat and react, then add trimethylchlorosilane to carry out the reaction, and obtain alkenyl polysiloxane. Step A2: The modified spherical carbon is dispersed in toluene, protected by nitrogen gas, stirred under ultraviolet light, and then alkenyl polysiloxane and 2,2-dimethoxy-2-phenylacetophenone are added to carry out the reaction to obtain pretreated thermally conductive particles. Step A3: Disperse the pretreated thermally conductive particles in toluene, purge with nitrogen, stir and add acrylic acid, p-hydroxyanisole and castor catalyst to react and obtain modified thermally conductive particles; Step A4: Weigh the following raw materials by weight: 40-60 parts ethylene glycol, 40-60 parts deionized water, 0.1-0.5 parts modified thermally conductive particles and 0.1-0.3 parts benzotriazole. Mix the raw materials evenly and add triethanolamine until the pH value is 8-8.5 to obtain the nanofluid coolant.
2. The method for preparing the nanofluid coolant according to claim 1, characterized in that: The molar ratio of lithium dimethylvinylsilyl alcohol, tetramethylcyclotetrasiloxane, hexamethylcyclotrisiloxane, and trimethylchlorosilane in step A1 is 1:3:3:1.
2.
3. The method for preparing the nanofluid coolant according to claim 1, characterized in that: The mass ratio of the modified spherical carbon and alkenyl polysiloxane mentioned in step A2 is 1:
1.
4. The method for preparing the nanofluid coolant according to claim 1, characterized in that: The molar ratio of Si-H bonds to acrylic acid on the pretreated thermally conductive particles described in step A3 is 1:1.
2.
5. The method for preparing the nanofluid coolant according to claim 1, characterized in that: The modified spherical carbon is prepared by the following steps: Step B1: Dissolve ferric nitrate in deionized water, stir and add nano alumina, stir and treat, filter to remove filtrate, place in a muffle furnace and calcine to obtain catalyst, place catalyst in tube furnace, introduce methane, hydrogen and argon to react and obtain precursor. Step B2: After mixing and stirring the precursor and dilute hydrochloric acid, filter to remove the filtrate, place the substrate in hydrofluoric acid and stir to obtain spherical carbon, and then mix and react the spherical carbon with concentrated nitric acid and concentrated sulfuric acid to obtain functionalized spherical carbon. Step B3: Mix ethanol and deionized water and stir, then add vinyltriethoxysilane and stir. Add functionalized spherical carbon and heat to react to obtain double-bonded spherical carbon. Disperse the double-bonded spherical carbon in toluene, purge with nitrogen for protection, irradiate with ultraviolet light and stir, then add 3-mercaptopropyltrimethoxysilane and 2,2-dimethoxy-2-phenylacetophenone to react and obtain pretreated spherical carbon. Step B4: Disperse the pretreated spherical carbon in ethanol, add tetraethoxysilane, methyltriethoxysilane, mercaptopropylmethyldimethoxysilane and deionized water, purge with nitrogen for protection, and carry out the reaction to obtain modified spherical carbon.
6. The method for preparing the nanofluid coolant according to claim 5, characterized in that: The ratio of ferric nitrate, deionized water, and nano-alumina used in step B1 is 3.6g:30mL:10g.
7. The method for preparing the nanofluid coolant according to claim 5, characterized in that: The ratio of the precursor, dilute hydrochloric acid, and hydrofluoric acid used in step B2 is 1g:20mL:20mL, and the ratio of spherical carbon, concentrated nitric acid, and concentrated sulfuric acid is 1g:10mL:30mL.
8. The method for preparing the nanofluid coolant according to claim 5, characterized in that: In step B3, the ratio of ethanol, deionized water, vinyltriethoxysilane, and functionalized spherical carbon is 45 mL: 5 mL: 2 mL: 1 g, and the ratio of double-bonded spherical carbon, toluene, and 3-mercaptopropyltrimethoxysilane is 1 g: 40 mL: 2 mL.
9. The method for preparing the nanofluid coolant according to claim 5, characterized in that: The ratio of the pretreated spherical carbon, ethanol, tetraethoxysilane, methyltriethoxysilane, mercaptopropylmethyldimethoxysilane, and deionized water in step B4 is 1g:100mL:2mL:1.5mL:1mL:3mL.
10. A nanofluid coolant, characterized in that: Prepared according to any one of the preparation methods described in claims 1-9.