Preparation method of dual-modal carbon nanotube reinforced aluminum matrix composites

By forming a dual-modal structure of soft and hard regions in aluminum matrix composites, combined with high-energy ball milling and extrusion treatment, the problem of yield strength fluctuation in the prior art was solved, and the simultaneous improvement of strength and plasticity and performance stability were achieved.

CN123063645APending Publication Date: 2026-11-10INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611147620.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-30
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The overall yield strength of existing bimodal carbon nanotube reinforced aluminum matrix composites fluctuates significantly with changes in extrusion ratio, resulting in unstable performance and hindering their engineering applications.

Method used

A dual-modal microstructure with soft and hard regions is formed by high-energy ball milling. The soft region does not contain carbon nanotubes, while the hard region contains uniformly dispersed carbon nanotubes. By combining extrusion, solution treatment and aging treatment, the grain size and composition distribution of the soft and hard regions are controlled to form a clear interface and reduce the sensitivity of yield strength to extrusion ratio.

Benefits of technology

The overall yield strength stability and plasticity of dual-modal carbon nanotube reinforced aluminum matrix composites were improved, the sensitivity to extrusion ratio changes was reduced, and the consistency and reliability of material properties were ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063645A_ABST
    Figure CN123063645A_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing a bimodal carbon nanotube-reinforced aluminum matrix composite material, comprising: 1) mixing carbon nanotube powder with aluminum alloy powder and performing a first high-energy ball milling treatment to obtain carbon nanotube-reinforced aluminum matrix composite material powder; 2) adding aluminum alloy powder and performing a second high-energy ball milling treatment to obtain bimodal composite material powder; 3) performing sintering treatment to obtain the bimodal carbon nanotube-reinforced aluminum matrix composite material. The bimodal carbon nanotube-reinforced aluminum matrix composite material includes soft regions and hard regions. The soft regions are discretely distributed in a "band-like" pattern within the hard regions, and there is a clear and abrupt interface between the soft and hard regions. The hard regions include an aluminum alloy matrix and carbon nanotubes uniformly dispersed within the aluminum alloy matrix, and the grain size of the aluminum alloy matrix in the hard regions is uniform. The soft regions include an aluminum alloy matrix without carbon nanotubes. The overall yield strength of the bimodal carbon nanotube-reinforced aluminum matrix composite material prepared by this invention does not change significantly under different extrusion ratios.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of composite material preparation technology, specifically relating to a method for preparing a dual-modal carbon nanotube reinforced aluminum matrix composite material. Background Technology

[0002] Carbon nanotubes (CNTs) are considered ideal reinforcements for aluminum matrix composites due to their excellent mechanical properties and good physicochemical stability. Studies have shown that introducing an appropriate amount of CNTs into aluminum alloys, combined with extrusion processing, can orient the CNTs along the extrusion direction, thereby fully utilizing their load transfer effect and significantly improving the strength of aluminum matrix composites. Extrusion is one of the most common and efficient plastic deformation methods for densifying and shaping metallic materials, especially aluminum matrix composites. For CNT-reinforced aluminum matrix composites, extrusion not only effectively closes residual pores between powder particles, but more importantly, it induces the CNTs to orient along the extrusion direction, which is essential for efficient load transfer from the matrix to the reinforcement. In fact, from laboratory research to industrial production, extrusion (including forward extrusion and reverse extrusion) has become the core process for preparing rod, profile, and tubular CNT-reinforced aluminum matrix composite products. Its process parameters (such as extrusion ratio and extrusion temperature) directly determine the macroscopic mechanical properties of the final components. However, the introduction of carbon nanotubes significantly refines the grain size of the aluminum matrix, reducing its dislocation storage capacity and consequently decreasing the work hardening ability of the composite material. Therefore, carbon nanotube-reinforced aluminum matrix composites generally suffer from insufficient plasticity. This inverse relationship between strength and plasticity has become a key bottleneck restricting the engineering applications of this type of composite material.

[0003] To overcome the aforementioned strength-ductility inversion problem, existing technologies have proposed constructing a dual-modal non-uniform microstructure to synergistically enhance the strength and ductility of carbon nanotube-reinforced aluminum matrix composites. For example, the paper "Enhancement of the strength-ductility relationship for carbon nanotube / Al-Cu-Mg nanocomposites by material parameter optimization" discloses a method that introduces a certain proportion of carbon nanotube-free soft regions into the composite material, forming a non-uniform microstructure with alternating soft regions (carbon nanotube-free regions) and hard regions (carbon nanotube-rich regions). This design mainly achieves a balance between strength and ductility based on two mechanisms: on the one hand, the uncoordinated deformation between the soft and hard regions induces the accumulation of geometrically necessary dislocations near the heterogeneous interface, generating a back stress strengthening effect, thereby further improving the strength of the composite material; on the other hand, the soft regions can effectively passivate crack propagation, improving the ductility of the composite material.

[0004] However, the above-mentioned non-uniform composite materials still have the following problems in practical applications:

[0005] First, extrusion plays an irreplaceable core role in the preparation process of this type of material, and existing bimodal microstructure design has not yet been adaptively optimized for extrusion process parameters. This results in the overall yield strength of the composite material being extremely sensitive to the extrusion ratio during the extrusion process. At a fixed extrusion temperature, as the extrusion ratio increases, the width of the soft zone strips becomes thinner, leading to a significant reduction in the strain hardening capacity of the soft zone, and thus reducing the contribution of the soft zone to the overall yield strength. Experimental results show that the overall yield strength of the composite material decreases with increasing extrusion ratio. For structural materials, yield strength is one of the core mechanical indicators for measuring the service safety and reliability of components, and its numerical stability is crucial. Given that extrusion is an essential step in the preparation of this type of composite material component, parameters such as the extrusion ratio must be adjusted according to the cross-sectional shape and size of the product. If the yield strength of the material is too sensitive to such unavoidable process fluctuations, it will seriously hinder the consistent control of its performance and its engineering application. Therefore, reducing the sensitivity of the overall yield strength of this type of composite material to the extrusion ratio is a key prerequisite for promoting its engineering application.

[0006] Therefore, there is an urgent need in the field for a bimodal carbon nanotube-reinforced aluminum matrix composite material with low extrusion ratio sensitivity to avoid significant fluctuations in overall yield strength with changes in extrusion ratio. Summary of the Invention

[0007] Therefore, the present invention provides a method for preparing a bimodal carbon nanotube reinforced aluminum matrix composite material to solve the problem that the overall yield strength of the bimodal carbon nanotube reinforced aluminum matrix composite material fluctuates greatly due to the change of extrusion ratio in the prior art, thereby preparing a bimodal carbon nanotube reinforced aluminum matrix composite material with low extrusion ratio sensitivity.

[0008] To address the aforementioned problems, this invention provides a method for preparing a dual-modal carbon nanotube-reinforced aluminum-based composite material, comprising the following steps:

[0009] Step 1): Mix carbon nanotube powder with aluminum alloy powder and perform a first high-energy ball milling process to obtain carbon nanotube reinforced aluminum matrix composite powder in which carbon nanotube powder is uniformly dispersed in aluminum alloy powder.

[0010] Step 2): Add the aluminum alloy powder to the carbon nanotube reinforced aluminum matrix composite powder and perform a second high-energy ball milling treatment to obtain a dual-modal composite powder;

[0011] Step 3): The dual-mode composite material powder is sintered to obtain a dual-mode carbon nanotube reinforced aluminum matrix composite material;

[0012] The dual-mode carbon nanotube reinforced aluminum matrix composite material includes soft regions and hard regions. The soft regions are discretely distributed in a "band-like" manner within the hard regions, and there is a clear and abrupt interface between the soft regions and the hard regions.

[0013] The hard region includes an aluminum alloy matrix and carbon nanotubes uniformly dispersed in the aluminum alloy matrix, and the grain size of the aluminum alloy matrix in the hard region is uniform.

[0014] The soft region comprises an aluminum alloy matrix without carbon nanotubes, and the unit size of the soft region is 0.8μm-2.5μm.

[0015] In some embodiments, the average radial dimension of the carbon nanotube powder is 10-100 nm.

[0016] In some embodiments, the aluminum alloy powder has an average particle size of 0.1-200 μm and an aluminum content greater than 85 wt.%.

[0017] In some embodiments, the first high-energy ball milling process includes: a ball-to-material ratio of 5:1 to 30:1, a milling time of 6 to 13 hours, and a milling speed of 200 to 250 rpm; and / or

[0018] The first high-energy ball milling process was carried out under an argon atmosphere.

[0019] In some embodiments, the mass fraction of carbon nanotubes in the carbon nanotube-reinforced aluminum matrix composite powder is 0.2-8 wt.%.

[0020] In some embodiments, in step 2), the mass ratio of the carbon nanotube-reinforced aluminum matrix composite powder to the aluminum alloy powder is (1-3):1.

[0021] In some embodiments, in the second high-energy ball milling process, the ball-to-material ratio is 5:1-30:1, the ball milling time is 2-6 hours, and the ball milling speed is 200-250 rpm; and / or

[0022] The second high-energy ball milling process was carried out under an argon atmosphere.

[0023] In some embodiments, the sintering process includes hot pressing sintering, hot isostatic pressing sintering, and spark plasma sintering.

[0024] In some embodiments, when pressure sintering is used in hot pressing, hot isostatic pressing, or spark plasma sintering, the sintering temperature is 350-660℃, the holding time is 0-4h, and the pressure is 20-100MPa; and / or

[0025] When the discharge plasma sintering treatment is performed using pressureless sintering, the sintering temperature is 600-700℃ and the holding time is 0-4h.

[0026] In some embodiments, step 3) is followed by step 4), which includes:

[0027] The bimodal carbon nanotube reinforced aluminum matrix composite material was subjected to extrusion, solution treatment, and aging treatment in sequence; and / or

[0028] In the extrusion process, the extrusion temperature is 350-500℃, and the extrusion ratio is 7:1-25:1; and / or

[0029] In the solution treatment, the temperature is 450-550℃ and the time is 1-4 hours; and / or

[0030] The time-dependent processing includes natural time-dependent processing or artificial time-dependent processing, and the time-dependent processing time is 5 to 120 hours.

[0031] When artificial aging is used, the temperature is 100-200℃.

[0032] The method for preparing a dual-modal carbon nanotube reinforced aluminum matrix composite material provided by this invention has the following beneficial effects:

[0033] 1. The preparation method provided by this invention involves intense collisions, shearing, and crushing between the grinding balls and the powder during the first high-energy ball milling process. The aluminum alloy powder undergoes repeated cold welding, fracture, and re-cold welding, causing carbon nanotubes to be gradually embedded and uniformly dispersed into the interior and surface of the aluminum alloy powder particles. Simultaneously, this process introduces a large number of dislocations, vacancies, and other defects into the interior of the aluminum alloy powder particles, forming subgrain boundaries, thereby effectively refining the grain size of the aluminum alloy and obtaining carbon nanotube-reinforced aluminum-based composite material powder.

[0034] During the second high-energy ball milling process, a certain proportion of unrefined aluminum alloy powder is added to the aforementioned carbon nanotube-reinforced aluminum matrix composite powder. These newly added aluminum alloy powders have relatively coarse grains, forming a "dual-modal" size distribution with the refined carbon nanotube-reinforced aluminum matrix composite powder. The hard region (carbon nanotube-rich region) provides high strength, with the carbon nanotubes bearing the load; the soft region (no carbon nanotube region) provides deformability, alleviating stress concentration and thus improving the overall plasticity of the composite material. The main purpose of the second ball milling is to uniformly mix the coarse-grained aluminum powder with the ultrafine-grained composite powder, while simultaneously causing slight plastic deformation and grain refinement on the surface and near-surface regions of the coarse-grained particles, resulting in a dual-modal composite powder. This invention actively adjusts the unit size and grain size of the soft region by controlling the parameters of the second ball milling. Because the carbon nanotube-reinforced aluminum matrix composite powder in the hard region has high strength and relatively small particle size, this process has a relatively small impact on the carbon nanotube-reinforced aluminum matrix composite powder in the hard region.

[0035] In subsequent sintering, the bimodal composite material is densified, and an interface with abrupt changes in composition and grain size is formed between the soft and hard regions, ultimately yielding a bimodal carbon nanotube-reinforced aluminum matrix composite. Due to the pinning effect of carbon nanotubes at grain boundaries and the high interfacial energy of the fine-grained regions in the hard region, excessive grain growth during sintering is effectively suppressed. Simultaneously, the soft region, with its initially coarser grains and lower interfacial energy, exhibits a relatively weak growth tendency, effectively preserving the predetermined bimodal grain size distribution in both the soft and hard regions within the bimodal carbon nanotube-reinforced aluminum matrix composite.

[0036] This invention actively regulates the grain size and unit size of the soft region by controlling the parameters of the second high-energy ball milling process. Refining the unit size of the soft region can weaken the sensitivity of the overall yield strength of the bimodal carbon nanotube reinforced aluminum matrix composite to extrusion ratio fluctuations while simultaneously improving strength and plasticity. Refining the grain size of the soft region can reduce the extrusion-induced stress. <111> Hard texture strength enhances the deformation coordination ability of soft areas. Attached Figure Description

[0037] To more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. The drawings described below are merely exemplary, and those skilled in the art can derive other embodiments based on the provided drawings without creative effort.

[0038] Figure 1 This is a schematic diagram of the structure of a bimodal carbon nanotube reinforced aluminum matrix composite material: (a) is the bimodal microstructure obtained by existing technology; (b) is the bimodal microstructure obtained by the preparation method of this invention.

[0039] Figure 2 The microstructure characterization results of the bimodal carbon nanotube reinforced aluminum matrix composite material prepared in Example 1 at 370℃ and 16:1 extrusion conditions are as follows: (a) is a metallographic photograph along the extrusion direction; (b) is a transmission image of the microstructure of the hard region; (c) is the inverse pole figure corresponding to the soft region.

[0040] Figure 3 The microstructure characterization results of the bimodal carbon nanotube reinforced aluminum matrix composite material prepared in Example 2 under extrusion conditions of 370℃ and 16:1 are as follows: (a) is a metallographic photograph along the extrusion direction; (b) is a transmission image of the microstructure of the hard region; (c) is the inverse pole figure corresponding to the soft region.

[0041] Figure 4The microstructure characterization results of the bimodal carbon nanotube reinforced aluminum matrix composite material prepared by Comparative Example 2 at 370℃ and 16:1 extrusion conditions are as follows: (a) is a metallographic photograph along the extrusion direction; (b) is a transmission image of the microstructure of the hard region; and (c) is the inverse pole figure corresponding to the soft region.

[0042] Figure 5 The microstructure characterization results of the bimodal carbon nanotube reinforced aluminum matrix composite material prepared by Comparative Example 3 at 370℃ and 16:1 extrusion conditions are as follows: (a) is a metallographic photograph along the extrusion direction; (b) is a transmission image of the microstructure of the hard region; and (c) is the inverse pole figure corresponding to the soft region.

[0043] Figure 6 The microstructure characterization results of the bimodal carbon nanotube reinforced aluminum matrix composite material prepared by Comparative Example 4 at 370℃ and 16:1 extrusion are as follows: (a) is a metallographic photograph along the extrusion direction; (b) is a transmission image of the microstructure of the hard region; and (c) is the inverse pole figure corresponding to the soft region.

[0044] Figure 7 The variation of strength and elongation with soft zone unit size under the conditions of extrusion temperature of 370℃ and extrusion ratio of 16:1 is shown. Detailed Implementation

[0045] To further illustrate the technical means and effects adopted by the present invention to achieve the intended purpose, the specific embodiments, structures, features, and effects according to the present invention will be described in detail below with reference to the accompanying drawings and preferred embodiments. In the following description, different "an embodiment" or "an embodiment" do not necessarily refer to the same embodiment. Furthermore, specific features, structures, or characteristics in one or more embodiments can be combined in any suitable form.

[0046] See also Figures 1 to 7 As shown in the embodiments of the present invention, a method for preparing a dual-modal carbon nanotube reinforced aluminum matrix composite material is provided, comprising the following steps:

[0047] Step 1): Mix carbon nanotube powder with aluminum alloy powder and perform a first high-energy ball milling process to obtain carbon nanotube reinforced aluminum matrix composite powder in which carbon nanotube powder is uniformly dispersed in aluminum alloy powder.

[0048] In the first high-energy ball milling process, intense collisions, shearing, and crushing occur between the grinding balls and the powder. The aluminum alloy powder undergoes repeated cold welding, fracture, and re-cold welding, causing carbon nanotubes to be gradually embedded and uniformly dispersed within and on the surface of the aluminum alloy powder particles. Simultaneously, this process introduces numerous dislocations, vacancies, and other defects into the interior of the aluminum alloy powder particles, forming subgrain boundaries, thereby effectively refining the grain size of the aluminum alloy and obtaining carbon nanotube-reinforced aluminum matrix composite powder.

[0049] Step 2): Add the aluminum alloy powder to the carbon nanotube reinforced aluminum matrix composite powder and perform a second high-energy ball milling treatment to obtain a dual-modal composite powder;

[0050] During the second high-energy ball milling process, a certain proportion of unrefined aluminum alloy powder is added to the aforementioned carbon nanotube-reinforced aluminum matrix composite powder. These newly added aluminum alloy powders have relatively coarse grains, forming a "dual-modal" size distribution with the refined carbon nanotube-reinforced aluminum matrix composite powder. The hard region (carbon nanotube-rich region) provides high strength, with the carbon nanotubes bearing the load; the soft region (no carbon nanotube region) provides deformability, alleviating stress concentration and thus improving the overall plasticity of the composite material. The main purpose of the second ball milling is to uniformly mix the coarse-grained aluminum powder with the ultrafine-grained composite powder, while simultaneously causing slight plastic deformation and grain refinement on the surface and near-surface regions of the coarse-grained particles, resulting in a dual-modal composite powder. This invention actively adjusts the unit size and grain size of the soft region by controlling the parameters of the second ball milling. Because the carbon nanotube-reinforced aluminum matrix composite powder in the hard region has high strength and relatively small particle size, this process has a relatively small impact on the carbon nanotube-reinforced aluminum matrix composite powder in the hard region.

[0051] Step 3): The dual-mode composite material powder is sintered to obtain a dual-mode carbon nanotube reinforced aluminum matrix composite material;

[0052] During sintering, the bimodal composite material is densified, and an interface with abrupt changes in composition and grain size is formed between the soft and hard regions, ultimately yielding a bimodal carbon nanotube-reinforced aluminum matrix composite. Due to the pinning effect of carbon nanotubes at grain boundaries and the high interfacial energy of the fine-grained regions in the hard region, excessive grain growth during sintering is effectively suppressed. Simultaneously, the soft region, with its initially coarser grains and lower interfacial energy, exhibits a relatively weak growth tendency, effectively preserving the predetermined bimodal grain size distribution.

[0053] like Figure 1 As shown, the dual-mode carbon nanotube reinforced aluminum matrix composite material includes soft regions and hard regions. The soft regions are discretely distributed in a "band-like" manner within the hard regions, and there is a clear and abrupt interface between the soft regions and the hard regions.

[0054] The hard region includes an aluminum alloy matrix and carbon nanotubes uniformly dispersed in the aluminum alloy matrix, and the grain size of the aluminum alloy matrix in the hard region is uniform.

[0055] In this invention, uniform grain size means that the equivalent circle diameter of no less than 200 grains is statistically analyzed using metallographic image analysis software, and the standard deviation SD is calculated to be ≤2.

[0056] The soft region comprises an aluminum alloy matrix without carbon nanotubes, and the unit size of the soft region is 0.8μm-2.5μm.

[0057] The method for calculating the unit size of soft areas in this invention is as follows: count no less than 200 soft areas, measure their width along the direction perpendicular to the extension of the soft area strip, take the width of each soft area as the unit size of the soft area, and then calculate the arithmetic mean of the unit sizes of all the counted soft areas, which is the average unit size of the soft area.

[0058] Microstructural analysis shows that significant microstructures form within the soft areas after extrusion processing. <111> The crystallographic texture is characterized by fine grains, while the orientation of hard grains is relatively random. The intense plastic flow and shear deformation generated during extrusion are the direct causes of the induced crystallographic texture, and face-centered cubic metals are prone to forming this texture during axial deformation. <111> The filamentary texture is its intrinsic deformation behavior. In face-centered cubic metals, <111> The crystallographic orientation is a hard orientation, and the presence of this texture limits the coordination ability of the soft areas during subsequent deformation, which is not conducive to further improvement of the plasticity of the composite material. This means that after the existing bimodal structure undergoes the necessary extrusion process, additional unfavorable textures will inevitably be introduced, thus partially offsetting the plasticity-improving effect that the soft areas should play.

[0059] This invention actively regulates the grain size and unit size of the soft region by controlling the parameters of the second high-energy ball milling process, refining the unit size of the soft region to 0.8μm-2.5μm. This not only weakens the sensitivity of the overall yield strength of the bimodal carbon nanotube reinforced aluminum matrix composite to extrusion ratio fluctuations but also simultaneously improves its strength and plasticity. Refining the grain size of the soft region can reduce the extrusion-induced stress. <111> The hard texture enhances the deformation coordination ability of the soft area, thereby maintaining the high strength of the dual-mode carbon nanotube reinforced aluminum matrix composite while further improving its plasticity.

[0060] In some embodiments, the average radial dimension of the carbon nanotube powder is 10-100 nm.

[0061] In some embodiments, the aluminum alloy powder has an average particle size of 0.1-200 μm and an aluminum content greater than 85 wt.%.

[0062] The larger the initial particle size of the aluminum alloy powder, the larger the final particle size after refinement under the same ball milling conditions, and the larger the unit size of the soft zone. The smaller the initial particle size of the aluminum alloy powder, the easier it is to be further refined during the ball milling process, and the smaller the unit size of the soft zone. This invention comprehensively controls the unit size and grain size of the soft and hard zones by controlling the particle size of the aluminum alloy powder and the parameters of the first high-energy ball milling treatment and the second high-energy ball milling treatment.

[0063] In some embodiments, the first high-energy ball milling process includes: a ball-to-material ratio of 5:1 to 30:1, a milling time of 6 to 13 hours, and a milling speed of 200 to 250 rpm; and / or

[0064] The first high-energy ball milling process was carried out under an argon atmosphere.

[0065] This invention controls the unit size and grain size of the hard zone by controlling the parameters of the first high-energy ball milling process.

[0066] In some embodiments, the mass fraction of carbon nanotubes in the carbon nanotube-reinforced aluminum matrix composite powder is 0.2-8 wt.%.

[0067] This invention controls the distribution of carbon nanotubes in the hard region by controlling the mass fraction of carbon nanotubes in the carbon nanotube-reinforced aluminum matrix composite powder, thereby controlling the parameters of the hard region and achieving performance matching between the soft and hard regions.

[0068] In some embodiments, in step 2), the mass ratio of the carbon nanotube-reinforced aluminum matrix composite powder to the aluminum alloy powder is (1-3):1.

[0069] This invention controls the distribution of soft and hard regions by controlling the mass ratio of carbon nanotube-reinforced aluminum matrix composite powder and aluminum alloy powder, thereby achieving performance matching between the soft and hard regions.

[0070] In some embodiments, in the second high-energy ball milling process, the ball-to-material ratio is 5:1-30:1, the ball milling time is 2-6 hours, and the ball milling speed is 200-250 rpm; and / or

[0071] The second high-energy ball milling process was carried out under an argon atmosphere.

[0072] This invention controls the unit size and grain size of the soft region by controlling the parameters of the second high-energy ball milling process. At the same time, the second high-energy ball milling process is carried out under an argon atmosphere to avoid the participation of reactive gases such as oxygen in the reaction.

[0073] In some embodiments, the sintering process includes hot pressing sintering, hot isostatic pressing sintering, and spark plasma sintering.

[0074] In some embodiments, when hot pressing sintering, hot isostatic pressing sintering, or spark plasma sintering is performed under pressure, the sintering temperature is 350-660℃, the holding time is 0-4h, and the pressure is 20-100MPa.

[0075] In some embodiments, when the discharge plasma sintering treatment is performed using pressureless sintering, the sintering temperature is 600-700℃ and the holding time is 0-4h.

[0076] In some embodiments, step 3) is followed by step 4), which includes:

[0077] The bimodal carbon nanotube reinforced aluminum matrix composite material was subjected to extrusion, solution treatment, and aging treatment in sequence.

[0078] In some embodiments, the extrusion temperature is 350-500°C and the extrusion ratio is 7:1-25:1.

[0079] In some embodiments, the solution treatment is performed at a temperature of 450-550°C for a time of 1-4 hours.

[0080] In some embodiments, the aging process includes natural aging or artificial aging, and the aging process lasts for 5 to 120 hours.

[0081] When artificial aging is used, the temperature is 100-200℃.

[0082] Extrusion densifies the composite material and induces carbon nanotubes to oriented along the extrusion direction, forming a bimodal microstructure with alternating soft and hard regions. Solution treatment fully dissolves the alloying elements in the matrix, resulting in a supersaturated solid solution. Aging treatment promotes the uniform precipitation of nanoscale reinforcing phases. The three processes work synergistically to fully utilize the load transfer and back stress strengthening of carbon nanotubes, while further enhancing strength through dispersed precipitation and preserving the contribution of soft regions to plasticity.

[0083] The overall yield strength of the dual-modal carbon nanotube reinforced aluminum matrix composite material provided by this invention will not change significantly due to fluctuations in the extrusion ratio, and it achieves simultaneous improvement in strength and plasticity.

[0084] The present invention will be further described below with reference to specific embodiments and comparative examples.

[0085] Example 1:

[0086] This embodiment provides a method for preparing a dual-modal carbon nanotube reinforced aluminum matrix composite material, including the following steps:

[0087] Step 1): Mix 75g of carbon nanotube powder with pre-alloyed 2009 aluminum alloy powder (Al-Cu-Mg system) with an average particle size of 13μm. The total mass of the powder is 3.75kg. Place the mixture in a stirred high-energy ball mill and load it with 75kg of stainless steel grinding balls. Under the protection of argon atmosphere, perform the first high-energy ball milling treatment at a speed of 200rpm for 12h to obtain carbon nanotube reinforced aluminum matrix composite powder in which carbon nanotube powder is uniformly dispersed in aluminum alloy powder.

[0088] Step 2): Add 1.25 kg of pre-alloyed 2009 aluminum alloy powder of the same specification to the same grinding jar of the stirred high-energy ball mill, and perform a second high-energy ball milling treatment at a speed of 200 rpm for 6 hours under argon atmosphere protection to obtain dual-modal composite material powder.

[0089] Step 3): The bimodal composite powder was vacuum hot-pressed and sintered at 540℃ and 70MPa for 1.5h to obtain a bimodal carbon nanotube reinforced aluminum matrix composite.

[0090] Step 4): The bimodal carbon nanotube reinforced aluminum matrix composite was extruded at 370℃ with extrusion ratios of 7:1, 16:1 and 25:1, respectively. Then, it was solution treated at 500℃ for 2 hours, water quenched and naturally aged for 96 hours to obtain bimodal carbon nanotube reinforced aluminum matrix composites under three different extrusion conditions.

[0091] The metallographic structure along the extrusion direction of the bimodal carbon nanotube-reinforced aluminum matrix composite material obtained under extrusion conditions of 370℃ and 16:1 is as follows: Figure 2 As shown in (a), the soft regions are distributed in a uniform, fine, and diffuse band-like morphology within the hard regions, with an average unit size of 1.5 μm. Transmission electron microscopy characterization results are as follows: Figure 2 As shown in (b), the carbon nanotubes in the hard region microstructure are uniformly distributed with approximately equal grain sizes, around 290 nm. The soft region texture strength test results are as follows... Figure 2 As shown in (c), it has typical <111> Silk texture, with a texture strength of 3.58.

[0092] The mechanical properties of bimodal carbon nanotube-reinforced aluminum matrix composites obtained at 370℃ with different extrusion ratios are as follows: At an extrusion ratio of 7:1, the overall yield strength is 702 MPa, the tensile strength is 769 MPa, and the elongation is 6.3%; at an extrusion ratio of 16:1, the overall yield strength is 700 MPa, the tensile strength is 761 MPa, and the elongation is 6.8%; at an extrusion ratio of 25:1, the overall yield strength is 694 MPa, the tensile strength is 758 MPa, and the elongation is 6.4%. It can be seen that under different extrusion ratios, the variation in the overall yield strength of the bimodal carbon nanotube-reinforced aluminum matrix composite is less than 3%, exhibiting good stability.

[0093] Example 2:

[0094] This embodiment provides a method for preparing a dual-modal carbon nanotube reinforced aluminum matrix composite material, including the following steps:

[0095] Step 1): Mix 75g of carbon nanotube powder with pre-alloyed 2009 aluminum alloy powder (Al-Cu-Mg system) with an average particle size of 13μm. The total mass of the powder is 3.75kg. Place the mixture in a stirred high-energy ball mill and load it with 75kg of stainless steel grinding balls. Under the protection of argon atmosphere, perform the first high-energy ball milling treatment at a speed of 200rpm for 13h to obtain carbon nanotube reinforced aluminum matrix composite powder in which carbon nanotube powder is uniformly dispersed in aluminum alloy powder.

[0096] Step 2): Add 1.25 kg of pre-alloyed 2009 aluminum alloy powder of the same specification to the same grinding jar of the stirred high-energy ball mill, and perform a second high-energy ball milling treatment at a speed of 200 rpm for 5 hours under argon atmosphere protection to obtain bimodal composite material powder.

[0097] Step 3): The bimodal composite powder was vacuum hot-pressed and sintered at 540℃ and 70MPa for 1.5h to obtain a bimodal carbon nanotube reinforced aluminum matrix composite.

[0098] Step 4): The bimodal carbon nanotube reinforced aluminum matrix composite was extruded at 370℃ with extrusion ratios of 7:1, 16:1 and 25:1, respectively. Then, it was solution treated at 500℃ for 2 hours, water quenched and naturally aged for 96 hours to obtain bimodal carbon nanotube reinforced aluminum matrix composites under three different extrusion conditions.

[0099] The metallographic structure along the extrusion direction of the bimodal carbon nanotube-reinforced aluminum matrix composite material obtained under extrusion conditions of 370℃ and 16:1 is as follows: Figure 3 As shown in (a), the soft regions are distributed in a uniform, fine, and diffuse band-like morphology within the hard regions, with an average unit size of 2.3 μm. Transmission electron microscopy characterization results are as follows: Figure 3 As shown in (b), the carbon nanotubes in the hard region microstructure are uniformly distributed with approximately equal grain sizes, around 285 nm. The soft region texture strength test results are as follows... Figure 3 As shown in (c), it has typical <111> Silk texture, with a texture strength of 3.4.

[0100] The mechanical properties of bimodal carbon nanotube-reinforced aluminum matrix composites obtained at 370℃ with different extrusion ratios are as follows: At an extrusion ratio of 7:1, the overall yield strength is 706 MPa, the tensile strength is 764 MPa, and the elongation is 6.6%; at an extrusion ratio of 16:1, the overall yield strength is 701 MPa, the tensile strength is 766 MPa, and the elongation is 6.5%; at an extrusion ratio of 25:1, the overall yield strength is 708 MPa, the tensile strength is 770 MPa, and the elongation is 6.2%. It can be seen that under different extrusion ratios, the variation in the overall yield strength of the bimodal carbon nanotube-reinforced aluminum matrix composite is less than 3%, exhibiting good stability.

[0101] Example 3:

[0102] This embodiment provides a method for preparing a dual-modal carbon nanotube reinforced aluminum matrix composite material, including the following steps:

[0103] Step 1): Mix 75g of carbon nanotube powder with pre-alloyed 6061 aluminum alloy powder (Al-Mg-Si system) with an average particle size of 13μm. The total mass of the powder is 3.75kg. Place the mixture in a stirred high-energy ball mill and load it with 75kg of stainless steel grinding balls. Under the protection of argon atmosphere, perform the first high-energy ball milling treatment at a speed of 250rpm for 6h to obtain carbon nanotube reinforced aluminum matrix composite powder in which carbon nanotube powder is uniformly dispersed in aluminum alloy powder.

[0104] Step 2): Add 3.75 kg of pre-alloyed 6061 aluminum alloy powder of the same specification to the same grinding jar of the stirred high-energy ball mill, and perform a second high-energy ball milling treatment at a speed of 250 rpm for 2 hours under argon atmosphere protection to obtain dual-modal composite material powder.

[0105] Step 3): The dual-mode composite powder was vacuum hot-pressed and sintered at 580℃ and 70MPa for 1.5h to obtain a dual-mode carbon nanotube reinforced aluminum matrix composite.

[0106] Step 4): The bimodal carbon nanotube reinforced aluminum matrix composite material was extruded at 450℃ with extrusion ratios of 7:1, 16:1 and 25:1, respectively. Then, it was solution treated at 530℃ for 2 hours, water quenched and aged at 170℃ for 6 hours to obtain bimodal carbon nanotube reinforced aluminum matrix composite materials under three different extrusion conditions.

[0107] The soft texture strength test results show that it has typical... <111> Silk texture, with a texture strength of 3.54.

[0108] The mechanical properties of bimodal carbon nanotube reinforced aluminum matrix composites obtained at 450℃ with different extrusion ratios are as follows: when the extrusion ratio is 7:1, the overall yield strength is 515 MPa, the tensile strength is 559 MPa, and the elongation is 5.8%; when the extrusion ratio is 16:1, the overall yield strength is 512 MPa, the tensile strength is 563 MPa, and the elongation is 5.6%; when the extrusion ratio is 25:1, the overall yield strength is 520 MPa, the tensile strength is 561 MPa, and the elongation is 5.3%.

[0109] Comparative Example 1:

[0110] This comparative example includes the following steps:

[0111] Step 1): Mix 75g of carbon nanotube powder with 5kg of pre-alloyed 2009 aluminum alloy powder with an average particle size of 13μm, place the mixture in a stirred high-energy ball mill, and load 75kg of stainless steel grinding balls. Under the protection of argon atmosphere, perform the first high-energy ball milling treatment at a speed of 200rpm for 18h to obtain carbon nanotube reinforced aluminum matrix composite powder in which carbon nanotube powder is uniformly dispersed in aluminum alloy powder.

[0112] Step 2): The carbon nanotube reinforced aluminum matrix composite powder was vacuum hot-pressed and sintered at 540℃ and 70MPa for 1.5h to obtain the carbon nanotube reinforced aluminum matrix composite.

[0113] Step 3): The carbon nanotube reinforced aluminum matrix composite material was extruded at 370℃ with extrusion ratios of 7:1, 16:1 and 25:1, respectively. Then, it was solution treated at 500℃ for 2 hours, water quenched and naturally aged for 96 hours to obtain carbon nanotube reinforced aluminum matrix composite materials under three different extrusion conditions.

[0114] The mechanical properties of carbon nanotube-reinforced aluminum matrix composites obtained at 370℃ with different extrusion ratios are as follows: when the extrusion ratio is 7:1, the overall yield strength is 713 MPa, the tensile strength is 742 MPa, and the elongation is 2.3%; when the extrusion ratio is 16:1, the overall yield strength is 710 MPa, the tensile strength is 748 MPa, and the elongation is 2.5%; when the extrusion ratio is 25:1, the overall yield strength is 715 MPa, the tensile strength is 754 MPa, and the elongation is 2.6%.

[0115] Compared to Examples 1 and 2, the overall yield strength of the carbon nanotube-reinforced 2009 aluminum composite material is also insensitive to changes in the extrusion ratio. However, due to the lack of soft regions in its microstructure, it cannot achieve toughening through a deformation mechanism that coordinates soft and hard regions. Therefore, under the same extrusion process conditions, its elongation is significantly lower than that of the dual-modal carbon nanotube-reinforced 2009 aluminum composite material.

[0116] Comparative Example 2:

[0117] This comparative example includes the following steps:

[0118] Step 1): Mix 100g of carbon nanotube powder with 5kg of pre-alloyed 2009 aluminum alloy powder (Al-Cu-Mg system) with an average particle size of 13μm, place it in a stirred high-energy ball mill, and load 75kg of stainless steel grinding balls. Under the protection of argon atmosphere, perform the first high-energy ball milling treatment at a speed of 200rpm for 18h to obtain carbon nanotube reinforced aluminum matrix composite powder in which carbon nanotube powder is uniformly dispersed in aluminum alloy powder.

[0119] Step 2): Weigh 750g of carbon nanotube reinforced aluminum matrix composite powder, mix 750g of carbon nanotube reinforced aluminum matrix composite powder with 250g of pre-alloyed 2009 aluminum alloy powder of the same specification, place in a mechanical mixer, and mix for 6 hours at a ball-to-powder ratio of 1:1 and a rotation speed of 50rpm to obtain dual-modal composite powder.

[0120] Step 3): The bimodal composite powder was vacuum hot-pressed and sintered at 540℃ and 70MPa for 1.5h to obtain a bimodal carbon nanotube reinforced aluminum matrix composite.

[0121] Step 4): The bimodal carbon nanotube reinforced aluminum matrix composite material was extruded at 370℃ with extrusion ratios of 7:1, 16:1 and 25:1, respectively. Then, it was solution treated at 500℃ for 2 hours, water quenched and naturally aged for 96 hours to obtain bimodal carbon nanotube reinforced aluminum matrix composite materials under three different extrusion conditions.

[0122] Compared with Examples 1 and 2, this comparative example obtains a bimodal microstructure using conventional processes. The specific bimodal microstructures obtained by conventional processes and the method of this invention are as follows: Figure 1 As shown, the metallographic structure along the extrusion direction of the bimodal carbon nanotube-reinforced aluminum matrix composite material obtained under extrusion conditions of 370℃ and 16:1 is as follows. Figure 4 As shown in (a), the soft regions are distributed in strips along the extrusion direction within the hard regions, and the average unit size of the soft regions is 4 μm. Transmission electron microscopy characterization results are as follows: Figure 4 As shown in (b), the carbon nanotubes in the hard region microstructure are uniformly distributed with approximately equal grain sizes, around 280 nm. The soft region texture strength test results are as follows... Figure 4 As shown in (c), it has typical <111> Silk texture, with a texture strength of 26.62.

[0123] The mechanical properties of bimodal carbon nanotube reinforced aluminum matrix composites obtained at 370℃ with different extrusion ratios are as follows: when the extrusion ratio is 7:1, the overall yield strength is 669 MPa, the tensile strength is 704 MPa, and the elongation is 3.2%; when the extrusion ratio is 16:1, the overall yield strength is 650 MPa, the tensile strength is 713 MPa, and the elongation is 3.7%; when the extrusion ratio is 25:1, the overall yield strength is 633 MPa, the tensile strength is 701 MPa, and the elongation is 3.5%.

[0124] The texture strength of the soft region in this comparative example is significantly higher than that in Examples 1 and 2, and the overall yield strength shows a high sensitivity to changes in the extrusion ratio, while the overall mechanical properties of high strength and plasticity are significantly lower. This performance difference mainly stems from two aspects: firstly, the size of the soft region was not stably maintained during extrusion, and its strain hardening capacity continuously decreased with increasing extrusion ratio, leading to a corresponding decrease in overall yield strength; secondly, a stronger texture was formed within the soft region. <111> The filament texture, which is a hard orientation in the face-centered cubic structure, will inhibit the initiation of multiple slip systems during plastic deformation, weaken the uniform deformation coordination ability of the soft region, and thus worsen the strong-plasticity matching of the material.

[0125] Comparative Example 3:

[0126] The difference between this comparative example and Examples 1 and 2 is that the first high-energy ball milling treatment has a rotation speed of 200 rpm and a milling time of 17 h; the second high-energy ball milling treatment has a rotation speed of 200 rpm and a milling time of 1 h; the remaining raw material composition and process steps are consistent with Examples 1 and 2.

[0127] The metallographic structure along the extrusion direction of the bimodal carbon nanotube-reinforced aluminum matrix composite material obtained under extrusion conditions of 370℃ and 16:1 is as follows: Figure 5 As shown in (a), the soft regions are distributed in a band-like pattern within the hard regions, and the average unit size of the soft regions is 2.8 μm. Transmission electron microscopy characterization results are as follows: Figure 5 As shown in (b), the carbon nanotubes in the hard region microstructure are uniformly distributed, with approximately equal grain sizes of about 270 nm. The soft region texture strength test results are as follows... Figure 5 As shown in (c), it has typical <111> Silk texture, with a texture strength of 4.7.

[0128] At 370℃ and an extrusion ratio of 16:1, the mechanical properties of the resulting bimodal carbon nanotube reinforced aluminum matrix composite are as follows: overall yield strength of 691 MPa, tensile strength of 745 MPa, and elongation of 5.6%.

[0129] It can be seen that although this comparative example has a texture strength of the soft region similar to that of Examples 1 and 2, the ball milling time of the soft region is insufficient, resulting in insufficient grain refinement of the soft region, thereby reducing the strength of the material. At the same time, the size matching between the soft region and the hard region is not optimal, which also has an adverse effect on the plasticity of the material, resulting in poor elongation.

[0130] Comparative Example 4:

[0131] The difference between this comparative example and Examples 1 and 2 is that the first high-energy ball milling treatment has a rotation speed of 200 rpm and a milling time of 10 h; the second high-energy ball milling treatment has a rotation speed of 200 rpm and a milling time of 8 h; the remaining raw material composition and process steps are consistent with Examples 1 and 2.

[0132] The metallographic structure along the extrusion direction of the bimodal carbon nanotube-reinforced aluminum matrix composite material obtained under extrusion conditions of 370℃ and 16:1 is as follows: Figure 6 As shown in (a), the unit size of the soft region is further refined, making it difficult to clearly identify under a metallographic microscope. The average unit size of the soft region is 0.7 μm. The transmission electron microscopy characterization results are as follows: Figure 6 As shown in (b), the carbon nanotubes in the hard region microstructure are uniformly distributed, with approximately equal grain sizes of about 300 nm. The soft region texture strength test results are as follows... Figure 6 As shown in (c), it has typical <111> Silk texture, with a texture strength of 1.99.

[0133] At 370℃ and an extrusion ratio of 16:1, the mechanical properties of the resulting bimodal carbon nanotube reinforced aluminum matrix composite material are as follows: overall yield strength of 705 MPa, tensile strength of 769 MPa, and elongation of 4.8%.

[0134] Compared to Examples 1 and 2, this comparative example extended the ball milling time in the soft zone. While the strength was comparable to Examples 1 and 2, the elongation decreased. This performance difference primarily stemmed from the excessive refinement of the soft zone units. Overly refined soft zone units weakened their crack-passivating ability, ultimately leading to a reduction in the material's elongation.

[0135] Comparative Example 5:

[0136] This comparative example includes the following steps:

[0137] Step 1): Mix 100g of carbon nanotube powder with 5kg of pre-alloyed 6061 aluminum alloy powder (Al-Mg-Si system) with an average particle size of 13μm, place it in a stirred high-energy ball mill, and load 50kg of stainless steel grinding balls. Under the protection of argon atmosphere, perform the first high-energy ball milling treatment at a speed of 250rpm for 8h to obtain carbon nanotube reinforced aluminum matrix composite powder in which carbon nanotube powder is uniformly dispersed in aluminum alloy powder.

[0138] Step 2): Weigh 500g of carbon nanotube reinforced aluminum matrix composite powder, mix 500g of carbon nanotube reinforced aluminum matrix composite powder with 500g of pre-alloyed 6061 aluminum alloy powder of the same specification, place in a mechanical mixer, and mix for 6 hours at a ball-to-powder ratio of 1:1 and a rotation speed of 50rpm to obtain dual-modal composite powder.

[0139] Step 3): The dual-mode composite powder was vacuum hot-pressed and sintered at 580℃ and 70MPa for 1.5h to obtain a dual-mode carbon nanotube reinforced aluminum matrix composite.

[0140] Step 4): The bimodal carbon nanotube reinforced aluminum matrix composite material was extruded at 450℃ with extrusion ratios of 7:1, 16:1 and 25:1, respectively. Then, it was solution treated at 530℃ for 2 hours, water quenched and aged at 170℃ for 6 hours to obtain bimodal carbon nanotube reinforced aluminum matrix composite materials under three different extrusion conditions.

[0141] Compared to Example 3, this comparative example obtained a bimodal microstructure through conventional processes. The bimodal carbon nanotube-reinforced aluminum matrix composite material obtained under extrusion conditions of 450°C and a 16:1 ratio showed that its soft-zone texture strength test results indicate that it possesses typical... <111> Silk texture, with a texture strength of 10.7.

[0142] Compared with Example 3, this comparative example obtained a bimodal microstructure through a conventional process. The mechanical properties of the bimodal carbon nanotube-reinforced aluminum matrix composites obtained at 450°C with different extrusion ratios are as follows: when the extrusion ratio is 7:1, the overall yield strength is 490 MPa, the tensile strength is 533 MPa, and the elongation is 4.1%; when the extrusion ratio is 16:1, the overall yield strength is 476 MPa, the tensile strength is 539 MPa, and the elongation is 4.8%; when the extrusion ratio is 25:1, the overall yield strength is 459 MPa, the tensile strength is 521 MPa, and the elongation is 4.3%.

[0143] Compared with Example 3, the overall yield strength of this comparative example is highly sensitive to changes in the extrusion ratio, and the comprehensive mechanical properties of strong plasticity are significantly lower.

[0144] By summarizing the mechanical property data from Examples 1, 2, 2, 3, and 4, the relationships between the overall yield strength, tensile strength, and elongation of Example 1 under the raw material conditions of Example 1, with respect to the soft zone unit size, were obtained under the conditions of an extrusion temperature of 370℃ and an extrusion ratio of 16:1. Figure 7 As shown in the figure, the materials in Examples 1 and 2 exhibit excellent overall performance at the soft cell size. Extensive testing has verified that when the soft cell size is controlled between 0.8 μm and 2.5 μm, the overall yield strength fluctuation of the bimodal carbon nanotube-reinforced aluminum matrix composite material under conventional extrusion processing conditions is less than 5%, and at this point, the material achieves the optimal balance between strength and plasticity.

[0145] It will be readily understood by those skilled in the art that, without conflict, the advantageous technical features of the above-mentioned methods can be freely combined and superimposed.

[0146] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the protection scope of the present invention.

Claims

1. A method for preparing a dual-modal carbon nanotube reinforced aluminum matrix composite material, characterized in that, Includes the following steps: Step 1): Mix carbon nanotube powder with aluminum alloy powder and perform a first high-energy ball milling process to obtain carbon nanotube reinforced aluminum matrix composite powder in which carbon nanotube powder is uniformly dispersed in aluminum alloy powder. Step 2): Add the aluminum alloy powder to the carbon nanotube reinforced aluminum matrix composite powder and perform a second high-energy ball milling treatment to obtain a dual-modal composite powder; Step 3): The dual-mode composite material powder is sintered to obtain a dual-mode carbon nanotube reinforced aluminum matrix composite material; The dual-mode carbon nanotube reinforced aluminum matrix composite material includes soft regions and hard regions. The soft regions are discretely distributed in a "band-like" manner within the hard regions, and there is a clear and abrupt interface between the soft regions and the hard regions. The hard region includes an aluminum alloy matrix and carbon nanotubes uniformly dispersed in the aluminum alloy matrix, and the grain size of the aluminum alloy matrix in the hard region is uniform. The soft region comprises an aluminum alloy matrix without carbon nanotubes, and the unit size of the soft region is 0.8μm-2.5μm.

2. The preparation method according to claim 1, characterized in that, The average radial dimension of the carbon nanotube powder is 10-100 nm.

3. The preparation method according to claim 1, characterized in that, The aluminum alloy powder has an average particle size of 0.1-200 μm and an aluminum content greater than 85 wt.%.

4. The preparation method according to claim 1, characterized in that, In the first high-energy ball milling process: the ball-to-material ratio is 5:1-30:1, the ball milling time is 6-13 hours, and the ball milling speed is 200-250 rpm; and / or The first high-energy ball milling process was carried out under an argon atmosphere.

5. The preparation method according to claim 1, characterized in that, The carbon nanotubes in the carbon nanotube-reinforced aluminum matrix composite powder have a mass fraction of 0.2-8 wt.%.

6. The preparation method according to claim 1, characterized in that, In step 2), the mass ratio of the carbon nanotube-reinforced aluminum matrix composite powder to the aluminum alloy powder is (1-3):

1.

7. The preparation method according to claim 1, characterized in that, In the second high-energy ball milling process, the ball-to-material ratio is 5:1-30:1, the ball milling time is 2-6 hours, and the ball milling speed is 200-250 rpm; and / or The second high-energy ball milling process was carried out under an argon atmosphere.

8. The preparation method according to claim 1, characterized in that, The sintering process includes hot pressing sintering, hot isostatic pressing sintering, and spark plasma sintering.

9. The preparation method according to claim 8, characterized in that, In the hot pressing sintering, hot isostatic pressing sintering, and spark plasma sintering, when pressure sintering is used, the sintering temperature is 350-660℃, the holding time is 0-4h, and the pressure is 20-100MPa; and / or When the discharge plasma sintering treatment is performed using pressureless sintering, the sintering temperature is 600-700℃ and the holding time is 0-4h.

10. The preparation method according to claim 1, characterized in that, Step 3) is followed by step 4), which includes: The bimodal carbon nanotube reinforced aluminum matrix composite material was subjected to extrusion, solution treatment, and aging treatment in sequence; and / or In the extrusion process, the extrusion temperature is 350-500℃, and the extrusion ratio is 7:1-25:1; and / or In the solution treatment, the temperature is 450-550℃ and the time is 1-4 hours; and / or The time-sensitivity processing includes natural time-sensitivity or artificial time-sensitivity, and the time-sensitivity processing time is 5-120 hours. When using artificial aging, the temperature is 100-200℃.