A method and product for producing sandblasted black titanium for 430 ferritic stainless steel

By employing gradient grinding, intelligent belt sanding management, and high-temperature curing, the quality and color consistency issues in the surface treatment of 430 stainless steel were resolved, the film performance was improved, and low-cost, high-quality sandblasted titanium products were produced.

CN123063833APending Publication Date: 2026-11-10ZHAOQING HONGWANG METAL IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611217319.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-12
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies for surface treatment of 430 stainless steel suffer from problems such as unstable surface grinding quality, difficulty in controlling color consistency, and insufficient film performance. In particular, when producing sandblasted black titanium products, issues such as intersecting sandblasting patterns, missed grinding, inconsistent pattern depth, reddish color, and substandard film adhesion and corrosion resistance often occur.

Method used

A gradient grinding process combined with intelligent abrasive belt management is adopted. By monitoring the performance parameters of the abrasive belt in real time and replacing it, the surface quality consistency is ensured. During the electrolytic coloring process, the color is monitored in real time and the electrolytic parameters are adjusted according to the preset correction rules to achieve closed-loop color control. Finally, high-temperature curing treatment is carried out to improve the film performance.

Benefits of technology

It significantly improves the surface quality and color consistency of 430 stainless steel, ensuring that the surface of sand black titanium products is delicate and uniform, the color is stable, the film adhesion and corrosion resistance are significantly improved, and the production of sand black titanium decorative materials with low cost is realized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063833A_ABST
    Figure CN123063833A_ABST
Patent Text Reader

Abstract

This invention provides a method and product for producing sandblasted black titanium on 430 ferritic stainless steel, relating to the field of stainless steel surface treatment technology. The method includes: gradient grinding of the surface of a 430 ferritic stainless steel substrate using abrasive belts; electrolytic coloring of the ground stainless steel substrate, with closed-loop control of color difference achieved by real-time monitoring of product color and adjustment of electrolytic parameters according to preset correction rules; and high-temperature curing of the electrolytically colored stainless steel substrate. Specifically, during the gradient grinding process, based on real-time monitoring of abrasive belt performance parameters, belt replacement is triggered when the monitored value deviates from the preset range. This invention enables stable and large-scale production of low-cost decorative-grade sandblasted black titanium surface treatment for 430 ferritic stainless steel, solving problems such as poor surface grinding quality, reddish color, and insufficient film performance, significantly improving product quality and reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of stainless steel surface treatment technology, and in particular to a method for producing sandblasted titanium dioxide of 430 ferritic stainless steel and its product. Background Technology

[0002] In the current decorative materials market, black titanium stainless steel is highly favored for its unique appearance and texture, with products based on 304 austenitic stainless steel dominating the market. However, 304 stainless steel contains the precious metal nickel, resulting in high raw material costs. In contrast, 430 ferritic stainless steel is nickel-free, costing 30%-40% less than 304 stainless steel. Furthermore, its natural ferromagnetism gives it unique advantages in applications requiring magnetic adsorption or welding, such as appliance casings, elevator cars, and building curtain walls.

[0003] Despite the cost and performance potential of 430 stainless steel, several technical bottlenecks remain in its large-scale production for high-end decorative applications, particularly for sandblasted titanium surfaces. Existing technologies for processing 430 stainless steel often face one or more of the following drawbacks: 1. Unstable surface grinding quality: The physical properties of 430 stainless steel are different from those of 304 stainless steel. Directly applying existing grinding processes can easily produce defects such as cross-grained sanding patterns, missed grinding, uneven texture depth, and large fluctuations in roughness on the stainless steel surface. It is impossible to form a uniform and delicate snowflake sand texture, which is difficult to meet the strict requirements of high-end decorative materials for surface consistency.

[0004] 2. Difficulty in color control and prone to reddish tinge: The industry lacks a dedicated black titanium electrolytic coloring process optimized for 430 stainless steel substrates. If traditional methods are used, due to the different characteristics of the passivation film on the surface of 430 stainless steel, uneven color and obvious reddish tinge are very likely to appear on the colored board surface, which seriously affects the aesthetics and consistency of the product.

[0005] 3. Insufficient film performance: The passivation film formed on the surface of 430 stainless steel is relatively unstable. The black titanium film obtained by conventional coloring process often fails to meet the standards in terms of adhesion, wear resistance and corrosion resistance. In subsequent transportation, processing and use, the film is prone to peeling, scratches or rust. Summary of the Invention

[0006] This invention aims to solve the technical problems existing in the prior art of surface grinding quality, difficulty in controlling color consistency, easy reddening, and insufficient film adhesion and corrosion resistance of 430 ferritic stainless steel when performing sandblasted titanium surface treatment. It provides a stable and large-scale production method for decorative-grade sandblasted titanium surface treatment of 430 ferritic stainless steel that can achieve low cost while ensuring high quality, as well as the products made therefrom.

[0007] To achieve the above-mentioned objective, this invention provides a method for producing 430 ferritic stainless steel sandblasted titanium, comprising: Gradient grinding steps: The surface of the 430 ferritic stainless steel substrate is treated with a gradient grinding process, which includes coarse grinding, fine grinding and fine grinding in sequence, using abrasive belts. Electrolytic coloring and color correction steps: The ground stainless steel substrate is subjected to electrolytic coloring treatment, and the color difference is controlled in a closed loop by real-time monitoring of product color and adjustment of electrolytic parameters according to preset correction rules. High-temperature curing step: The stainless steel substrate that has been electrolytically colored is subjected to high-temperature curing treatment; During the gradient grinding process, the performance parameters of the abrasive belt are monitored in real time. When the monitored value of the performance parameter deviates from the preset range, the abrasive belt is replaced.

[0008] Optionally, the gradient grinding process is a three-stage gradient grinding process, which sequentially uses a No. 120 abrasive belt for coarse grinding, a No. 180 abrasive belt for fine grinding, and a No. 240 abrasive belt for fine grinding.

[0009] Optionally, the gradient grinding process, after fine grinding, further includes a step of ultrafine grinding using a 400-grit abrasive belt.

[0010] Optionally, the performance parameter is the grinding current.

[0011] Optionally, the deviation of the monitored value of the performance parameter from the preset range means that: a preset nominal working current is set, and when the absolute value of the deviation between the real-time value of the grinding current and the preset nominal working current exceeds 10% of the preset nominal working current.

[0012] Optionally, the performance parameters are surface quality data obtained by an online sand texture detector.

[0013] Optionally, the conditions for triggering the sanding belt replacement may also include: triggering the sanding belt replacement when the usage mileage of the sanding belt reaches a preset mileage.

[0014] Optionally, the electrolytic coloring and color correction step includes: obtaining the preset correction rules from a reddish correction database.

[0015] Optionally, the high-temperature curing process is carried out at a temperature of 85-118°C.

[0016] Optionally, the high-temperature curing step includes: preliminary curing at 85-95°C, followed by final curing at 110-118°C.

[0017] Optionally, the 430 ferritic stainless steel substrate is 430W ferritic stainless steel with a thickness of 0.3-1.5mm.

[0018] This invention also provides a 430 ferritic stainless steel sandblasted titanium product, the product comprising: 430 ferritic stainless steel substrate; and A black titanium film layer is formed on the substrate; The product has a snowflake sand texture on its surface, and its colorimetric index is: L value between 31 and 32, A value between -0.8 and 0, and B value between 0 and 1.2.

[0019] Compared with the prior art, the embodiments of the present invention have the following beneficial effects: 1. Significantly improves surface quality and consistency: By adopting a gradient grinding process and combining it with a real-time monitoring and replacement mechanism for abrasive belt performance parameters, the problems of cross-grain texture and missed grinding that are prone to occur in the grinding of 430 stainless steel are effectively solved, ensuring that the abrasive surface texture is delicate, uniform and highly consistent, laying a solid foundation for subsequent high-quality plating.

[0020] 2. Effectively solves the problem of reddish tint and ensures color stability: By implementing closed-loop control of color difference during the electrolytic coloring process according to preset correction rules, especially by obtaining correction rules from the reddish tint correction database, the electrolytic parameters can be precisely adjusted, successfully stabilizing the product's chromaticity A value within the ideal range, effectively suppressing the reddish tint phenomenon on the board surface, and ensuring the high consistency and stability of the product color.

[0021] 3. Enhanced film performance and improved product reliability: By introducing a high-temperature curing process after electrolytic coloring, the adhesion, corrosion resistance, and wear resistance of the black titanium film on 430 stainless steel substrate are significantly improved, enabling the product to adapt to subsequent secondary processing and extending its service life.

[0022] 4. Achieving low-cost, high-quality production: This invention successfully realizes the application of low-cost 430 stainless steel in the field of high-end sandblasted titanium decorative materials. The produced products have excellent surface quality, stable color, and reliable performance, while having significant cost advantages, providing a low-cost application solution for 430 stainless steel in the field of high-end decorative materials. Attached Figure Description

[0023] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0024] Figure 1 This is a schematic flowchart of a production method according to an embodiment of the present invention.

[0025] Figure 2 This is a schematic diagram of the gradient grinding and intelligent belt abrasive management system according to an embodiment of the present invention.

[0026] Figure 3 This is a schematic diagram of the structure of a color control and curing system according to an embodiment of the present invention.

[0027] In the diagram: 1 is the coarse grinding unit, 2 is the fine grinding unit, 3 is the fine grinding unit, 4 is the central controller, 5 is the sanding belt mileage database, 6 is the current sensor, 7 is the sanding texture detector, 8 is the sanding belt replacement actuator, 10 is the electrolytic cell, 11 is the spectrophotometer, 12 is the electrolytic power controller, 13 is the red correction database, and 14 is the high-temperature curing tank. Detailed Implementation

[0028] To make the objectives, technical solutions, and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings. The described embodiments should not be regarded as limitations on the present invention. All other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0029] Unless otherwise defined, all technical and scientific terms used in the embodiments of this invention have the same meaning as commonly understood by one of ordinary skill in the art. The terminology used in the embodiments of this invention is for descriptive purposes only and is not intended to limit the invention.

[0030] Before providing a further detailed description of the embodiments of the present invention, the nouns and terms involved in the embodiments of the present invention will be explained, and the nouns and terms involved in the embodiments of the present invention shall be interpreted as follows.

[0031] (1) Snowflake sand texture: refers to a uniform, delicate, non-directional frosted texture formed on the surface of stainless steel through a multi-level gradient grinding process. Visually, it presents a uniform sand dot effect similar to scattered snowflakes. Its surface quality usually corresponds to the NO.4 grade surface standard in the industry. In the embodiments of the present invention, the texture is further defined by objective parameters, such as having an extremely low defect rate, such as the surface area occupied by cross-pattern or scratch-type sand texture being less than 0.5% of the total surface area of ​​the product, and its surface roughness Ra value being controllable within a specific range, thereby ensuring the measurability and determinability of the texture and avoiding inconsistencies caused by subjective judgment.

[0032] (2) Gradient grinding: refers to a surface treatment process in which the surface of a workpiece is ground in multiple stages by using grinding tools (such as abrasive belts) of different grit sizes (mesh count) from coarse to fine, in order to gradually reduce the surface roughness and finally obtain a surface with a specific texture and smoothness. This step-by-step optimization method can avoid the deep scratches and surface stress concentration problems that may be caused by heavy grinding in a single process.

[0033] (3) Redness Correction Database: This refers to a database that stores the correspondence between the product's chromaticity value (especially the A value representing red / green) and electrolytic process parameters (such as electrolytic current, process speed, electrolyte composition, etc.) during the electrolytic coloring process of stainless steel surfaces. When the product color deviates from the target (such as redness, i.e., the A value is too high), this database can be queried to obtain targeted parameter adjustment strategies, thereby achieving closed-loop control and precise correction of the color.

[0034] (4) High-temperature curing: This refers to the step of placing the stainless steel substrate with the incompletely stabilized film layer in a chemical solution (chemical treatment tank) or environment at a specific temperature after electrolytic coloring. The aim is to promote the transformation and stabilization of the film layer structure through heat energy, thereby improving the film layer's density, adhesion, corrosion resistance, and wear resistance. This step is crucial for ensuring the long-term reliability of the black titanium film layer on low-cost 430 ferritic stainless steel substrates.

[0035] Please see Figure 1 This invention aims to provide a method for producing sandblasted titanium on 430 ferritic stainless steel, addressing existing technical problems in the sandblasted titanium surface treatment of 430 stainless steel, such as poor surface grinding quality, difficulty in controlling color consistency and a tendency to turn reddish, and insufficient film performance. This method, through a series of synergistic steps, achieves the goal of stable and large-scale production of high-quality decorative-grade sandblasted titanium products on low-cost 430 ferritic stainless steel substrates. The core process of this method includes a gradient grinding step S10, an electrolytic coloring and color correction step S30, and a high-temperature curing step S40.

[0036] In the gradient grinding step S10, abrasive belts are used to treat the surface of the 430 ferritic stainless steel substrate. The purpose of this step is to address the difference in physical properties between 430 and 304 stainless steel by gradually improving the surface condition of the substrate through an orderly, coarse-to-fine grinding method, thus laying a high-quality foundation for the subsequent formation of a uniform black titanium film. By implementing gradient grinding, defects such as cross-grain patterns, missed areas, and inconsistent texture depth caused by improper processes can be effectively avoided, thereby solving the problem of unstable surface grinding quality in the prior art.

[0037] To ensure the stability and consistency of the gradient grinding step S10, this method also includes a crucial quality control step: during the execution of the gradient grinding step, based on real-time monitoring of the performance parameters of the abrasive belt, abrasive belt replacement is triggered when the monitored values ​​of the performance parameters deviate from a preset range. This design (in...) Figure 1 The principle behind the intelligent sanding belt management step S20 (which can be understood as running parallel to S10) is that the performance of the sanding belt continuously degrades during use, directly affecting the grinding effect. Traditional methods relying on manual experience or fixed-time replacement cannot accurately address the actual wear and tear of the sanding belt. By introducing a real-time monitoring and automatic triggering replacement mechanism, it can be ensured that the sanding belt always operates within its optimal performance range, thereby fundamentally guaranteeing the high consistency of the sanding surface texture of the entire roll of product and solving the problem of uneven sanding depth caused by sanding belt wear.

[0038] After high-quality surface grinding, the process proceeds to step S30, which involves electrolytic coloring and color correction. In this step, the ground stainless steel substrate undergoes electrolytic coloring. The key innovation of this step lies in its closed-loop control of color difference through real-time monitoring of product chromaticity and adjustment of electrolytic parameters according to preset correction rules. This design aims to solve the problem of difficult color control and a tendency to turn reddish due to variations in the surface passivation film characteristics of 430 stainless steel. By introducing real-time chromaticity monitoring and closed-loop feedback control, this method can dynamically and precisely adjust the electrolytic process, ensuring that the final product's color remains stable within the target range. This achieves online proactive control of color quality, rather than traditional offline sampling and passive adjustment.

[0039] Finally, a high-temperature curing step S40 is performed to cure the electrolytically colored stainless steel substrate at high temperatures. The design principle of this step is that the black titanium film formed on the surface of 430 stainless steel may not yet have reached its optimal structure and adhesion in the initial stage. By applying a specific high-temperature treatment, the internal structure of the film can be optimized and densified, while simultaneously enhancing the bonding force between the film and the substrate. Implementing this step effectively solves the problems of insufficient film performance, poor adhesion, and substandard corrosion resistance in the prior art, significantly improving the reliability and service life of the final product.

[0040] Furthermore, in a preferred embodiment, the gradient grinding process is a three-stage gradient grinding process, sequentially using a 120-grit abrasive belt for coarse grinding, a 180-grit abrasive belt for fine grinding, and a 240-grit abrasive belt for fine grinding. This specific combination of abrasive belt grits was optimized through extensive experimentation, enabling the stable preparation of an ideal snowflake-textured substrate on the surface of 430 stainless steel in an efficient and economical manner. The 120-grit coarse abrasive belt is responsible for quickly removing original defects on the substrate surface and establishing the basic texture, while the 180-grit fine abrasive belt refines the texture and eliminates coarse grinding marks. Finally, the 240-grit fine abrasive belt achieves the final surface refinement. The three work synergistically to achieve a good balance between surface quality and processing efficiency.

[0041] In another preferred embodiment, the gradient grinding process, after fine grinding, further includes an ultrafine grinding step using 400-grit abrasive belts. This approach targets specific high-end applications with higher requirements for surface texture. Adding 400-grit ultrafine grinding further reduces surface roughness compared to 240-grit belts, resulting in a finer, softer texture, even with a slightly silky finish. By adding this step, the technical solution of this method gains greater scalability and can meet the diverse needs of different market segments.

[0042] Furthermore, in a preferred embodiment, the performance parameter used to trigger belt replacement is specifically the grinding current. The grinding current is a direct electrical parameter reflecting the load on the grinding head motor, and the motor load is closely related to the frictional force (i.e., grinding force) between the belt and the workpiece. When the abrasive grains on the belt become dull and severely worn, to achieve the same cutting effect, the operator often unconsciously increases the grinding pressure, or the system automatically compensates, leading to a significant change in the grinding current. Therefore, monitoring the grinding current is a low-cost, fast-response, and highly reliable method for indirectly judging the wear state of the belt. By monitoring the grinding current, the problem of how to achieve real-time monitoring of belt performance in a simple and economical way is solved.

[0043] Based on the above, more specifically, the deviation of the monitored performance parameter value from the preset range means that: a preset nominal operating current is set, and when the absolute value of the deviation between the real-time value of the grinding current and the preset nominal operating current exceeds 10% of the preset nominal operating current, replacement is triggered. This technical solution provides a clear and operable quantitative judgment standard for monitoring the grinding current. The 10% threshold is an empirical value summarized from production practice. It can sensitively reflect significant degradation of the abrasive belt performance while avoiding frequent false triggers caused by normal current fluctuations, thus achieving accuracy and robustness in judging the timing of abrasive belt replacement.

[0044] In another optional implementation, the performance parameter is surface quality data obtained through an online sanding texture detector. This is a more direct and precise monitoring method. The online sanding texture detector uses technologies such as machine vision to directly photograph and analyze the polished stainless steel surface, calculating in real time indicators such as surface roughness, texture uniformity, and defects (such as scratches and bright spots). Compared to monitoring indirect parameters like polishing current, directly monitoring surface quality data can more fundamentally reflect whether the polishing effect meets the standards. In this way, even if the polishing current does not change significantly (e.g., local chipping of the sanding belt leading to scratches), the system can immediately detect the problem and trigger replacement, thus reliably ensuring the surface quality of the product.

[0045] Furthermore, in a more reliable implementation, the condition for triggering belt replacement also includes: triggering belt replacement when the belt's usage mileage reaches a preset mileage. This solution adds a guaranteed replacement strategy based on the belt's design life, in addition to real-time performance monitoring (whether based on current or vision). The belt's usage mileage (i.e., the cumulative length of steel belt ground) is a macroscopic cumulative indicator of its wear degree. By setting an experimentally verified upper limit for safe usage mileage, gradual performance degradation due to sensor failure or failure of the monitoring system to detect it in time can be prevented. This guarantee mechanism, combining real-time monitoring and periodic replacement, greatly improves the reliability of belt management and the stability of the production process, helping to ensure a high degree of product quality stability.

[0046] Furthermore, in the electrolytic coloring and color correction steps, the preset correction rules are specifically obtained from a reddish correction database. This scheme provides the core control logic for color closed-loop control. This reddish correction database is the core knowledge base of the method of this invention; it pre-stores a large amount of experimental data and expert experience, establishing a precise mathematical model or rule set between the chromaticity A value and key parameters such as electrolytic current and process speed. When the online colorimeter detects a trend of the A value deviating from the target, the control system no longer performs simple PID adjustment, but directly queries the database to obtain optimized, targeted adjustment instructions. In this way, the shortcomings of traditional color control—slow response, easy overshoot, and weak ability to handle specific problems (such as reddish tint)—are solved, achieving fast and accurate color correction.

[0047] Furthermore, in a preferred embodiment, the high-temperature curing treatment is performed at a temperature of 85-118°C. This temperature range is a critical process window to ensure the effective curing of the black titanium film on the 430 stainless steel surface. If the temperature is too low, the curing reaction will be insufficient, and the density and adhesion of the film will not be effectively improved; if the temperature is too high, it may cause excessive internal stress in the film, or even cause cracking or discoloration. By strictly controlling the curing temperature within this optimized range of 85-118°C, a good balance between improved film performance and process stability is achieved.

[0048] In a more preferred embodiment, the high-temperature curing step includes: preliminary curing at 85-95°C, followed by final curing at 110-118°C. This two-stage curing process offers advantages over single-stage isothermal curing. The first stage of low-temperature preliminary curing (85-95°C) allows the film layer to release stress and achieve initial stabilization under relatively gentle conditions, essentially "preheating" the film layer. The second stage of high-temperature final curing (110-118°C) further promotes the densification of the film layer structure, achieving optimal physicochemical properties. This stepped heating curing strategy yields black titanium films with lower internal stress, denser structure, and superior performance, significantly improving the product's long-term weather resistance and durability.

[0049] Furthermore, the 430 ferritic stainless steel substrate processed by the method of the present invention can specifically be 430W ferritic stainless steel with a thickness of 0.3-1.5mm. The 430W grade is a steel optimized for specific application scenarios, while the thickness range of 0.3-1.5mm covers most mainstream applications such as home appliances, elevators, and architectural decoration. This limitation clearly defines an important and specific application target of the method of the present invention, indicating that its technical solution has strong industrial relevance and practical value.

[0050] This invention also provides a 430 ferritic stainless steel sandblasted black titanium product. This product is produced using any of the methods described above. Structurally, the product comprises a 430 ferritic stainless steel substrate and a black titanium film layer formed on the substrate through electrolytic coloring and high-temperature curing. The core feature of this product is its unique snowflake-like sandblasted texture on its surface, and its chromaticity index is precisely controlled within an extremely narrow range, specifically: L value between 31 and 32, A value between -0.8 and 0, and B value between 0 and 1.2. The L value represents brightness, ranging from 31 to 32; the A value represents reddish-green, and the range of -0.8 to 0 ensures a pure black or slightly cool tone, effectively suppressing reddish tint; the B value represents yellowish-blue, and the range of 0 to 1.2 controls the balance of warm and cool colors. This set of precise chromaticity parameters collectively defines a high-quality, highly consistent sandblasted black titanium appearance.

[0051] Furthermore, to more objectively define the high surface quality of the product, in a preferred embodiment, the surface area occupied by cross-hatching or scratch-like abrasion marks on the product surface is less than 0.5% of the total surface area of ​​the product. This quantitative indicator directly corresponds to the technical problem of unstable surface grinding quality that the method of the present invention aims to solve. By controlling the upper limit of the proportion of undesirable surface defects (such as cross-hatching and scratches) to such an extremely low level of 0.5%, this technical solution, from the perspective of the product, demonstrates the advancement and effectiveness of its gradient grinding and intelligent belt management methods, constituting a strong constraint on the high-quality standard of the product.

[0052] The specific embodiments of the present invention will now be described in more detail with reference to the accompanying drawings.

[0053] Please see Figure 1 This invention demonstrates the basic process of a method for producing sandblasted black titanium from 430 ferritic stainless steel. The method first involves a gradient grinding step S10 on the 430 ferritic stainless steel substrate, designed to impart a uniform initial texture. During grinding, a parallel intelligent belt management step S20 is implemented, ensuring uniform grinding quality by real-time monitoring of the belt status and replacement as needed. After grinding, the substrate enters an electrolytic coloring and color correction step S30, where a black titanium film is formed, and a closed-loop control system ensures color consistency. Finally, a high-temperature curing step S40 enhances the physicochemical properties of the film, yielding the final product.

[0054] The basic embodiment, which contains only the technical features of the independent claims, will now be described. In this embodiment, a method for producing 430 ferritic stainless steel sandblasted titanium is provided. First, a 430 ferritic stainless steel substrate coil is prepared. Then, the coil is fed into a continuous surface treatment production line. The first part of the production line is a gradient grinding unit, such as... Figure 2 As shown, this unit can contain multiple grinding heads connected in series, such as a coarse grinding unit 1, a fine grinding unit 2, and a fine grinding unit 3. The stainless steel substrate passes sequentially through these grinding heads, with the abrasive belts on each head grinding the substrate surface from coarse to fine at different grit sizes. This is the gradient grinding step S10. This design ensures the gradual refinement of the surface texture, laying the foundation for forming a uniform snowflake-like texture.

[0055] While the gradient grinding step S10 is being performed, an intelligent belt abrasive management system (which can be understood as...) is in operation. Figure 1 S20 in the middle is also working. Figure 2As shown, the system is centered around a central controller 4. The central controller 4 monitors the performance parameters of the abrasive belts in each grinding unit (1, 2, 3) in real time. These performance parameters reflect the wear status of the abrasive belts. When the central controller 4 determines that the monitored performance parameter value of a certain abrasive belt deviates from the preset normal range, it means that the abrasive belt may be excessively worn and unable to guarantee grinding quality. At this time, the central controller 4 immediately issues a command to trigger the abrasive belt replacement actuator 8 to replace the corresponding grinding unit with a new abrasive belt. This process is an automated closed-loop control, the principle of which lies in dynamically maintaining the optimal state of the grinding tools through real-time feedback, thereby ensuring a high degree of consistency in the surface texture of the final product.

[0056] After gradient grinding and achieving the required surface quality, the stainless steel substrate is then fed into the second part of the production line, namely the electrolytic coloring and curing system, such as... Figure 3 As shown, the substrate first enters the electrolytic cell 10 for electrolytic coloring and color correction step S30. In the electrolytic cell 10, a black titanium oxide film is generated on the stainless steel surface through an electrochemical reaction. To solve the problems of uneven color and reddish tint, this step adopts a closed-loop control strategy. Specifically, a spectrophotometer 11 is set at the outlet of the electrolytic cell 10, which continuously measures the chromaticity value of the steel strip surface after coloring in real time. The measurement signal is sent to the electrolytic power controller 12. The controller has preset correction rules, which dynamically adjust the electrolytic parameters (such as current, voltage, or waveform) applied to the electrolytic cell 10 according to the deviation between the received real-time chromaticity value and the target chromaticity value. This real-time feedback loop of "measurement-comparison-adjustment" ensures that the color of the entire roll of steel strip can be precisely controlled within a very small tolerance range.

[0057] After coloring, the steel strip immediately enters the high-temperature curing tank 14 to perform the high-temperature curing step S40. In the high-temperature curing tank 14, a chemical solution or environment at a specific temperature heat-treats the newly formed black titanium film. This process promotes the stability and densification of the film's microstructure, significantly enhances the adhesion between the film and the 430 stainless steel substrate, and improves its corrosion resistance and wear resistance. Through the organic combination of the above four steps—gradient grinding, intelligent belt management, closed-loop electrolytic coloring, and high-temperature curing—this method can stably produce sandblasted black titanium products with excellent surface quality, color, and durability on 430 ferritic stainless steel at low cost.

[0058] In a preferred embodiment, based on the above embodiments, the gradient grinding step S10 can be implemented more specifically. For example... Figure 2As shown, the gradient grinding process is specifically a three-stage process, consisting of coarse grinding unit 1, fine grinding unit 2, and fine grinding unit 3. Coarse grinding unit 1 uses 120-grit abrasive belts, fine grinding unit 2 uses 180-grit abrasive belts, and fine grinding unit 3 uses 240-grit abrasive belts. This increasing grit configuration from 120 to 240 is an effective combination for achieving a fine and uniform snowflake-like texture. Its technical advantage lies in the fact that by rationally allocating the cutting tasks of different abrasive belts, it ensures both a high material removal rate and a fine final surface finish. Compared to single-stage grinding or an unreasonable combination of abrasive belts, it can obtain an ideal NO.4 grade surface with higher efficiency and stability, providing a high-quality substrate for subsequently obtaining a uniform black titanium film layer.

[0059] In another preferred embodiment, to meet the specific requirements of applications with extremely high surface texture, the gradient grinding process can add an ultrafine grinding step after fine grinding. For example, in Figure 2 In the grinding line shown, an additional grinding unit using 400-grit abrasive belt can be added after the fine grinding unit 3. The technical advantage of this is that it achieves a surface finish that is finer, more glossy, and smoother to the touch than standard abrasive. This allows the method of this invention to cover a wider range of market demands, from mainstream to high-end, demonstrating the flexibility and scalability of its process route.

[0060] Furthermore, the performance parameters in the intelligent belt abrasive management step S20 are described in detail. In a simple and efficient implementation, the performance parameter can be the grinding current. For example... Figure 2 As shown, each grinding unit (1, 2, 3) has a drive motor equipped with a current sensor 6, which transmits the real-time current value to the central controller 4. When the abrasive belt wears and its cutting ability decreases, the grinding pressure increases to maintain the grinding effect, leading to an increase in motor load and a rise in grinding current. Conversely, if the abrasive belt breaks, the current drops sharply. Therefore, monitoring current changes to determine the abrasive belt condition is a cost-effective and responsive solution. More specifically, a preset nominal operating current (e.g., 60A, an empirical value) can be set. When the absolute value of the real-time value monitored by the current sensor 6 deviates from this nominal value by more than 10% (i.e., exceeding the range of 54A-66A), the central controller 4 determines that the abrasive belt performance is abnormal and triggers a belt replacement. This quantitative threshold judgment automates and standardizes the abrasive belt replacement decision-making process, avoiding the subjectivity and delay of manual judgment. Its technical effect is to significantly improve the batch stability of the abrasive surface quality.

[0061] In another alternative implementation, the performance parameters of intelligent belt sander management can also be more direct surface quality data. For example... Figure 2As shown, an online sanding texture detector 7 can be installed after each grinding unit. This detector uses a high-speed camera and image processing algorithms to directly analyze whether the texture of the steel belt surface after grinding meets the requirements. The technical advantage of this method is that it can capture defects that cannot be reflected by indirect parameters such as current, such as local scratches caused by belt chipping. Therefore, it provides a high level of quality assurance and can minimize the defect rate caused by sanding belt problems. To achieve the most comprehensive sanding belt management, a preferred solution is to combine multiple monitoring methods. Specifically, the conditions for triggering sanding belt replacement can be set as a combination logic: replacement is triggered when the grinding current deviation exceeds 10%, or the online sanding texture detector 7 detects a defect, or the sanding belt usage mileage reaches a preset mileage. Among them, the sanding belt usage mileage is read by the central controller 4 from the sanding belt mileage database 5 and compared with the actual operating mileage. For example, sanding belts of different mesh sizes can have different preset mileages, such as 20,000 meters. This assurance strategy, which combines "real-time performance monitoring" with "planned life management," is effective in addressing both unexpected problems and preventing progressive wear, thus helping to ensure the stability and reliability of the grinding process.

[0062] The electrolytic coloring and color correction step S30 will now be explained in more detail. For example... Figure 3 As shown, the core of this step is to use a reddish correction database 13 to guide the operation of the electrolysis power controller 12. This database 13 stores a large amount of process knowledge; for example, it might record that "when the spectrophotometer 11 detects that the A value rises from -0.5 to 0, the electrolysis current should be reduced from 80A to 75A." When a reddish trend appears on the plate surface during production, the electrolysis power controller 12 no longer adjusts blindly, but instead obtains precise and targeted correction instructions from the reddish correction database 13 and controls the power supply of the electrolytic cell 10. This knowledge-based intelligent control effectively and quickly controls the color difference, especially the A value, within the target range (e.g., achieving -0.8 ≤ A ≤ 0), effectively solving the problem of reddish tint in 430 stainless steel coloring and ensuring high consistency in product color.

[0063] I. Specific Implementation Examples of the Modified Rules The following combination Figure 3 The color control and curing system shown provides a detailed explanation of the correction rules used in the electrolytic coloring and color correction step S30.

[0064] 1.1 Electrolysis Current Correction Rule Based on Colorimetric Deviation On the continuous production line, the spectrophotometer 11 acquires the colorimetric values ​​(L, A, B) of the steel strip surface in real time at a sampling frequency of at least once per second. The electrolysis power controller 12 compares the measured values ​​with the target values ​​(L0=31.5, A0=-0.4, B0=0.6) and adjusts the electrolysis current according to the deviation as shown in Table 1.

[0065] Table 1. Electrolysis current correction rules based on A-value deviation (ΔA= - )

[0066] 1.2 Comprehensive Correction Rules Based on L and B Values Besides the A value, deviations in the L value (brightness) and B value (yellow-blue tint) also affect color quality. Table 2 provides correction rules when considering the deviations in the L and B values.

[0067]

[0068] II. Precise Mathematical Model In a preferred embodiment, the core control logic of the redness correction database 13 is implemented using a multiple linear regression model. This model is obtained by fitting historical production data and can directly calculate the required electrolysis parameter adjustment based on the current chromaticity deviation.

[0069] 2.1 Model Type A multiple linear regression model was adopted, with the deviation values ​​of the three chromaticity channels as input variables and the electrolysis current adjustment and production line speed adjustment as output variables.

[0070] 2.2 Input Variables and Output Variables Input variables: x1 = ΔA = +0.4 (A value deviation) x2 = ΔL = - 31.5 (L value deviation) x3 = ΔB = - 0.6 (B-value deviation) Output variables: y1 = ΔI (Electrolysis current adjustment, unit: A) y2 = Δv (Production line speed adjustment, unit: %) 2.3 Specific Form of the Regression Model The regression equation for the electrolysis current adjustment is: y1 = 5.2·x1 + 0.8·x2 + 1.5·x3 The regression equation for the production line speed adjustment is: y2 = -1.0·x1 + 2.5·x2 + 3.0·x3 Where y1 is a positive value indicating an increase in current and a negative value indicating a decrease in current; y2 is a positive value indicating an increase in speed and a negative value indicating a decrease in speed.

[0071] 2.4 Valid range of the model The effective range of the above regression model is: -1.2 ≤ x1 ≤ 1.2 (i.e., the value of A ranges from -1.6 to 0.8) -2.0 ≤ x2 ≤ 2.0 (i.e., L is between 29.5 and 33.5) -1.5 ≤ x3 ≤ 1.5 (i.e., B values ​​range from -0.9 to 2.1) When the chromaticity deviation exceeds the above range, the control system will first use the segmented rules in Tables 1 and 2 for large-scale open-loop adjustment, and then switch to the regression model for fine closed-loop control after the chromaticity value enters the effective range of the model.

[0072] 2.5 Model Update and Optimization The coefficients of this regression model are not static. As production data accumulates, the electrolysis power controller 12 refits and updates the model coefficients every certain production cycle (e.g., after every 10,000 meters of steel strip produced) using the latest collected data, ensuring that the model always reflects the actual process characteristics of the current production line. The initial coefficients (5.2, 0.8, 1.5, -1.0, 2.5, 3.0) were obtained through prior orthogonal experiments and response surface methodology.

[0073] III. Methods for Establishing a Redness Correction Database The experimental methods and steps for establishing the reddish correction database 13 are described in detail below, so that those skilled in the art can replicate the database without creative effort.

[0074] 3.1 Experimental Design Using a full factorial design combined with response surface methodology, we systematically investigated the effects of three key process parameters—electrolysis current (I), production line speed (v), and electrolyte temperature (T)—on the color values ​​(L, A, B) of the colored product.

[0075] 3.1.1 Factor Level Design

[0076] 3.1.2 Experimental Scheme Using the Box-Behnken design, a total of 15 experiments are required (including 3 sets of center point repeat experiments). The specific experimental scheme is shown in Table 3.

[0077] Table 3 Box-Behnken Experimental Design

[0078] 3.2 Experimental Materials and Equipment 3.2.1 Substrate Preparation 430W ferritic stainless steel coils with a thickness of 0.8 mm were selected and pretreated according to the gradient grinding step S10 described in this invention to obtain a snowflake-textured substrate with a consistent surface texture. The pretreated coils were cut into 200 mm × 300 mm test pieces. Test pieces cut from adjacent portions of the same coil were used in each batch of experiments to eliminate the influence of substrate differences on the experimental results. Three parallel test pieces were prepared under each experimental condition, and the average of their colorimetric measurements was taken as the representative value under that condition.

[0079] 3.2.2 Electrolytic coloring solution formulation The electrolytic coloring solution uses a chromic acid-sulfuric acid system, and the concentrations of each component are controlled as follows: Hexavalent chromium (as CrO3): 110-130 g / L Sulfuric acid (H2SO4): 450-550 g / L Additives (optional): as needed 3.2.3 Measuring equipment A spectrophotometer (such as X-Rite Ci64 or equivalent precision) was used for measurement with a D65 light source, a 10° viewing angle, and SCI (including specular reflection) mode. Measurements were taken at no fewer than five different locations for each sample, and the average value was used as the representative colorimetric value for that sample.

[0080] 3.3 Experimental Data Acquisition Following the experimental scheme in Table 3, electrolytic coloring experiments were conducted one by one. After each group of experiments was completed, the L, A, and B values ​​of the sample were immediately measured using a spectrophotometer, and the corresponding process parameter combinations (I, v, T) were recorded. The experimental data are summarized in Table 4 (the data in the table are exemplary data, and should be re-measured according to the specific production line conditions in actual production).

[0081] Table 4. Examples of Experimental Data Recording

[0082] 3.4 Data Analysis and Model Fitting 3.4.1 Response Surface Analysis Using the experimental data above, a quadratic polynomial regression model was used to fit the L, A, and B values ​​respectively. Taking the A value as an example, its response surface model is as follows: A = β0+ β1·I + β2·v + β3·T + β 12 ·I·v + β 13 ·I·T + β 23 ·v·T + β 11 ·I² + β 22 ·v² + β 33 ·T² The coefficient estimates are obtained by fitting using the least squares method (example data):

[0083] 3.4.2 Derivation of the Modification Rule Based on the above response surface model, the required parameter adjustment amount when the measured colorimetric value deviates from the target value can be derived. The specific method is as follows: For the current combination of process parameters (I0, v0, T0), if the measured value of A... Deviation from target value (=-0.4), then by taking the partial derivative with respect to the response surface model, the current adjustment ΔI required to make the value of A return to the target value is calculated: ΔI ≈ ( - ) / ( A / I) in A / I = β1 + β 12 ·v + β 13 ·T + 2β 11 ·I.

[0084] The above derivation results, together with the segmentation rules in Tables 1-2 and the regression model in Section 2.3, constitute the core content of the redness correction database 13.

[0085] 3.5 Database Validation and Optimization 3.5.1 Verification Experiment After completing the model fitting, five sets of process parameter combinations that were not involved in the modeling were randomly selected for verification experiments. The chromaticity values ​​predicted by the model were compared with the measured values. If the average prediction error (|predicted value - measured value|) exceeded 0.3 chromaticity units, the experimental data needed to be re-examined or experimental points needed to be added to refit the model.

[0086] 3.5.2 Production Validation The initially established reddish correction database 13 was deployed to the electrolytic power controller 12 for trial production for no less than 8 consecutive hours (or no less than 500 meters of steel strip). During the trial production, the triggering conditions, adjustment amount, and corrected chromaticity value for each color correction were recorded. If the corrected chromaticity value remained stable within the target range (31≤L≤32, -0.8≤A≤0, 0≤B≤1.2) in three consecutive measurements, the database was deemed valid; otherwise, the rules and model coefficients in the database were corrected based on the trial production data, and the verification was repeated until the target was met.

[0087] 3.5.3 Dynamic Updates of the Database The reddish correction database 13 is not static. As production batches increase (it is recommended to update the database every 10,000 meters of accumulated production or every quarter), the database is updated using the newly acquired production data: newly collected data pairs (process parameters, chromaticity values) are incorporated into the dataset, response surface analysis or regression fitting is re-performed, and model coefficients and correction rules are updated. This dynamic update mechanism ensures that the database can adaptively reflect the impact of long-term drift factors such as electrolyte aging and electrode state changes on the coloring effect, thereby maintaining the accuracy of color control over the long term.

[0088] For the high-temperature curing step S40, its process parameters are crucial to the final film performance. In a preferred embodiment, the temperature within the high-temperature curing tank 14 is controlled between 85-118°C. This temperature range is an effective process window to ensure good adhesion and corrosion resistance of the black titanium film on 430W stainless steel (a specific substrate with a thickness between 0.3-1.5 mm). To further improve film performance, a more preferred two-stage curing process can be employed. Specifically, the high-temperature curing tank 14 can be designed with two temperature zones, or two curing tanks connected in series can be used. The steel strip first enters the low-temperature zone of 85-95°C for preliminary curing to release internal stress in the film; then it enters the high-temperature zone of 110-118°C for final curing to fully densify the film structure. This staged heating curing strategy achieves the technical advantage of obtaining a film with lower internal stress and higher density than single-stage isothermal curing, thereby significantly improving the long-term reliability indicators of the product, such as salt spray resistance and wear resistance.

[0089] This invention also provides a 430 ferritic stainless steel sandblasted black titanium product prepared by the above method. Structurally, this product consists of a 430 ferritic stainless steel substrate and a black titanium film layer on its surface. Its unique value lies in its precisely defined appearance and quality. First, its surface exhibits a uniform and delicate snowflake sandblasted texture, thanks to the aforementioned gradient grinding and intelligent sanding belt management. Second, its color is strictly defined; measured by a spectrophotometer, its chromaticity indicators meet the following requirements: luminance L value between 31 and 32 (31≤L≤32), red-green hue A value between -0.8 and 0 (-0.8≤A≤0), and yellow-blue hue B value between 0 and 1.2 (0≤B≤1.2). This set of parameters collectively defines a deep, pure, and non-reddish black. Finally, the product has extremely high surface quality, with the surface area occupied by defects such as cross-grain or scratch-like sandblasting controlled to less than 0.5% of the total product surface area. These characteristics together constitute a high-quality, highly consistent, and highly reliable decorative material product.

[0090] The following describes an embodiment integrating multiple preferred technical features to demonstrate the synergistic effect of the various inventive points. In this embodiment, a 0.8mm thick 430W ferritic stainless steel coil is selected as the substrate. First, the substrate undergoes pretreatment such as precision rolling and bright annealing. Then, it proceeds as follows... Figure 2 The gradient grinding line shown is equipped with three grinding units: a coarse grinding unit 1 with a 120-gauge abrasive belt, a fine grinding unit 2 with a 180-gauge abrasive belt, and a fine grinding unit 3 with a 240-gauge abrasive belt. The steel belt travels at a speed of 18 m / min, and the grinding current of each grinding unit is controlled between 55-65 A. The central controller 4 simultaneously monitors the grinding current of each unit (via current sensor 6) and the used mileage of the abrasive belt (referencing the abrasive belt mileage database 5). If the current of any unit deviates from the set center value by more than 10%, or its mileage reaches 20,000 meters, the abrasive belt replacement actuator 8 is triggered, completing the automatic replacement.

[0091] The steel belt that has been ground enters as follows Figure 3 The coloring and curing line is shown. First, the strip passes through an electrolytic cell 10, with the coloring acid parameters controlled within the following ranges: hexavalent chromium concentration 110-130 g / L, sulfuric acid concentration 450-550 g / L. A spectrophotometer 11 continuously monitors the color of the strip surface. Once an A value is detected to be trending towards 0, the electrolytic power controller 12 immediately queries the reddish correction database 13 and adjusts it according to the returned instructions (e.g., reducing the electrolytic current by 5A) until the A value returns to the target range of [-0.8, 0]. After coloring, the steel strip continuously enters a two-stage high-temperature curing tank 14. The first stage is at 90°C for 20 seconds for preliminary curing; the second stage is at 115°C for another 20 seconds for final curing.

[0092] This embodiment combines several preferred technical features, including specific three-stage gradient grinding, intelligent sanding belt management based on dual monitoring of current and mileage, closed-loop color control based on a reddish correction database, and two-stage high-temperature curing, to achieve significant comprehensive technical effects. First, precise grinding and intelligent management ensure a high-quality snowflake-like sand base; second, the knowledge-based color control system achieves reddish-free and highly consistent coloring on this high-quality base; finally, the two-stage curing process endows the film layer with excellent adhesion and durability. These interconnected and synergistic technical features ultimately enable the large-scale production of high-quality sandblasted black titanium decorative materials on low-cost 430 stainless steel, achieving a good balance between quality, efficiency, and cost.

[0093] The 430 ferritic stainless steel sandblasted titanium product produced by this invention has broad application prospects due to its excellent performance, aesthetic value, and cost advantages. In the household appliance field, it can be used to manufacture refrigerator door panels, range hood shells, microwave oven panels, etc. Its unique sandblasted texture is resistant to fingerprints and easy to clean, while the ferromagnetic nature of its substrate facilitates the magnetic installation of internal components. In the architectural decoration field, it can be used as elevator car interior walls, door frames, skirting boards, and wall panels and column edging in shopping malls and hotels. Its uniform color and texture ensure high consistency in large-area applications, while its excellent wear resistance and corrosion resistance ensure aesthetics and durability for long-term use in public places. Furthermore, its cost advantage compared to 304 stainless steel products makes it possible to replace the price-sensitive 304 black titanium in large-scale projects.

Claims

1. A method for producing sandblasted black titanium for 430 ferritic stainless steel, characterized in that, Includes the following steps: gradient Grinding steps: The surface of the 430 ferritic stainless steel substrate is treated with a gradient grinding process, which includes coarse grinding, fine grinding and fine grinding in sequence, using abrasive belts; Electrolytic coloring and color correction steps: The ground stainless steel substrate is subjected to electrolytic coloring treatment, and the color difference is controlled in a closed loop by real-time monitoring of product color and adjustment of electrolytic parameters according to preset correction rules. High-temperature curing step: The stainless steel substrate that has been electrolytically colored is subjected to high-temperature curing treatment; During the gradient grinding process, the performance parameters of the abrasive belt are monitored in real time. When the monitored value of the performance parameter deviates from the preset range, the abrasive belt is replaced.

2. The method according to claim 1, characterized in that, The gradient grinding process is a three-stage gradient grinding process, which uses a No. 120 abrasive belt for coarse grinding, a No. 180 abrasive belt for fine grinding, and a No. 240 abrasive belt for fine grinding.

3. The method according to claim 1, characterized in that, The gradient grinding process includes an ultrafine grinding step after fine grinding, using a 400-grit abrasive belt.

4. The method according to claim 1, characterized in that, The performance parameter is the grinding current.

5. The method according to claim 4, characterized in that, The deviation of the monitored value of the performance parameter from the preset range means that: a preset nominal working current is set, and when the absolute value of the deviation between the real-time value of the grinding current and the preset nominal working current exceeds 10% of the preset nominal working current.

6. The method according to claim 1, characterized in that, The conditions for triggering the replacement of the sanding belt also include: when the usage mileage of the sanding belt reaches a preset mileage, the sanding belt replacement is triggered.

7. The method according to claim 1, characterized in that, The electrolytic coloring and color correction steps include: obtaining the preset correction rules from a reddish correction database.

8. The method according to claim 1, characterized in that, The high-temperature curing step includes: preliminary curing at 85-95°C, followed by final curing at 110-118°C.

9. The method according to claim 1, characterized in that, The 430 ferritic stainless steel substrate is 430W ferritic stainless steel with a thickness of 0.3-1.5mm.

10. A 430 ferritic stainless steel sandblasted titanium product, characterized in that, The products include: 430 ferritic stainless steel substrate; and A black titanium film layer is formed on the substrate; The product has a snowflake sand texture on its surface, and its colorimetric index is: L value between 31 and 32, A value between -0.8 and 0, and B value between 0 and 1.2.