Iron-silicon-aluminum magnetic powder core, preparation method and application thereof
By forming an Al2O3+SiO2 insulating layer on the surface of iron-silicon-aluminum alloy powder and precipitating α-Fe in the inner layer, the problems of magnetic loss and insulation performance of iron-silicon-aluminum magnetic powder cores were solved, and iron-silicon-aluminum magnetic powder cores with low loss, high DC bias and high saturation magnetization were realized.
Patent Information
- Application Number
- CN202611073259.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-20
- Publication Date
- 2026-11-10
AI Technical Summary
The magnetic loss of existing iron-silicon-aluminum magnetic powder cores is limited by the performance of the insulating layer on the particle surface. Furthermore, existing coating methods suffer from insufficient heat resistance, low interfacial bonding strength, and poor uniformity of the insulating layer, making it difficult to achieve a synergistic improvement in soft magnetic properties.
Iron-silicon-aluminum alloy powder was modified by oxygen plasma to form an Al2O3+SiO2 insulating layer on its surface and α-Fe was precipitated in the inner layer, thus constructing an Al2O3+SiO2+α-Fe composite structure. After high-temperature annealing, a high-temperature resistant insulating layer was formed.
Significantly reduces magnetic loss, improves DC bias performance and saturation magnetization, and enhances overall soft magnetic performance.
Smart Images

Figure CN123072867A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of soft magnetic materials technology, specifically relating to an iron-silicon-aluminum magnetic powder core, its preparation method, and its application. Background Technology
[0002] Soft magnetic composite materials are a new type of soft magnetic material prepared by coating soft magnetic alloy powder with an insulating layer, followed by pressing and heat treatment. Because the magnetic particles are isolated by the insulating layer, a large number of uniformly distributed air gaps are formed inside the material, giving it advantages such as high resistivity, low eddy current loss, and good DC bias performance. It is widely used in high-frequency electromagnetic devices such as power supplies for new energy vehicles, high-frequency inductors, photovoltaic inverters, 5G communications, data centers, and artificial intelligence servers.
[0003] Currently, commonly used magnetic powders for soft magnetic composite materials include crystalline alloy powders (carbonyl iron powder, iron-silicon powder, iron-silicon-aluminum alloy powder, iron-nickel alloy powder, etc.) and amorphous / nanocrystalline alloy powders. Our research group previously filed patent CN 120473280 A, which discloses an amorphous composite magnetic powder core modified by argon-oxygen plasma discharge, its preparation method, and its applications. This invention patent, through a well-designed argon-oxygen flow rate ratio, obtains an oxide + α-Fe double-cluster structure (<5nm) on the surface of the amorphous powder. Although this structure reduces magnetic loss to some extent, the reduction is limited. Furthermore, amorphous powders are more expensive than crystalline iron-silicon-aluminum alloy powders, making comprehensive engineering applications difficult. Iron-silicon-aluminum alloy powders, due to their low price and high resistivity, low core loss, and excellent high-frequency soft magnetic properties, can balance permeability and magnetic loss performance, and have become one of the most widely used soft magnetic materials in the field of magnetic powder cores, with broad application prospects in switching power supplies, power inductors, automotive electronics, electric vehicles, energy storage systems, and consumer electronics.
[0004] However, the magnetic loss of iron-silicon-aluminum magnetic powder cores is still limited by the performance of the insulating layer on the particle surface. Currently, the coating methods used in preparing iron-silicon-aluminum magnetic powder cores are mainly divided into organic coating, inorganic coating, and organic-inorganic coating. However, the insulating layers prepared by these methods generally suffer from insufficient heat resistance, easy decomposition or damage during heat treatment, low interfacial bonding strength, and poor uniformity. When high-temperature annealing is used to eliminate compressive stress, the insulating layer is prone to failure, leading to increased interparticle conductivity, decreased material resistivity, and increased eddy current losses. Furthermore, while excessively increasing the insulating agent content can reduce losses and improve DC bias performance, it also leads to a decrease in permeability and saturation magnetization, making it difficult to achieve a synergistic improvement in soft magnetic properties. It is well known that α-Fe has a higher saturation magnetization than iron-silicon-aluminum, and Al2O3 and SiO2 are often used as inorganic coating agents due to their high resistivity. Developing a novel surface modification method for iron-silicon-aluminum powder that can produce a uniform and high-temperature resistant insulating layer would have significant theoretical and engineering application value for further improving the overall soft magnetic properties of iron-silicon-aluminum magnetic powder cores. Summary of the Invention
[0005] To address the shortcomings and deficiencies of existing technologies, the primary objective of this invention is to provide an Al₂O₃+SiO₂ magnetic powder core. This core has an Al₂O₃+SiO₂ insulating layer formed on its powder surface, with α-Fe precipitated in the inner layer, constructing an Al₂O₃+SiO₂+α-Fe composite structure. Compared to existing magnetic powder cores, this Al₂O₃+SiO₂ magnetic powder core exhibits reduced losses, improved DC bias performance, and increased magnetization.
[0006] The second objective of this invention is to provide a method for preparing an iron-silicon-aluminum magnetic powder core. Specifically, the method involves placing iron-silicon-aluminum alloy powder into a stainless steel ball mill jar without grinding balls, evacuating the jar, and introducing an oxygen atmosphere. High-energy electrons, ions, and reactive oxygen free radicals bombard the powder, creating a localized, instantaneous high temperature in a micro-region. Due to Al's affinity for oxygen, Al atoms in the inner layer of the iron-silicon-aluminum alloy powder migrate to the outer layer, while Fe and Si atoms in the outer layer migrate to the inner layer. The instantaneous electron temperature in the plasma interaction region is high, but it cannot provide the energy for atomic motion, thus forming an amorphous Al₂O₃ layer on the surface of the iron-silicon-aluminum alloy powder. After high-temperature annealing, an Al₂O₃+SiO₂ insulating layer forms on the surface of the modified iron-silicon-aluminum alloy powder, and α-Fe precipitates in the inner layer. The Al₂O₃+SiO₂ significantly reduces the loss of the iron-silicon-aluminum magnetic powder core and improves DC bias performance. The formation of α-Fe also increases the saturation magnetization of the iron-silicon-aluminum magnetic powder core.
[0007] The third objective of this invention is to provide the application of the aforementioned iron-silicon-aluminum magnetic powder core in electronic devices in the medium- and high-frequency fields.
[0008] The primary objective of this invention is achieved through the following technical solution:
[0009] A type of iron-silicon-aluminum magnetic powder core has a powder size of 2–150 μm. An Al2O3+SiO2 insulating layer is formed on the powder surface of the core, and α-Fe is precipitated in the inner layer, forming an Al2O3+SiO2+α-Fe composite structure. The thickness of the Al2O3+SiO2 insulating layer is 10–100 nm, and the thickness of the α-Fe is 10–50 nm.
[0010] The second objective of this invention is achieved through the following technical solution:
[0011] A method for preparing an iron-silicon-aluminum magnetic powder core includes the following steps:
[0012] (1) The iron-silicon-aluminum alloy powder is modified by oxygen plasma, then mixed with insulating resin to form a mixed powder, then mixed with organic solvent, dried to form an insulating coated powder, and finally mixed with lubricant to prepare an insulating resin coated iron-silicon-aluminum alloy composite powder.
[0013] (2) Iron-silicon-aluminum alloy composite powder coated with insulating resin is warm-pressed and heat-treated to prepare iron-silicon-aluminum magnetic powder core.
[0014] Preferably, the iron-silicon-aluminum alloy powder in step (1) has the chemical formula Fe. x Si y Al z Where x is 84.5~86.5, y is 8.5~10, and z is 5.0~6.5; the average particle size of the iron-silicon-aluminum alloy powder is 10~150μm.
[0015] Preferably, the average particle size of the iron-silicon-aluminum alloy powder in step (1) is 10-100 μm, more preferably 10-75 μm.
[0016] Preferably, the oxygen plasma modification treatment in step (1) is carried out in a stainless steel ball mill jar without grinding balls, and oxygen is introduced into the stainless steel ball mill jar at a flow rate of 0.2 to 2 L / min, so that the pressure of the mixed gas in the ball mill jar is 0.05 to 0.5 MPa; more preferably, the flow rate of the oxygen is 0.8 to 1.2 L / min, and the pressure of the oxygen is 0.1 to 0.2 MPa.
[0017] Preferably, the duration of the oxygen plasma modification treatment in step (1) is 0.25 to 2.5 h; more preferably 0.5 to 2.25 h; and most preferably 0.75 to 2 h.
[0018] Preferably, the parameters of the oxygen plasma modification treatment in step (1) are: frequency 5-9kHz, current 90-110mA, voltage 4-5kV, power 400-500W, and motor speed 500-1300rpm; more preferably, the parameters of the plasma modification treatment are: frequency 7.5-8kHz, current 100-103mA, voltage 4.2-4.5kV, power 420-480W, and motor speed 900-1000rpm.
[0019] Preferably, in step (1), the mass ratio of the iron-silicon-aluminum alloy powder to the insulating resin is 100:(1-4), the mass ratio of the organic solvent to the mixed powder is 1-5:1, and the mass ratio of the lubricant to the insulating coating powder is 0.5-1:100.
[0020] Preferably, the mass ratio of the iron-silicon-aluminum alloy powder to the insulating resin in step (1) is 100:(2-4); more preferably, it is 100:(2-3).
[0021] Preferably, the insulating resin in step (1) is at least one of silicone resin, phenolic resin and epoxy modified resin; the organic solvent is at least one of acetone and anhydrous ethanol; and the lubricant is zinc stearate.
[0022] Preferably, the mass ratio of the organic solvent to the mixed powder is 2 to 3:1.
[0023] Preferably, the temperature of the warm pressing in step (2) is 100~180℃, the pressure is 600~900MPa, and the holding time is 5~10s; more preferably, the temperature of the warm pressing is 120~150℃, the pressure is 700~800MPa, and the holding time is 5~6s.
[0024] Preferably, the heat treatment annealing temperature in step (2) is 500-800°C and the time is 0.5-3h; more preferably, the heat treatment annealing temperature is 700-750°C and the time is 0.5-1h.
[0025] The third objective of this invention is achieved through the following technical solution:
[0026] Application of an iron-silicon-aluminum magnetic powder core in the fabrication of inductive components.
[0027] Preferably, the inductor is used in fields such as new energy vehicles, photovoltaic inverters, AI servers, communication power supplies, consumer electronics, industrial power supplies, energy storage systems, and home appliances.
[0028] The mechanism of the iron-silicon-aluminum magnetic powder core described in this invention is as follows:
[0029] This invention utilizes oxygen plasma modification to obtain an Al2O3+SiO2+α-Fe microstructure from iron-silicon-aluminum alloy powder. After coating with a coating agent, the powder is pressed and sintered to obtain an iron-silicon-aluminum magnetic powder core with high saturation magnetization, high DC bias, and low loss. During the oxygen plasma modification process, high-energy electrons, ions, and reactive oxygen radicals bombard the powder. Due to Al's affinity for oxygen, Al atoms in the inner layer of the iron-silicon-aluminum alloy powder migrate to the outer layer, while Fe and Si atoms migrate to the inner layer. The plasma treatment region experiences instantaneous high temperatures, but this cannot maintain the kinetic energy driven by the atoms, thus forming an amorphous Al2O3 layer on the surface of the iron-silicon-aluminum alloy powder. After high-temperature annealing, an Al2O3+SiO2 insulating layer forms on the surface of the modified iron-silicon-aluminum alloy powder, and α-Fe precipitates in the inner layer. The resistivity of the generated Al2O3+SiO2 insulating layer is higher than that of the untreated iron-silicon-aluminum magnetic powder core. Therefore, the modified iron-silicon-aluminum magnetic powder core exhibits reduced loss and improved DC bias performance. In addition, the modified iron-silicon-aluminum magnetic powder core precipitates α-Fe, which increases the saturation magnetization.
[0030] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0031] (1) This invention modifies iron-silicon-aluminum alloy powder with oxygen plasma to obtain an Al2O3+SiO2 insulating layer on its surface, which can improve the resistivity of the iron-silicon-aluminum magnetic powder core, reduce the loss of the magnetic powder core, and solve the problems of organic coating not being resistant to high temperature and inorganic coating having weak adhesion.
[0032] (2) The present invention modifies iron-silicon-aluminum alloy powder with oxygen plasma to obtain α-Fe in the inner layer, thereby improving the saturation magnetization of the iron-silicon-aluminum magnetic powder core.
[0033] (3) Compared with iron-silicon-aluminum magnetic powder cores without oxygen plasma modification and composite magnetic powder cores with other modification treatments, the iron-silicon-aluminum magnetic powder cores prepared in this invention have improved DC bias performance by 35.9% to 68%, reduced magnetic loss by 35.9% to 68%, and increased saturation magnetic flux density by 3.0% to 7.0%;
[0034] (4) The iron-silicon-aluminum magnetic powder core of the present invention can use iron-silicon-aluminum alloy powder of various compositions. The process is simple, environmentally friendly and low cost. At the same time, it can significantly reduce magnetic loss, improve DC bias performance and saturation magnetization intensity, and achieve a balance of comprehensive soft magnetic properties, which has broad application prospects. Attached Figure Description
[0035] Figure 1 This is a schematic diagram of the microstructure of the oxygen plasma modified iron-silicon-aluminum alloy powder in this invention.
[0036] Figure 2The image shows the microstructure of the iron-silicon-aluminum alloy powder surface after oxygen plasma modification in Example 1. As can be seen from the image, the powder surface is amorphous Al2O3 with a thickness of about 20 nm, and the interior is FeSiAl powder.
[0037] Figure 3 The image shows the microstructure of the iron-silicon-aluminum alloy powder modified by oxygen plasma in Example 1 after high-temperature annealing. As can be seen from the image, the outer two layers of the powder are Al2O3+SiO2 insulating layers with a thickness of about 20 nm, the inner α-Fe layer with a thickness of about 10 nm, and the innermost layer is FeSiAl.
[0038] Figure 4 The graph shows a comparison of the magnetic losses of the magnetic powder cores corresponding to Example 1 and Comparative Example 1.
[0039] Figure 5 This is a comparison diagram of the saturation magnetization of the magnetic powder cores corresponding to Example 1 and Comparative Example 1;
[0040] Figure 6 This is a comparison chart of the DC bias performance of the magnetic powder cores corresponding to Example 1 and Comparative Example 1. Detailed Implementation
[0041] The present invention will be further described in detail below with reference to the embodiments and accompanying drawings, but the implementation of the present invention is not limited thereto.
[0042] Unless otherwise specified in the embodiments of this invention, the conditions shall be performed according to conventional conditions or conditions recommended by the manufacturer. All raw materials and reagents used, unless otherwise specified, are commercially available conventional products.
[0043] Example 1
[0044] A method for preparing an iron-silicon-aluminum magnetic powder core includes the following steps:
[0045] (1) Oxygen plasma modification treatment: Fe with an average particle size of 75 μm was modified. 84.5 Si 10 Al5 alloy powder was added to a stainless steel ball mill jar without grinding balls; the ball mill jar was evacuated, and oxygen was introduced into the ball mill jar at a flow rate of 1.0 L / min to make the atmosphere pressure of the ball mill jar 0.1 MPa; the parameters of plasma modification treatment were: frequency 7.5 kHz, current 100 mA, voltage 4.2 kV, power 450 W, motor speed 950 rpm, and discharge time 1 h.
[0046] (2) Mixed coating: The oxygen plasma modified iron-silicon-aluminum alloy powder (50g) in step (1) is mixed with organosilicon resin (1g) to form a mixed powder, and then acetone is added and stirred; the mass ratio of the iron-silicon-aluminum alloy powder to organosilicon resin is 100:2, and the mass ratio of the mixed powder to acetone is 1:2; the stirring time is 45min, and after stirring, it is dried in a drying oven at 80℃ for 1h to obtain insulating coated powder; finally, 0.5wt.% (by mass of mixed powder) of zinc stearate is added to the dried insulating coated powder and stirred for 2h to prepare organosilicon resin coated iron-silicon-aluminum alloy composite powder;
[0047] (3) Warm pressing: The iron-silicon-aluminum alloy composite powder coated with organosilicon resin in step (3) is pressed into an iron-silicon-aluminum magnetic powder core blank at a temperature of 120°C and a pressure of 750MPa for 6 seconds.
[0048] (4) Heat treatment annealing: The iron-silicon-aluminum magnetic powder core green blank is annealed at 750°C for 1 hour in a vacuum environment to prepare the iron-silicon-aluminum magnetic powder core.
[0049] The iron-silicon-aluminum magnetic powder core obtained in this embodiment has an Al2O3+SiO2 insulating layer on the powder surface and an α-Fe inner layer. The Al2O3+SiO2 insulating layer is approximately 20 nm thick. The loss of the iron-silicon-aluminum magnetic powder core is 105.62 kW / m. 3 (50 mT, 100 kHz), DC bias of 51% (100 Oe), saturation magnetization of 139.1 emu / g. Compared with the untreated iron-silicon-aluminum magnetic powder core (Comparative Example 1), this embodiment shows a 68% reduction in loss, a 96.2% increase in DC bias, and a 7% increase in saturation magnetization.
[0050] Example 2
[0051] A method for preparing an iron-silicon-aluminum magnetic powder core includes the following steps:
[0052] (1) Oxygen plasma modification treatment: Fe with an average particle size of 20 μm was modified. 85.5 Si9Al 5.5 Iron-silicon-aluminum alloy powder was added to a stainless steel ball mill jar without grinding balls; the ball mill jar was evacuated, and oxygen was introduced into the ball mill jar at a flow rate of 1.2 L / min to make the atmosphere pressure inside the ball mill jar 0.2 MPa; the parameters for plasma modification treatment were: frequency 8 kHz, current 100 mA, voltage 4.5 kV, power 480 W, motor speed 1000 rpm, and discharge time 1.5 h;
[0053] (2) Mixed coating: The iron-silicon-aluminum alloy powder (50g) modified by oxygen plasma in step (1) was mixed with organosilicon resin (0.5g) to form a mixed powder. Acetone was then added and stirred. The mass ratio of the iron-silicon-aluminum alloy powder to the organosilicon resin was 100:1, and the mass ratio of the mixed powder to the acetone was 1:3. The stirring time was 60min. After stirring, the powder was dried in a drying oven at 60℃ for 2h to obtain an insulating coated powder. Finally, 0.5wt% (by mass of the mixed powder) of zinc stearate was added to the dried insulating coated powder and stirred for 3h to prepare an organosilicon resin coated iron-silicon-aluminum alloy composite powder.
[0054] (3) Warm pressing: The iron-silicon-aluminum alloy composite powder coated with organosilicon resin in step (3) is pressed for 10 seconds at a temperature of 150°C and a pressure of 800MPa to form an iron-silicon-aluminum magnetic powder core blank.
[0055] (4) Heat treatment annealing: The iron-silicon-aluminum magnetic powder core green blank is annealed at 800℃ for 0.75h in a vacuum environment to prepare the iron-silicon-aluminum magnetic powder core.
[0056] The iron-silicon-aluminum magnetic powder core obtained in this embodiment has an Al2O3+SiO2 insulating layer, α-Fe, and nanoparticles on its powder surface. The Al2O3+SiO2 insulating layer is approximately 30 nm thick. The loss of the iron-silicon-aluminum magnetic powder core is 230.85 kW / m. 3 (50 mT, 100 kHz), DC bias of 30% (100 Oe), saturation magnetization of 135.5 emu / g. Compared with the untreated iron-silicon-aluminum magnetic powder core (Comparative Example 2), this embodiment shows a 41% reduction in loss, a 26% increase in DC bias, and a 1.5% increase in saturation magnetization.
[0057] Example 3
[0058] A method for preparing an iron-silicon-aluminum magnetic powder core includes the following steps:
[0059] (1) Oxygen plasma modification treatment: Fe with an average particle size of 50 μm was modified. 86.5 Si 8.5 Al5 iron-silicon-aluminum alloy powder was added to a stainless steel ball mill jar without grinding balls; the ball mill jar was evacuated, and oxygen was introduced into the ball mill jar at a flow rate of 0.8 L / min to make the atmosphere pressure of the ball mill jar 0.5 MPa; the parameters for plasma modification treatment were: frequency 8 kHz, current 103 mA, voltage 4.5 kV, power 420 W, motor speed 1000 rpm, and discharge time 2 h.
[0060] (2) Mixed coating: The iron-silicon-aluminum alloy powder (50g) modified by oxygen plasma in step (1) was mixed with organosilicon resin (1.5g) to form a mixed powder. Acetone was then added and stirred. The mass ratio of the iron-silicon-aluminum alloy powder to the organosilicon resin was 100:3, and the mass ratio of the mixed powder to the acetone was 1:4. The stirring time was 75min. After stirring, the powder was dried in a drying oven at 100℃ for 0.5h to obtain an insulating coated powder. Finally, 0.5wt% (by mass of the mixed powder) of zinc stearate was added to the dried insulating coated powder and stirred for 3h to prepare an organosilicon resin coated iron-silicon-aluminum alloy composite powder.
[0061] (3) Warm pressing: The iron-silicon-aluminum alloy composite powder coated with organosilicon resin in step (3) is pressed for 10 seconds at a temperature of 180℃ and a pressure of 900MPa to form an iron-silicon-aluminum magnetic powder core blank.
[0062] (4) Heat treatment annealing: The iron-silicon-aluminum magnetic powder core green blank is annealed at 550°C for 1 hour in a vacuum environment to prepare the iron-silicon-aluminum magnetic powder core.
[0063] In this embodiment, the iron-silicon-aluminum magnetic powder core obtained by the above method has an Al2O3+SiO2 insulating layer and α-Fe on its powder surface, with the Al2O3+SiO2 insulating layer having a thickness of approximately 25 nm. The loss of the iron-silicon-aluminum composite magnetic powder core is 210.3 kW / m. 3 (50 mT, 100 kHz), DC bias of 35% (100 Oe), saturation magnetization of 137.6 emu / g. Compared with the unmodified iron-silicon-aluminum magnetic powder core (Comparative Example 3), this embodiment shows a 19% reduction in loss, an 8% increase in DC bias, and a 5% increase in saturation magnetization.
[0064] Comparative Example 1
[0065] Compared with Example 1, the difference of this comparative example is that the operations of steps (1) to (2) are not performed, and the operations of steps (3) to (5) are performed directly, that is, the oxygen plasma modification treatment is not performed.
[0066] The loss of the iron-silicon-aluminum composite magnetic powder core obtained by the above method in this comparative example is 335.53 kW / m. 3 (50 mT, 100 kHz), DC bias of 26.5% (100 Oe), saturation magnetization of 129.3 emu / g.
[0067] Comparative Example 2
[0068] Compared with Example 2, the difference is that steps (1) to (2) are not performed, and steps (3) to (5) are performed directly, that is, oxygen plasma modification treatment is not performed.
[0069] The loss of the iron-silicon-aluminum composite magnetic powder core obtained by the above method in this comparative example is 390.82 kW / m. 3 (50 mT, 100 kHz), DC bias of 22.3% (100 Oe), saturation magnetization of 133.1 emu / g.
[0070] Comparative Example 3
[0071] Compared with Example 3, the difference is that steps (1) to (2) are not performed, and steps (3) to (5) are performed directly, that is, oxygen plasma modification treatment is not performed.
[0072] The loss of the iron-silicon-aluminum composite magnetic powder core obtained by the above method in this comparative example is 260.5 kW / m. 3 (50 mT, 100 kHz), DC bias of 32.5% (100 Oe), saturation magnetization of 130.4 emu / g.
[0073] The soft magnetic properties of the iron-silicon-aluminum magnetic powder cores prepared in the above embodiments and comparative examples were tested, and the results are as follows:
[0074] Table 1 compares the test results of soft magnetic powder cores in Examples 1-3 and Comparative Examples 1-3.
[0075] <![CDATA[Magnetic loss (kW / m 3 ) @ (50 mT, 100 kHz)]]> DC bias (%) @ 100 Oe Saturation magnetization (emu / g) Example 1 105.62 51 139.1 Example 2 230.85 30 135.5 Example 3 210.3 35 137.6 Comparative Example 1 335.53 26.5 129.3 Comparative Example 2 390.82 22.3 133.1 Comparative Example 3 260.5 32.5 130.4
[0076] Saturation magnetization, DC bias performance, and iron loss are key indicators for evaluating the comprehensive soft magnetic properties of magnetic powder cores. Among them, saturation magnetization determines the load-carrying capacity of the magnetic powder core, DC bias performance determines its ability to maintain stable permeability under high current conditions, and iron loss determines the energy loss level of the magnetic powder core under high-frequency operating conditions. These three indicators jointly determine the comprehensive application performance of magnetic powder cores in high-frequency power electronic devices, such as power supply inductors and high-power converters. As shown in Table 1, comparing Examples 1 to 3 and Comparative Examples 1 to 3, it can be seen that the loss is reduced by 19% to 68%, the DC bias performance is improved by 26% to 96.2%, and the saturation magnetization is improved by 1.5% to 7%. This invention effectively synergistically optimizes the performance of magnetic cores, including iron-silicon-aluminum alloy magnetic powder cores, which will significantly expand the application fields of iron-silicon-aluminum alloy magnetic powder cores.
[0077] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A type of iron-silicon-aluminum magnetic powder core, characterized in that, The powder size is 2-150 μm; an Al2O3+SiO2 insulating layer is formed on the powder surface of the iron-silicon-aluminum magnetic powder core, and α-Fe is precipitated in the inner layer, forming an Al2O3+SiO2+α-Fe composite structure; the thickness of the Al2O3+SiO2 insulating layer is 10-100 nm, and the thickness of the α-Fe is 10-50 nm.
2. The method for preparing the iron-silicon-aluminum magnetic powder core according to claim 1, characterized in that, Includes the following steps, (1) The iron-silicon-aluminum alloy powder is modified by oxygen plasma, then mixed with insulating resin to form a mixed powder, then mixed with organic solvent, dried to form an insulating coated powder, and finally mixed with lubricant to prepare an insulating resin coated iron-silicon-aluminum alloy composite powder. (2) Iron-silicon-aluminum alloy composite powder coated with insulating resin is warm-pressed and heat-treated to prepare iron-silicon-aluminum magnetic powder core.
3. The method for preparing the iron-silicon-aluminum magnetic powder core according to claim 2, characterized in that, The iron-silicon-aluminum alloy powder mentioned in step (1) has the chemical formula Fe. x Si y Al z Where x is 84.5~86.5, y is 8.5~10, and z is 5.0~6.5; the average particle size of the iron-silicon-aluminum alloy powder is 10~150μm.
4. The method for preparing the iron-silicon-aluminum magnetic powder core according to claim 2, characterized in that, The specific method of oxygen plasma modification treatment in step (1) is as follows: it is carried out in a stainless steel ball mill jar without grinding balls. Oxygen is introduced into the stainless steel ball mill jar at a flow rate of 0.2 to 2 L / min, so that the pressure of the mixed gas in the ball mill jar is 0.05 to 0.5 MPa.
5. The method for preparing the iron-silicon-aluminum magnetic powder core according to claim 2, characterized in that, The duration of the oxygen plasma modification treatment in step (1) is 0.25 to 2.5 hours.
6. The method for preparing the iron-silicon-aluminum magnetic powder core according to claim 2, characterized in that, The parameters for the oxygen plasma modification treatment in step (1) are: frequency 5-9kHz, current 90-110mA, voltage 4-5kV, power 400-500W, and motor speed 500-1300rpm.
7. The method for preparing the iron-silicon-aluminum magnetic powder core according to claim 2, characterized in that, In step (1), the mass ratio of the iron-silicon-aluminum alloy powder to the insulating resin is 100:(1-4), the mass ratio of the organic solvent to the mixed powder is 1-5:1, and the mass ratio of the lubricant to the insulating coating powder is 0.5-1:
100.
8. The method for preparing the iron-silicon-aluminum magnetic powder core according to claim 2, characterized in that, The insulating resin mentioned in step (1) is at least one of silicone resin, phenolic resin and epoxy modified resin; the organic solvent is at least one of acetone and anhydrous ethanol; and the lubricant is zinc stearate.
9. The method for preparing the iron-silicon-aluminum magnetic powder core according to claim 2, characterized in that, The temperature for warm pressing in step (2) is 100~180℃, the pressure is 600~900MPa, and the holding time is 5~10s.
10. The method for preparing the iron-silicon-aluminum magnetic powder core according to claim 2, characterized in that, The heat treatment annealing temperature in step (2) is 500-800℃ and the time is 0.5-3h.
11. The application of the iron-silicon-aluminum magnetic powder core according to claim 1 in the preparation of inductive components.
12. The application according to claim 11, characterized in that, The inductor components are used in fields such as new energy vehicles, photovoltaic inverters, AI servers, communication power supplies, consumer electronics, industrial power supplies, energy storage systems, and home appliances.
Citation Information
Patent Citations
Amorphous composite magnetic powder core based on argon oxygen plasma discharge modification and preparation method and application thereof
CN120473280A