A flip-chip light-emitting diode and its fabrication method

By improving the electrode pad structure of flip-chip LEDs and employing multi-layer gradient conductive materials and magnetron sputtering technology, the heat dissipation and shock resistance issues of flip-chip LEDs in automotive lighting have been solved, achieving improved high-efficiency heat dissipation and shock resistance.

CN123076076APending Publication Date: 2026-11-10JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611424911.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Flip-chip LEDs present heat dissipation and vibration resistance issues in automotive lighting applications. Traditional pad structures cannot effectively conduct heat and are prone to micro-deformation and poor contact under vibration.

Method used

The structure employs a composite reflective layer, insulating layer, and electrode pads. The electrode pads include a multi-layered Ti metal layer, a nano-diamond and nano-silver composite pad layer, and a gold-tin alloy layer. A gradient conductive structure is formed by magnetron sputtering to improve heat dissipation and shock resistance.

Benefits of technology

This improves the chip's heat dissipation efficiency and shock resistance, extends the chip's lifespan, and ensures stability and reliability in automotive applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076076A_ABST
    Figure CN123076076A_ABST
Patent Text Reader

Abstract

This invention relates to the field of semiconductor device technology, specifically to a flip-chip light-emitting diode (LED) and its fabrication method. The electrode pads of the flip-chip comprise a first pad layer, a second pad layer, a third pad layer, and a fourth pad layer stacked along the epitaxial direction. The first pad layer is a Ti metal layer. The second pad layer comprises at least two composite pad layers, each made of nanodiamond and nanosilver, with the weight content of nanodiamond decreasing progressively along the epitaxial direction in the at least two composite pad layers. The third pad layer comprises a third Ti metal layer and a third Pt metal layer periodically and alternately stacked along the epitaxial direction. The fourth pad layer is made of a gold-tin alloy. This invention improves the chip's heat dissipation efficiency while ensuring conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor device technology, and in particular to a flip-chip light-emitting diode and its fabrication method. Background Technology

[0002] Flip-chip LEDs are a special type of LED product in the semiconductor device field. They are light-emitting diode chips with electrodes arranged on the opposite side of the light-emitting surface of the chip, using a back-emitting light design. The back-emitting light structure can avoid the electrodes blocking the light and greatly improve the light extraction efficiency.

[0003] Due to the high reliability of flip-chip LED lamps, they can maintain stable light intensity for extended periods, making them suitable for automotive lighting. This ensures that the lamps meet road lighting brightness requirements throughout their entire lifespan, preventing insufficient illumination caused by rapid light decay. Simultaneously, flip-chip LED lamps have high luminous efficiency and consume significantly less energy than traditional halogen lamps, reducing vehicle energy consumption and meeting the fuel economy requirements of gasoline vehicles and the range demands of new energy vehicles. Therefore, in recent years, they have gradually become the mainstream application solution in the automotive lighting field, replacing traditional halogen and xenon lamps.

[0004] However, its application in automotive lighting also presents challenges related to heat dissipation and vibration resistance. During vehicle use, headlights often require prolonged high-power operation, especially at night when driving with high beams on, which continuously outputs large currents and generates a significant amount of heat in a short period. Simultaneously, vehicles experience continuous bumps and vibrations under various road conditions, coupled with the continuous vibration transmission from the engine compartment itself, placing demands on the chip's resistance to deformation far exceeding those of ordinary civilian lighting.

[0005] Traditional flip-chip LED pads use only conventional metal stacking structures and do not have specially designed high thermal conductivity composite heat dissipation channels. The heat generated during operation cannot be quickly and efficiently conducted to the external packaging substrate, which can easily lead to heat accumulation and excessive junction temperature. At the same time, the overall strength of the metal material of conventional pads is relatively low. Under the continuous vibration of vehicles, the internal structure of the chip is prone to micro-deformation, which can lead to failure problems such as poor contact and interlayer delamination after long-term operation. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of the prior art. This invention provides a flip-chip light-emitting diode and its preparation method. The prepared chip improves the heat dissipation rate while maintaining conductivity, and has good shock resistance.

[0007] To address the aforementioned issues, this invention proposes a flip-chip light-emitting diode, comprising an epitaxial wafer, a current spreading layer, a current blocking layer, and an electrode structure sequentially stacked on the epitaxial wafer. The electrode structure includes a composite reflective layer, an insulating layer, and an electrode pad. The composite reflective layer and the insulating layer are disposed below the electrode pad. The electrode pad includes a first pad layer, a second pad layer, a third pad layer, and a fourth pad layer stacked along the epitaxial direction. The first pad layer is a Ti metal layer; The second pad layer includes at least two composite pad layers, each of which is made of nanodiamond and nanosilver, and the weight content of nanodiamond in the at least two composite pad layers decreases layer by layer along the epitaxial direction. The third pad layer includes a third Ti metal layer and a third Pt metal layer that are periodically and alternately stacked along the epitaxial direction; The fourth pad layer is made of gold-tin alloy.

[0008] As an improvement to the above technical solution, the thickness of the first pad layer is 3nm~5nm; The thickness of the second pad layer is 5μm~7μm; The third pad layer includes a third Ti metal layer and a third Pt metal layer that are periodically and alternately stacked along the epitaxial direction, with a period number ≥ 2; The thickness of the third Ti metal layer is 100nm~200nm, and the thickness of the third Pt metal layer is 100nm~200nm; The thickness of the fourth pad layer is 1μm~3μm, and the mass ratio of Au to Su is 1:0.25.

[0009] As an improvement to the above technical solution, the weight content of nanodiamonds in the composite solder pad layer is 4% to 16%, and the weight content of nanodiamonds in the multilayer composite solder pad layer decreases linearly along the epitaxial direction.

[0010] As an improvement to the above technical solution, the second pad layer is prepared by the following method: Deposition was performed using magnetron sputtering at a temperature of 80℃~120℃, a deposition pressure of 0.3Pa~0.6Pa, an Ar discharge gas, and a flow rate of 30sccm~50sccm. The discharge gas is introduced to bombard the high-purity silver target and the nanodiamond target, and the bombardment power of bombarding the high-purity silver target and the nanodiamond target is adjusted during the deposition of each layer of the composite solder pad. The bombardment power of the nanodiamond target decreases layer by layer, while the bombardment power of the high-purity silver target increases layer by layer.

[0011] As an improvement to the above technical solution, the bombardment power of the nanodiamond target is 20W~125W, and the bombardment power of the high-purity silver target is 190W~310W.

[0012] As an improvement to the above technical solution, the second pad layer includes a first composite pad layer, a second composite pad layer and a third composite pad layer stacked sequentially along the epitaxial direction. The thickness ratio of the second composite solder pad layer to the first composite solder pad layer is 1:1 to 1:2, and the thickness ratio of the third composite solder pad layer to the second composite solder pad layer is 1:1 to 1:2. The weight content of nanodiamonds in the first composite solder pad layer is 14%~16%; The weight content of nanodiamonds in the second composite solder pad layer is 9%~10%; The weight content of nanodiamonds in the third composite solder pad layer is 4%~5%.

[0013] As an improvement to the above technical solution, the composite reflective layer includes a Bragg reflective layer and a metal reflective layer stacked sequentially. The Bragg reflector layer comprises periodically alternating layers of TiO2 and SiO2, with a period number of 3 to 5. The metal reflective layer has an Ag / Ti / Ni / Pt / Ti / Ni / Pt / Ti structure; The insulating layer includes a first insulating layer and a second insulating layer; The first insulating layer is composed of a stack of Al2O3 and SiO2 thin films, and the second insulating layer is composed of a SiO2 thin film.

[0014] Accordingly, the present invention also provides a method for fabricating a flip-chip light-emitting diode, comprising the following steps: Provide epitaxial wafers; A current spreading layer is deposited on the epitaxial wafer; A current blocking layer is deposited on the current spreading layer; An electrode structure is deposited on the current blocking layer; wherein the electrode structure includes a composite reflective layer, an insulating layer, and electrode pads; The electrode pads include a first pad layer, a second pad layer, a third pad layer, and a fourth pad layer stacked along the epitaxial direction; The first pad layer is a Ti metal layer; The second pad layer includes at least two composite pad layers, which are made of nanodiamond and nanosilver, and the weight content of nanodiamond in the at least two composite pad layers decreases layer by layer along the epitaxial direction. The third pad layer includes a third Ti metal layer and a third Pt metal layer that are periodically and alternately stacked along the epitaxial direction; The fourth pad layer is made of gold-tin alloy.

[0015] As an improvement to the above technical solution, the method for preparing the electrode pad includes the following steps: The device is placed in the reaction chamber, and the first and second pad layers are deposited by magnetron sputtering. The method for preparing the second pad layer includes the following steps: Ar was introduced as the discharge gas at a flow rate of 30 sccm to 50 sccm. The deposition temperature was controlled at 80℃ to 120℃ and the deposition pressure was controlled at 0.3 Pa to 0.6 Pa. The discharge gas bombarded the high-purity silver target and the nanodiamond target. The bombardment power of the high-purity silver target and the nanodiamond target during the deposition of each composite solder pad layer is adjusted. The bombardment power of the nanodiamond target decreases layer by layer, while the bombardment power of the high-purity silver target increases layer by layer. A third pad layer and a fourth pad layer are sequentially deposited on the second pad layer.

[0016] As an improvement to the above technical solution, the bombardment power of the nanodiamond target is 20W~125W, and the bombardment power of the high-purity silver target is 190W~310W. The implementation of this invention has the following beneficial effects: This invention improves the electrode pads in the electrode structure. Specifically, the electrode pads include a first pad layer, a second pad layer, a third pad layer, and a fourth pad layer stacked along the epitaxial direction.

[0017] (1) The first pad layer is a Ti metal layer, which enhances the adhesion between the electrode pads and the epitaxial wafer, thereby improving the chip's shock resistance; (2) The second pad layer includes at least two composite pad layers, which are made of nanodiamond and nanosilver. The weight content of nanodiamond in the at least two composite pad layers decreases layer by layer along the epitaxial direction. While ensuring conductivity, the diamond skeleton transfers the chip heat to the substrate after soldering, improving the chip heat dissipation capacity. At the same time, the high strength of the diamond can also suppress the micro-deformation of the chip during operation. (3) The third pad layer includes a third Ti metal layer and a third Pt metal layer that are periodically and alternately stacked along the epitaxial direction; the Ti metal and Pt metal can effectively prevent the diffusion and migration of Ag metal in the second pad layer. (4) The fourth pad layer is made of gold-tin alloy and is used to weld with the subsequent packaging substrate to improve its welding and fixing function with the packaging substrate, thereby improving its shock resistance when used in automobiles and increasing its service life when used in automobiles. Attached Figure Description

[0018] Figure 1This is a schematic diagram of the structure of a flip-chip light-emitting diode according to an embodiment of the present invention; Figure 2 This is a schematic diagram of the electrode pads of a flip-chip light-emitting diode according to an embodiment of the present invention; Figure 3 This is a schematic diagram of the third pad layer of a flip-chip light-emitting diode according to an embodiment of the present invention; Figure 4 This is a schematic diagram of the composite reflective layer of a flip-chip light-emitting diode according to an embodiment of the present invention; Figure 5 This is a schematic diagram of the insulating layer of a flip-chip light-emitting diode according to an embodiment of the present invention. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings.

[0020] See Figures 1 to 5 As shown, an embodiment of the present invention provides a flip-chip light-emitting diode, including an epitaxial wafer 100, a current spreading layer 200, a current blocking layer 300 and an electrode structure 400 sequentially stacked on the epitaxial wafer 100.

[0021] Specifically, the electrode structure 400 includes a composite reflective layer 410, an insulating layer 420, and an electrode pad 430. The composite reflective layer 410 and the insulating layer 420 are disposed below the electrode pad 430. The electrode pad 430 includes a first pad layer 431, a second pad layer 432, a third pad layer 433, and a fourth pad layer 434 stacked along the epitaxial direction. The first pad layer 431 is a Ti metal layer; See Figure 2 As shown, the second pad layer 432 includes at least two composite pad layers 432a, which are made of nanodiamond and nanosilver, and the weight content of nanodiamond in the at least two composite pad layers 432a decreases layer by layer along the epitaxial direction. See Figure 3 As shown, the third pad layer 433 includes a third Ti metal layer 433a and a third Pt metal layer 433b that are periodically and alternately stacked along the epitaxial direction; The fourth pad layer 434 is made of a gold-tin alloy.

[0022] The first pad layer 431 is a Ti metal layer, which enhances the adhesion between the electrode pad 430 and the epitaxial wafer 100, thereby improving the chip's shock resistance.

[0023] The second pad layer 432 employs a composite material of nanodiamond and nanosilver, with a structure where the weight content of nanodiamond decreases layer by layer along the epitaxial direction, significantly improving thermal management efficiency. Nanodiamond has high thermal conductivity, far exceeding that of conventional metals, which, combined with the conductivity of nanosilver, forms a highly efficient heat conduction channel. The higher weight content of nanodiamond near the epitaxial wafer directly absorbs the heat generated by the chip, and the layer-by-layer decreasing design achieves stepped heat diffusion, avoiding localized heat accumulation. The gradient structure optimizes the matching of thermal expansion coefficients, reducing interfacial thermal resistance.

[0024] The third pad layer 433 features an alternating Ti / Pt structure, with periodically stacked Ti and Pt metal layers providing excellent mechanical stability. The high strength of Ti and the corrosion resistance of Pt complement each other, and the alternating stacking suppresses the propagation of microcracks caused by vibration. The Ti layer acts as a buffer layer to absorb stress, while the Pt layer prevents electrochemical corrosion, thus improving the overall resistance of the pads to deformation. The multilayer design increases the interface bonding area and reduces the risk of interlayer delamination.

[0025] Preferably, the thickness of the first pad layer 431 is 3nm to 5nm; the thickness of the first pad layer 431 can be 3nm, 3.2nm, 3.8nm, 4.3nm, 4.5nm, or 5nm, but is not limited to these.

[0026] The first pad layer 431 serves as an adhesion layer, enhancing the bond between the epitaxial wafer 100 and the upper metal layer and preventing peeling. When the thickness of the first pad layer 431 is less than 3 nm, the adhesion is insufficient, and delamination is likely under high-temperature operation, leading to increased contact resistance or open-circuit failure. When the thickness of the first pad layer 431 is greater than 5 nm, the excessively thick Ti layer has high resistivity, increasing the overall electrode impedance and reducing current spreading efficiency.

[0027] The thickness of the second pad layer 432 is 5μm to 7μm; the thickness of the second pad layer 432 can be 5μm, 5.3μm, 5.8μm, 6.2μm, 6.8μm, 7μm, but is not limited to these.

[0028] The second pad layer 432 serves as the core heat dissipation layer, with gradient-designed nanodiamonds providing an ultra-high thermal conductivity path. When the thickness of the second pad layer 432 is less than 5μm, the heat capacity is insufficient, failing to effectively dissipate the heat generated by the large current, leading to an increase in device temperature. When the thickness of the second pad layer 432 is greater than 7μm, excessive thickness causes thermal stress concentration, making the device prone to cracking after prolonged use.

[0029] The third pad layer 433 includes a third Ti metal layer 433a and a third Pt metal layer 433b that are periodically and alternately stacked along the epitaxial direction, with a period number ≥ 2; the period number can be 2, 3, 4, 5, 6, 7, 8, or 9, but is not limited to these.

[0030] The thickness of the third Ti metal layer 433a is 100nm~200nm, and the thickness of the third Pt metal layer 433b is 100nm~200nm. The thickness of the third Ti metal layer 433a can be 100nm, 110nm, 125nm, 135nm, 155nm, 186nm, 195nm, or 200nm, but is not limited to these values. The thickness of the third Pt metal layer 433b can be 100nm, 110nm, 125nm, 135nm, 155nm, 186nm, 195nm, or 200nm, but is not limited to these values.

[0031] The third Ti metal layer 433a buffers stress, the third Pt metal layer 433b inhibits electron migration, and the alternating structure of Ti and Pt metal layers improves fatigue resistance.

[0032] The fourth pad layer 434 is made of an alloy of Au and Su, and the thickness of the fourth pad layer 434 is 1μm to 3μm, with a weight ratio of Au to Su of 1:0.25. The thickness of the fourth pad layer 434 can be 1μm, 1.4μm, 1.7μm, 2.3μm, 2.9μm, or 3μm, but is not limited to these.

[0033] Au provides oxidation resistance, while Sn enables eutectic bonding, and the weight ratio ensures reliability during low-temperature reflow soldering. When the thickness of the fourth pad layer 434 is less than 1μm, insufficient solder leads to excessive void ratio, increased thermal resistance, and susceptibility to cracking. When the thickness of the fourth pad layer 434 is greater than 3μm, the excessive solder expands under heat, compressing adjacent pads and causing bridging short circuits.

[0034] Preferably, the weight content of nanodiamond in the composite solder pad layer 432a is 4% to 16%, and the weight content of nanodiamond in the multilayer composite solder pad layer 432a decreases linearly along the epitaxial direction.

[0035] When the weight content of nanodiamond in the composite pad layer 432a is less than 4%, an effective heat conduction path cannot be formed, resulting in a sharp drop in thermal conductivity, which leads to an increase in chip junction temperature and accelerated optical decay. When the weight content of nanodiamond in the composite pad layer 432a is greater than 16%, the excessive diamond blocks the conductive path of the silver substrate, causing a significant increase in resistivity, which in turn increases the driving voltage and energy consumption.

[0036] More preferably, the second pad layer 432 is prepared by the following method: Deposition was performed using magnetron sputtering at a temperature of 80℃~120℃, a deposition pressure of 0.3Pa~0.6Pa, an Ar discharge gas, and a flow rate of 30sccm~50sccm. The discharge gas is introduced to bombard the high-purity silver target and the nanodiamond target, and the bombardment power of each composite solder pad layer 432a is adjusted during deposition. The bombardment power of the nanodiamond target decreases layer by layer, while the bombardment power of the high-purity silver target increases layer by layer.

[0037] The above preparation method directly achieves a linear decrease in nanodiamond content from the chip side to the substrate side by adjusting the diamond target power to decrease layer by layer and the silver target power to increase layer by layer, forming a continuously transitioning composite material gradient structure.

[0038] The bombardment power of the nanodiamond target is 20W~125W, and the bombardment power of the high-purity silver target is 190W~310W.

[0039] The bombardment power of nanodiamond targets can be 20W, 50W, 70W, 100W, 110W, or 125W, but is not limited to these values. The bombardment power of high-purity silver targets can be 210W, 250W, 270W, 290W, 300W, or 310W, but is not limited to these values.

[0040] In some embodiments of the present invention, the second pad layer 432 is composed of three composite pad layers 432a stacked along the epitaxial direction. The second pad layer 432 includes a first composite pad layer, a second composite pad layer and a third composite pad layer stacked sequentially along the epitaxial direction. The thickness ratio of the second composite solder pad layer to the first composite solder pad layer is 1:1 to 1:2, and the thickness ratio of the third composite solder pad layer to the second composite solder pad layer is 1:1 to 1:2. The weight content of nanodiamonds in the first composite solder pad layer is 14%~16%; The weight content of nanodiamonds in the second composite solder pad layer is 9%~10%; The weight content of nanodiamonds in the third composite solder pad layer is 4%~5%.

[0041] See Figure 4 As shown, in some embodiments, the composite reflective layer 410 includes a Bragg reflective layer 411 and a metal reflective layer 412 stacked sequentially. The Bragg reflector layer 410 comprises periodically alternating layers of TiO2 and SiO2, with a period number of 3 to 5. The metal reflective layer 412 has an Ag / Ti / Ni / Pt / Ti / Ni / Pt / Ti structure; The insulating layer 420 includes a first insulating layer 421 and a second insulating layer 422; The first insulating layer 421 is composed of a stack of Al2O3 and SiO2 thin films, and the second insulating layer 422 is composed of a SiO2 thin film.

[0042] See Figures 1 to 5 As shown, the present invention also provides a method for fabricating a flip-chip light-emitting diode, comprising the following steps: Provide 100 epitaxial wafers; Specifically, a substrate 110 is provided, and an N-type GaN layer 120, an active light-emitting layer 130, and a P-type GaN layer 140 are sequentially grown on the substrate 110 along the epitaxial direction to obtain an epitaxial wafer 100; A current spreading layer 200 is deposited on the epitaxial wafer 100; A current blocking layer 300 is deposited on the current spreading layer 200; An electrode structure 400 is deposited on the current blocking layer 300; wherein the electrode structure 400 includes a composite reflective layer 410, an insulating layer 420, and an electrode pad 430. Specifically, the composite reflective layer 410 includes a Bragg reflective layer 411 and a metal reflective layer 412 stacked sequentially; the insulating layer 420 includes a first insulating layer 421 and a second insulating layer 422. The electrode pad 430 includes a first pad layer 431, a second pad layer 432, a third pad layer 433 and a fourth pad layer 434 stacked along the extension direction; The first pad layer 431 is a Ti metal layer; The second pad layer 432 includes at least two composite pad layers 432a, which are made of nanodiamond and nanosilver, and the weight content of nanodiamond in the at least two composite pad layers 432a decreases layer by layer along the epitaxial direction. The third pad layer 433 includes a third Ti metal layer 433a and a third Pt metal layer 433b that are periodically and alternately stacked along the epitaxial direction; The fourth pad layer 434 is made of a gold-tin alloy.

[0043] Preferably, the method for preparing the electrode pad 430 includes the following steps: The device is placed in the reaction chamber, and the first pad layer 431 and the second pad layer 432 are deposited by magnetron sputtering. The method for preparing the second pad layer 432 includes the following steps: Ar was introduced as the discharge gas at a flow rate of 30 sccm to 50 sccm. The deposition temperature was controlled at 80℃ to 120℃ and the deposition pressure was controlled at 0.3 Pa to 0.6 Pa. The discharge gas bombarded the high-purity silver target and the nanodiamond target. The bombardment power of the high-purity silver target and the nanodiamond target during the deposition of each composite solder pad layer 432a is adjusted. The bombardment power of the nanodiamond target decreases layer by layer, while the bombardment power of the high-purity silver target increases layer by layer. A third pad layer 433 and a fourth pad layer 434 are sequentially deposited on the second pad layer 432.

[0044] More preferably, the bombardment power of the nanodiamond target is 20W~125W, and the bombardment power of the high-purity silver target is 190W~310W.

[0045] The present invention will be further described below through specific embodiments.

[0046] Example 1 (1) This embodiment provides a flip-chip light-emitting diode, including an epitaxial wafer, a current spreading layer, a current blocking layer and an electrode structure are stacked sequentially on the epitaxial wafer; The electrode structure includes a composite reflective layer, an insulating layer, and an electrode pad, wherein the composite reflective layer and the insulating layer are disposed below the electrode pad; The composite reflective layer comprises a Bragg reflective layer and a metallic reflective layer stacked sequentially. The Bragg reflector layer comprises periodically alternating layers of TiO2 and SiO2, with a period number of 4. The metal reflective layer has an Ag / Ti / Ni / Pt / Ti / Ni / Pt / Ti structure; The insulating layer includes a first insulating layer and a second insulating layer; The first insulating layer is composed of a stack of Al2O3 and SiO2 thin films, and the second insulating layer is composed of a SiO2 thin film; The electrode pads include a first pad layer, a second pad layer, a third pad layer, and a fourth pad layer stacked along the epitaxial direction; The first pad layer is a Ti metal layer with a thickness of 4nm; The second pad layer is composed of three composite pad layers stacked together, wherein the composite pad layers are made of nano-diamond and nano-silver; The second pad layer includes a first composite pad layer, a second composite pad layer, and a third composite pad layer stacked sequentially along the epitaxial direction; The weight content of nanodiamond in the first composite solder pad layer is 15%; The weight content of nanodiamonds in the second composite solder pad layer is 10%; The nanodiamond content of the third composite solder pad layer is 5% by weight; The thickness of the second pad layer is 6μm, the thickness ratio of the second composite pad layer to the first composite pad layer is 1:1, and the thickness ratio of the third composite pad layer to the second composite pad layer is 1:1. The third pad layer includes a third Ti metal layer and a third Pt metal layer that are periodically and alternately stacked along the epitaxial direction, with a period number of 2; The thickness of the third Ti metal layer is 150 nm, and the thickness of the third Pt metal layer is 150 nm; The fourth pad layer is made of gold-tin alloy and has a thickness of 2μm; The weight ratio of Au to Su in the fourth pad layer is 1:0.25.

[0047] (2) A method for fabricating a flip-chip light-emitting diode is also provided, wherein the method for fabricating the electrode pads includes the following steps: The device is placed in the reaction chamber, and the first and second pad layers are deposited by magnetron sputtering. The method for preparing the second pad layer includes the following steps: Ar was introduced as the discharge gas at a flow rate of 40 sccm, the deposition temperature was controlled at 100℃, and the deposition pressure was controlled at 0.5 Pa. The discharge gas bombarded the high-purity silver target and the nanodiamond target. The bombardment power of the nanodiamond target material of the first composite solder pad layer is 120W, and the bombardment power of the high-purity silver target material is 200W. The bombardment power of the nanodiamond target material of the second composite solder pad layer is 75W, and the bombardment power of the high-purity silver target material is 260W. The bombardment power of the nanodiamond target in the third composite solder pad layer is 25W, and the bombardment power of the high-purity silver target is 310W.

[0048] Example 2 The difference between this embodiment and Embodiment 1 is that: The second pad layer is composed of two composite pad layers stacked together, the composite pad layers being made of nanodiamond and nanosilver; The second pad layer includes a first composite pad layer and a second composite pad layer stacked sequentially along the epitaxial direction; The weight content of nanodiamonds in the first composite solder pad layer is 14%; The weight content of nanodiamonds in the second composite solder pad layer is 10%; The thickness of the second pad layer is 6μm, and the thickness ratio of the second composite pad layer to the first composite pad layer is 1:2. The method for preparing the second pad layer includes the following steps: Ar was introduced as the discharge gas at a flow rate of 40 sccm, the deposition temperature was controlled at 100℃, and the deposition pressure was controlled at 0.5 Pa. The discharge gas bombarded the high-purity silver target and the nanodiamond target. The bombardment power of the nanodiamond target material of the first composite solder pad layer is 115W, and the bombardment power of the high-purity silver target material is 190W. The bombardment power of the nanodiamond target in the second composite solder pad layer is 65W, and the bombardment power of the high-purity silver target is 260W.

[0049] Example 3 The difference between this embodiment and Embodiment 1 is that: The second pad layer consists of eight composite pad layers stacked along the epitaxial direction. The weight content of nanodiamond in the multilayer composite pad layer decreases linearly from 12% to 6%, and the thickness of the second pad layer is 7μm.

[0050] Example 4 The difference between this embodiment and Embodiment 1 is that: The second pad layer is composed of three composite pad layers stacked together, and the composite pad layers are made of nano-diamond and nano-silver; specifically, the second pad layer includes a first composite pad layer, a second composite pad layer and a third composite pad layer stacked sequentially along the epitaxial direction. The thickness of the first composite solder pad layer is 4 μm; The thickness of the second composite solder pad layer is 2 μm; The thickness of the third composite solder pad layer is 1 μm; The thickness of the second pad layer is 7 μm, the thickness ratio of the second composite pad layer to the first composite pad layer is 1:2, and the thickness ratio of the third composite pad layer to the second composite pad layer is 1:2.

[0051] Comparative Example 1 The difference between this comparative example and Example 1 is as follows: The electrode pads are made of an Al metal layer with a thickness of 8 μm.

[0052] Examples 1 to 4, and Comparative Example 1, were fabricated into flip-chip LEDs with dimensions of 1400 μm × 1400 μm. The junction temperature of the chips was measured by applying a 1500 mA current at an ambient temperature of 85°C.

[0053] The junction temperature test results are shown in the table below:

[0054] Referring to the test results above, the second pad layer includes at least two composite pad layers, which are made of nanodiamond and nanosilver. The weight content of nanodiamond in the multiple composite pad layers decreases layer by layer along the epitaxial direction. While ensuring conductivity, the diamond framework transfers the chip heat to the substrate after soldering, thereby improving the chip's heat dissipation capability.

[0055] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A flip-chip light-emitting diode, characterized in that, It includes an epitaxial wafer, a current spreading layer, a current blocking layer and an electrode structure sequentially stacked on the epitaxial wafer; The electrode structure includes a composite reflective layer, an insulating layer, and an electrode pad. The composite reflective layer and the insulating layer are disposed below the electrode pad. The electrode pad includes a first pad layer, a second pad layer, a third pad layer, and a fourth pad layer stacked along the epitaxial direction. The first pad layer is a Ti metal layer; The second pad layer includes at least two composite pad layers, each of which is made of nanodiamond and nanosilver, and the weight content of nanodiamond in the at least two composite pad layers decreases layer by layer along the epitaxial direction. The third pad layer includes a third Ti metal layer and a third Pt metal layer that are periodically and alternately stacked along the epitaxial direction; The fourth pad layer is made of gold-tin alloy.

2. The flip-chip LED as described in claim 1, characterized in that, The thickness of the first pad layer is 3nm~5nm; The thickness of the second pad layer is 5μm~7μm; The third pad layer includes a third Ti metal layer and a third Pt metal layer that are periodically and alternately stacked along the epitaxial direction, with a period number ≥ 2; The thickness of the third Ti metal layer is 100nm~200nm, and the thickness of the third Pt metal layer is 100nm~200nm; The thickness of the fourth pad layer is 1μm~3μm, and the mass ratio of Au to Su is 1:0.

25.

3. The flip-chip LED as described in claim 1, characterized in that, The weight content of nanodiamonds in the composite solder pad layer is 4% to 16%, and the weight content of nanodiamonds in the multilayer composite solder pad layer decreases linearly along the epitaxial direction.

4. The flip-chip LED as described in claim 2, characterized in that, The second pad layer is prepared by the following method: Deposition was performed using magnetron sputtering at a temperature of 80℃~120℃, a deposition pressure of 0.3Pa~0.6Pa, an Ar discharge gas, and a flow rate of 30sccm~50sccm. The discharge gas is introduced to bombard the high-purity silver target and the nanodiamond target, and the bombardment power of bombarding the high-purity silver target and the nanodiamond target is adjusted during the deposition of each layer of the composite solder pad. The bombardment power of the nanodiamond target decreases layer by layer, while the bombardment power of the high-purity silver target increases layer by layer.

5. The flip-chip LED as described in claim 4, characterized in that, The bombardment power of the nanodiamond target is 20W~125W, and the bombardment power of the high-purity silver target is 190W~310W.

6. The flip-chip light-emitting diode as described in claim 2, characterized in that, The second pad layer includes a first composite pad layer, a second composite pad layer, and a third composite pad layer stacked sequentially along the epitaxial direction; The thickness ratio of the second composite solder pad layer to the first composite solder pad layer is 1:1 to 1:2, and the thickness ratio of the third composite solder pad layer to the second composite solder pad layer is 1:1 to 1:

2. The weight content of nanodiamonds in the first composite solder pad layer is 14%~16%; The weight content of nanodiamonds in the second composite solder pad layer is 9%~10%; The weight content of nanodiamonds in the third composite solder pad layer is 4%~5%.

7. The flip-chip light-emitting diode as described in claim 1, characterized in that, The composite reflective layer comprises a Bragg reflective layer and a metallic reflective layer stacked sequentially. The Bragg reflector layer comprises periodically alternating layers of TiO2 and SiO2, with a period number of 3 to 5. The metal reflective layer has an Ag / Ti / Ni / Pt / Ti / Ni / Pt / Ti structure; The insulating layer includes a first insulating layer and a second insulating layer; The first insulating layer is composed of a stack of Al2O3 and SiO2 thin films, and the second insulating layer is composed of a SiO2 thin film.

8. A method for fabricating a flip-chip light-emitting diode as described in any one of claims 1 to 7, characterized in that, Includes the following steps: Provide epitaxial wafers; A current spreading layer is deposited on the epitaxial wafer; A current blocking layer is deposited on the current spreading layer; An electrode structure is deposited on the current blocking layer; wherein the electrode structure includes a composite reflective layer, an insulating layer, and electrode pads; The electrode pads include a first pad layer, a second pad layer, a third pad layer, and a fourth pad layer stacked along the epitaxial direction; The first pad layer is a Ti metal layer; The second pad layer includes at least two composite pad layers, which are made of nanodiamond and nanosilver, and the weight content of nanodiamond in the at least two composite pad layers decreases layer by layer along the epitaxial direction. The third pad layer includes a third Ti metal layer and a third Pt metal layer that are periodically and alternately stacked along the epitaxial direction; The fourth pad layer is made of gold-tin alloy.

9. The method for fabricating a flip-chip light-emitting diode as described in claim 8, characterized in that, The method for preparing the electrode pads includes the following steps: The device is placed in the reaction chamber, and the first and second pad layers are deposited by magnetron sputtering. The method for preparing the second pad layer includes the following steps: Ar was introduced as the discharge gas at a flow rate of 30 sccm to 50 sccm. The deposition temperature was controlled at 80℃ to 120℃ and the deposition pressure was controlled at 0.3 Pa to 0.6 Pa. The discharge gas bombarded the high-purity silver target and the nanodiamond target. The bombardment power of the high-purity silver target and the nanodiamond target during the deposition of each composite solder pad layer is adjusted. The bombardment power of the nanodiamond target decreases layer by layer, while the bombardment power of the high-purity silver target increases layer by layer. A third pad layer and a fourth pad layer are sequentially deposited on the second pad layer.

10. The method for fabricating a flip-chip light-emitting diode as described in claim 9, characterized in that, The bombardment power of the nanodiamond target is 20W~125W, and the bombardment power of the high-purity silver target is 190W~310W.