A protective diaper and its preparation method

By surface treatment and loading modification of barium titanate, and combined with long-chain quaternary ammonium salt finishing, an antibacterial surface layer is formed and combined with other layers of the diaper. This solves the problems of leaching safety and heat resistance of antibacterial agents in the diaper surface layer, and achieves high-efficiency antibacterial performance and comfort.

CN123101720APending Publication Date: 2026-11-17FUJIAN XINJUSEN HYGIENE PRODUCTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611461066.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing antibacterial agents in the surface layer of diapers have issues with leaching safety and poor heat resistance, making it difficult to maintain effective antibacterial performance under high-temperature processing conditions and easily leading to bacterial resistance.

Method used

Barium titanate is used as a piezoelectric catalytic antibacterial material. It is modified by surface treatment agent and loaded into PET yarn. Combined with long-chain quaternary ammonium salt antibacterial finishing, it forms an antibacterial surface layer. It is then combined with the flow-guiding layer, absorbent core and breathable bottom layer to form a protective diaper.

Benefits of technology

It achieves uniform dispersion of the antibacterial surface layer and improved interfacial bonding. The directional distribution of long-chain quaternary ammonium salts improves antibacterial efficiency. Through synergistic effect, it significantly inhibits bacterial adhesion and odor generation, while maintaining good protection and wearing comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123101720A_ABST
    Figure CN123101720A_ABST
Patent Text Reader

Abstract

This invention relates to a protective diaper and its preparation method, belonging to the field of hygiene product technology. The invention designs a protective diaper composed of an antibacterial surface layer, a flow-guiding layer, an absorbent core, and a breathable bottom layer. The antibacterial surface layer is woven from antibacterial yarn. After the yarn is spun, the PET yarn undergoes an antibacterial treatment to introduce long-chain quaternary ammonium salts. This modification not only effectively avoids structural damage to the long-chain quaternary ammonium salts during the high-temperature melt extrusion process but also allows the long-chain quaternary ammonium salts to be directionally distributed in the near-surface area of ​​the PET yarn, effectively improving the contact antibacterial efficiency of the long-chain quaternary ammonium salts. The diaper designed by this invention combines antibacterial, flow-guiding, absorbent, leak-proof, and breathable functions. Furthermore, the antibacterial surface layer selects non-leaching antibacterial components, which are not easily migrated or leached, providing excellent protection and wearing comfort.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of hygiene products technology, specifically relating to a protective diaper and its preparation method. Background Technology

[0002] As a daily hygiene product for infants and incontinent adults, disposable diapers' surface layer, which comes into direct contact with the skin, is constantly exposed to secretions such as urine, sweat, and feces during use, making it highly susceptible to bacterial and fungal growth. The proliferation of microorganisms not only produces unpleasant odors but can also induce skin redness, itching, diaper rash, and even infections, seriously affecting the user's comfort and health. Therefore, it is necessary to endow the diaper surface layer with sufficient antibacterial properties to ensure the diaper's protective function.

[0003] Antibacterial modification of the diaper surface layer is usually achieved by adding antibacterial agents. Commonly used antibacterial agents include silver-based, zinc-based, and organic antibacterial agents. Among them, silver-based and zinc-based antibacterial agents have leaching problems, which may pose safety risks with long-term skin contact. Organic antibacterial agents have poor heat resistance, making them difficult to adapt to the high-temperature processing conditions of melt spinning, and they are prone to inducing bacterial resistance.

[0004] In recent years, piezoelectric catalytic antibacterial materials have attracted attention due to their characteristics such as not relying on the release of chemical antibacterial agents, not easily inducing bacterial resistance, and good durability. Barium titanate, as a typical piezoelectric catalytic antibacterial material, can generate surface charges when subjected to mechanical stress, and further generate active oxygen in an aqueous environment, thereby achieving an antibacterial effect. However, the piezoelectric catalytic antibacterial efficiency of barium titanate alone is relatively low, making it difficult to achieve the ideal antibacterial effect. To overcome the above technical shortcomings, this invention provides a protective diaper and its preparation method. Summary of the Invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a protective diaper and a method for preparing the same.

[0006] This invention provides a protective diaper, the structure of which, from top to bottom, comprises an antibacterial top layer, a diversion layer, an absorbent core, and a breathable bottom layer.

[0007] Preferably, the antibacterial surface layer is prepared by the following steps: Step 1: Mix 3-aminopyridine, 2-pyridinecarboxaldehyde or 4-pyridinecarboxaldehyde, and cyanoacetic acid and react them to obtain a surface treatment agent; The second step is to load a surface treatment agent onto the surface of barium titanate to modify the barium titanate and obtain modified barium titanate. The third step involves mixing polyethylene terephthalate, modified barium titanate, antioxidants, and lubricants, then adding the mixture to a screw extruder and melt spinning it to obtain PET yarn. Step 4: After applying n-dodecyl bromide to the PET yarn for antibacterial treatment, antibacterial yarn is obtained. The antibacterial yarn is then spun into shape to obtain the antibacterial surface layer. Preferably, the barium titanate is tetragonal barium titanate.

[0008] Preferably, the antioxidant is at least one of antioxidant 1010, antioxidant 1035, antioxidant 1076, and antioxidant 168.

[0009] Preferably, the lubricant is at least one of pentaerythritol stearate and ethylene bis-stearamide.

[0010] Preferably, the loading modification conditions are as follows: 0.5-1.5 parts by mass of surface treatment agent, 10 parts by mass of barium titanate, and 100-150 parts by mass of anhydrous ethanol are mixed and reacted at a temperature of 60-80°C for 8-24 hours. After the reaction is completed, the solid is filtered to separate the solid and the obtained solid is washed with anhydrous ethanol and deionized water in sequence and then dried to constant weight to obtain modified barium titanate.

[0011] Preferably, the melt spinning conditions are as follows: screw extruder temperature: zone 1 260-270℃, zone 2 270-280℃, zone 3 275-285℃, die head temperature 280-290℃, spinning speed 800-1200m / min, side blowing temperature 15-25℃, and drawing ratio 2.0-3.5.

[0012] Preferably, the antibacterial finishing conditions are as follows: 100 parts by weight of PET yarn, 0.5 to 1.2 parts by weight of n-dodecyl bromide, and 400 to 500 parts by weight of acetonitrile are mixed and reacted at a temperature of 70 to 90°C for 6 to 12 hours. After the reaction is completed, the yarn is filtered and separated, and the yarn is washed successively with anhydrous ethanol and deionized water and then dried to obtain antibacterial yarn.

[0013] Preferably, the textile forming conditions are as follows: using weft knitting, with a loop length of 2.0–3.0 mm and a knitting speed of 100–300 r / min, the knitting forming yields an areal density of 25–40 g / m². 2 Antibacterial surface layer.

[0014] Preferably, the flow guiding layer is an ES fiber hot air nonwoven fabric, and the areal density of the flow guiding layer is 20-30 g / m². 2 .

[0015] Preferably, the absorbent core is a mixture of fluff pulp and superabsorbent resin, wherein the mass fraction of superabsorbent resin is 40-55%, and the areal density of the absorbent core is 250-450 g / m³. 2 .

[0016] Preferably, the breathable bottom layer is a composite layer of a breathable membrane and SMS nonwoven fabric, the water vapor transmission rate of the breathable membrane is 2400-3200 g / (m2·24h), and the areal density of the breathable bottom layer is 25-45 g / m2. 2 .

[0017] The present invention also provides a method for preparing the product as described above.

[0018] A method for preparing a protective diaper includes the following steps: The antibacterial top layer, the diversion layer, the absorbent core, and the breathable bottom layer are stacked in order from top to bottom. Hot melt adhesive is applied between adjacent layers and they are pressed together and then cooled to room temperature. The layers are then cut and shaped to obtain a protective diaper.

[0019] Preferably, the hot melt adhesive is applied at a temperature of 150–170°C using a spiral application method, and the interlayer application rate is 1.5–2.5 g / m². 2 .

[0020] Preferably, the pressing conditions are: pressing roller temperature 25-45℃, linear pressure 0.2-0.6MPa, and compounding speed 150-350m / min.

[0021] In summary, the present invention has at least the following beneficial effects: 1) The protective diaper designed in this invention is composed of an antibacterial surface layer, a diversion layer, an absorbent core, and a breathable bottom layer. It has antibacterial, diversion, absorption, leak-proof, and breathable functions. The antibacterial surface layer is made of non-leaching antibacterial components, which are not easy to migrate and leach out, and has good protective properties and wearing comfort.

[0022] 2) This invention effectively improves the dispersion uniformity and interfacial bonding of modified barium titanate in yarn by modifying barium titanate, and enhances the effective piezoelectric response efficiency of modified barium titanate by improving the stress transfer efficiency between the polymer matrix and filler particles in the yarn.

[0023] 3) This invention involves antibacterial finishing of the PET yarn after yarn spinning to introduce long-chain quaternary ammonium salts. This modification method not only effectively avoids the structural damage of long-chain quaternary ammonium salts during the high-temperature melt extrusion process, but also allows the long-chain quaternary ammonium salts to be oriented and distributed in the near-surface area of ​​the PET yarn, effectively improving the contact antibacterial efficiency of the long-chain quaternary ammonium salts. In addition, the contact antibacterial effect of the long-chain quaternary ammonium salts and the piezoelectric catalytic antibacterial effect of the modified barium titanate work together to achieve a broader antibacterial spectrum and better antibacterial effect, effectively inhibiting the adhesion of live bacteria and the formation of biofilms, and significantly reducing the odor generated by diapers during use.

[0024] Of course, any product implementing this invention does not necessarily need to achieve all of the advantages described above at the same time. Attached Figure Description

[0025] Figure 1 This is a scanning electron microscope image of barium titanate without loading modification.

[0026] Figure 2 This is a scanning electron microscope image of the modified barium titanate after load modification in Example 3.

[0027] Figure 3 This is the infrared spectrum of the surface treatment agent obtained in Example 3 of the present invention. Detailed Implementation

[0028] It should be understood that the expression “one or more of…” individually includes each of the objects described after the expression, as well as various different combinations of two or more of the described objects, unless otherwise understood from the context and usage. The expression “and / or” combined with three or more described objects should be understood to have the same meaning, unless otherwise understood from the context.

[0029] The terms “including,” “having,” or “containing,” including the use of their grammatical synonyms, should generally be understood as open-ended and non-restrictive, for example, not excluding other unstated elements or steps, unless otherwise specifically stated or understood from the context.

[0030] It should be understood that the order of steps or the sequence of actions is not important as long as this application remains operational. Furthermore, two or more steps or actions may be performed simultaneously.

[0031] The use of any and all instances or exemplary language such as “e.g.” or “including” herein is merely intended to better illustrate the application and does not constitute a limitation on the scope of the application unless the claims are made. No language in this specification should be construed as indicating that any unclaimed element is essential to the practice of this application.

[0032] Furthermore, the numerical ranges and parameters used to define this application are approximate values, and the relevant values ​​in the specific embodiments have been presented as precisely as possible. However, any numerical value inevitably contains standard deviations due to individual test methods. Therefore, unless otherwise explicitly stated, it should be understood that all ranges, quantities, values, and percentages used in this disclosure are modified with the word "approximately." Here, "approximately" generally means that the actual value is within plus or minus 10%, 5%, 1%, or 0.5% of a specific value or range.

[0033] In a specific embodiment of the present invention, a protective diaper has a structure comprising, from top to bottom, an antibacterial surface layer, a diversion layer, an absorbent core, and a breathable bottom layer.

[0034] In a specific embodiment of the present invention, the antibacterial surface layer is made by the following steps: S101. Mix 1 part by mass of 3-aminopyridine, 1.2 parts by mass of 2-pyridinecarboxaldehyde or 4-pyridinecarboxaldehyde, 1.1-1.3 parts by mass of cyanoacetic acid, 0.5-0.8 parts by mass of p-toluenesulfonic acid, and 15-20 parts by mass of N,N-dimethylformamide and react at 60-100℃ for 4-8 hours. After the reaction is completed, pour the reaction solution into deionized water to precipitate. After filtering and separating the precipitate, wash the precipitate with deionized water and dry it to obtain the surface treatment agent. In this stage, 3-aminopyridine, 2-pyridinecarboxaldehyde, or 4-pyridinecarboxaldehyde undergo a Mannich reaction with cyanoacetic acid under the catalysis of p-toluenesulfonic acid to obtain a surface treatment agent with two pyridine rings, one cyano group, and one carboxyl group in its structure. S102. Mix 0.5-1.5 parts by mass of surface treatment agent, 10 parts by mass of barium titanate, and 100-150 parts by mass of anhydrous ethanol and react at 60-80℃ for 8-24 hours. After the reaction is completed, filter to separate the solid and wash the obtained solid with anhydrous ethanol and deionized water in sequence and dry to constant weight to obtain modified barium titanate. During this stage, the carboxyl groups in the surface treatment agent react with the Ti groups on the barium titanate surface. 4+ and Ba 2+ Modifying barium titanate by forming coordinate bonds can passivate surface defects and improve surface uniformity. S103. Mix 100 parts by weight of polyethylene terephthalate, 3-5 parts by weight of modified barium titanate, 0.5-0.8 parts by weight of antioxidant, and 0.2-0.5 parts by weight of lubricant, and add the mixture to a screw extruder. Set the screw extruder temperature as follows: Zone 1 260-270℃, Zone 2 270-280℃, Zone 3 275-285℃, and Die head temperature 280-290℃. After melt extrusion, spin the mixture at a spinning speed of 800-1200 m / min, a side blowing temperature of 15-25℃, and a draw ratio of 2.0-3.5 to obtain PET yarn. During this stage, the modified barium titanate surface has a pyridine ring structure and a cyano structure. These two structures can improve the interfacial bonding force between the modified barium titanate and polyethylene terephthalate and the dispersion uniformity of the modified barium titanate through π-π stacking and dipole interaction, effectively suppress the formation of agglomerates, improve the stress transfer efficiency in the matrix, and thus improve the effective piezoelectric response efficiency of barium titanate. S104. Mix 100 parts by weight of PET yarn, 0.5-1.2 parts by weight of n-dodecyl bromide, and 400-500 parts by weight of acetonitrile and react at 70-90℃ for 6-12 hours. After the reaction, filter to separate the yarn and wash it successively with anhydrous ethanol and deionized water, then dry to obtain antibacterial yarn. Weft knit the antibacterial yarn at a loop length of 2.0-3.0 mm and a knitting speed of 100-300 r / min to obtain a surface density of 25-40 g / m². 2 Antibacterial surface layer; In this stage, the PET yarn is treated with antibacterial agents. The dodecyl bromide reacts with the pyridine ring on the modified barium titanate surface in the near-surface region of the PET yarn to form a quaternary ammonium salt. Long-chain quaternary ammonium salts are selectively generated in the near-surface region of the PET yarn, which effectively improves the antibacterial efficiency of the long-chain quaternary ammonium salts. Moreover, the generated long-chain quaternary ammonium salts are loaded on the modified barium titanate surface and are not easy to migrate and dissolve, thus having good safety. During this stage, long-chain quaternary ammonium salt and modified barium titanate can produce a synergistic antibacterial effect. On the one hand, the reactive oxygen species generated by modified barium titanate can oxidize the unsaturated fatty acids in the bacterial cell membrane, causing the bacterial cell membrane structure to disintegrate. This allows the long-chain alkyl groups in the long-chain quaternary ammonium salt to more effectively pierce the bacterial cell membrane. On the other hand, the long-chain alkyl groups in the long-chain quaternary ammonium salt destroy the integrity of the bacterial cell membrane, allowing the reactive oxygen species generated by modified barium titanate to more effectively enter the bacterial cell and cause oxidative damage to key biomolecules such as DNA, ribosomes, and respiratory chain, significantly accelerating the bacterial death rate. In a specific embodiment of the present invention, barium titanate is tetragonal barium titanate.

[0035] In a specific embodiment of the present invention, the antioxidant is at least one of antioxidant 1010, antioxidant 1035, antioxidant 1076, and antioxidant 168.

[0036] In a specific embodiment of the present invention, the lubricant is at least one of pentaerythritol stearate and ethylene bis-stearamide.

[0037] In a specific embodiment of the present invention, the flow guiding layer is an ES fiber hot air nonwoven fabric, and the areal density of the flow guiding layer is 20-30 g / m². 2 .

[0038] In a specific embodiment of the present invention, the absorbent core is a mixture of fluff pulp and superabsorbent resin, wherein the mass fraction of superabsorbent resin is 40-55%, and the areal density of the absorbent core is 250-450 g / m³. 2 .

[0039] In a specific embodiment of the present invention, the breathable bottom layer is a composite layer of a breathable membrane and SMS nonwoven fabric. The water vapor permeability of the breathable membrane is 2400-3200 g / (m²·24h), and the areal density of the breathable bottom layer is 25-45 g / m². 2 .

[0040] In a specific embodiment of the present invention, a method for preparing a protective diaper includes the following steps: The antibacterial top layer, the diversion layer, the absorbent core, and the breathable bottom layer are stacked in order from top to bottom. Hot melt adhesive is applied between adjacent layers and they are pressed together and then cooled to room temperature. The layers are then cut and shaped to obtain a protective diaper.

[0041] In a specific embodiment of the present invention, the hot melt adhesive is Technomelt DM527 type SIS-based hot melt pressure-sensitive adhesive with a softening point of 102°C and a melt viscosity of 2300 mPa·s at 160°C.

[0042] In a specific embodiment of the present invention, the application temperature of the hot melt adhesive is 150–170°C, the application method is spiral application, and the interlayer application amount is 1.5–2.5 g / m. 2 .

[0043] In a specific embodiment of the present invention, the pressing conditions are: pressing roller temperature 25-45°C, linear pressure 0.2-0.6 MPa, and compounding speed 150-350 m / min.

[0044] The present invention is further illustrated below with reference to the embodiments. The scope of protection of the present invention is not limited to the following embodiments.

[0045] Example 1 A protective diaper, the structure of which, from top to bottom, includes an antibacterial top layer, a diversion layer, an absorbent core, and a breathable bottom layer.

[0046] In this embodiment, the antibacterial surface layer is made by the following steps: S101. Mix 1 part by mass of 3-aminopyridine, 1.2 parts by mass of 2-pyridinecarboxaldehyde, 1.1 parts by mass of cyanoacetic acid, 0.5 parts by mass of p-toluenesulfonic acid, and 15 parts by mass of N,N-dimethylformamide and react at 60°C for 8 hours. After the reaction is completed, pour the reaction solution into deionized water to precipitate. After filtering to separate the precipitate, wash the precipitate with deionized water and dry it to obtain the surface treatment agent. S102. Mix 0.5 parts by mass of surface treatment agent, 10 parts by mass of tetragonal barium titanate, and 100 parts by mass of anhydrous ethanol and react at 60°C for 24 hours. After the reaction is completed, filter to separate the solid and wash the obtained solid with anhydrous ethanol and deionized water in sequence and dry to constant weight to obtain modified barium titanate. S103. Mix 100 parts by weight of polyethylene terephthalate, 3 parts by weight of modified barium titanate, 0.3 parts by weight of antioxidant 1010, 0.2 parts by weight of antioxidant 168, and 0.2 parts by weight of pentaerythritol stearate, and add them to a screw extruder. Set the screw extruder temperature as follows: Zone 1 260℃, Zone 2 270℃, Zone 3 275℃, and Die head temperature 280℃. After melt extrusion, spin the yarn at a spinning speed of 800m / min, a side blowing temperature of 25℃, and a draw ratio of 2.0 to obtain PET yarn. S104. 100 parts by weight of PET yarn, 0.5 parts by weight of n-dodecyl bromide, and 400 parts by weight of acetonitrile were mixed and reacted at 70℃ for 12 hours. After the reaction, the yarn was separated by filtration and washed successively with anhydrous ethanol and deionized water, then dried to obtain antibacterial yarn. The antibacterial yarn was then weft-knitted at a loop length of 3.0 mm and a knitting speed of 300 r / min to obtain a surface density of 40 g / m². 2 Antibacterial surface layer.

[0047] In this embodiment, the flow guiding layer is an ES fiber hot air nonwoven fabric, and the areal density of the flow guiding layer is 30 g / m². 2 .

[0048] In this embodiment, the absorbent core is a mixture of fluff pulp and superabsorbent resin, wherein the mass fraction of superabsorbent resin is 55%, and the areal density of the absorbent core is 250 g / m³. 2 .

[0049] In this embodiment, the breathable bottom layer is a composite layer of a breathable membrane and SMS nonwoven fabric. The water vapor transmission rate of the breathable membrane is 2400 g / (m2·24h), and the areal density of the breathable bottom layer is 25 g / m2. 2 .

[0050] A method for preparing a protective diaper includes the following steps: The antibacterial top layer, the flow-guiding layer, the absorbent core, and the breathable bottom layer are stacked in that order from top to bottom. Hot melt adhesive is applied between adjacent layers at a temperature of 150℃ using a spiral application method, with an interlayer adhesive application rate of 1.5 g / m². 2 After applying the adhesive, the diapers are pressed together at a temperature of 25°C, a linear pressure of 0.2 MPa, and a lamination speed of 150 m / min. After pressing, the diapers are cooled to room temperature and then slit and shaped to obtain protective diapers.

[0051] Example 2 A protective diaper, the structure of which, from top to bottom, includes an antibacterial top layer, a diversion layer, an absorbent core, and a breathable bottom layer.

[0052] In this embodiment, the antibacterial surface layer is made by the following steps: S101. Mix 1 part by mass of 3-aminopyridine, 1.2 parts by mass of 4-pyridinecarboxaldehyde, 1.2 parts by mass of cyanoacetic acid, 0.65 parts by mass of p-toluenesulfonic acid, and 18 parts by mass of N,N-dimethylformamide and react at 80°C for 6 hours. After the reaction is completed, pour the reaction solution into deionized water to precipitate. After filtering and separating the precipitate, wash the precipitate with deionized water and dry it to obtain the surface treatment agent. S102. Mix 1 part by mass of surface treatment agent, 10 parts by mass of tetragonal barium titanate and 125 parts by mass of anhydrous ethanol and react at 70°C for 16 h. After the reaction is completed, filter to separate the solid and wash the obtained solid with anhydrous ethanol and deionized water in sequence and dry to constant weight to obtain modified barium titanate. S103. Mix 100 parts by weight of polyethylene terephthalate, 4 parts by weight of modified barium titanate, 0.4 parts by weight of antioxidant 1035, 0.25 parts by weight of antioxidant 168, and 0.35 parts by weight of pentaerythritol stearate, and add the mixture to a screw extruder. Set the screw extruder temperature as follows: Zone 1 265℃, Zone 2 275℃, Zone 3 280℃, and Die head temperature 285℃. After melt extrusion, spin the mixture at a spinning speed of 1000m / min, a side blowing temperature of 20℃, and a draw ratio of 3.0 to obtain PET yarn. S104. 100 parts by weight of PET yarn, 0.9 parts by weight of n-dodecyl bromide, and 450 parts by weight of acetonitrile were mixed and reacted at 80℃ for 9 hours. After the reaction, the yarn was separated by filtration and washed successively with anhydrous ethanol and deionized water, then dried to obtain antibacterial yarn. The antibacterial yarn was then weft-knitted at a loop length of 2.5 mm and a knitting speed of 200 r / min to obtain a surface density of 30 g / m². 2 Antibacterial surface layer.

[0053] In this embodiment, the flow guiding layer is an ES fiber hot air nonwoven fabric, and the areal density of the flow guiding layer is 25 g / m². 2 .

[0054] In this embodiment, the absorbent core is a mixture of fluff pulp and superabsorbent resin, wherein the superabsorbent resin has a mass fraction of 50%, and the areal density of the absorbent core is 350 g / m³. 2 .

[0055] In this embodiment, the breathable bottom layer is a composite layer of a breathable membrane and SMS nonwoven fabric. The water vapor permeability of the breathable membrane is 2800 g / (m2·24h), and the areal density of the breathable bottom layer is 35 g / m2. 2 .

[0056] A method for preparing a protective diaper includes the following steps: The antibacterial top layer, the flow-guiding layer, the absorbent core, and the breathable bottom layer are stacked in order from top to bottom. Hot melt adhesive is applied between adjacent layers at a temperature of 160℃ using a spiral application method, with an interlayer adhesive application rate of 2g / m². 2 After applying the adhesive, the diapers are pressed together at a temperature of 35°C, a linear pressure of 0.4 MPa, and a lamination speed of 250 m / min. After pressing, the diapers are cooled to room temperature and then slit and shaped to obtain protective diapers.

[0057] Example 3 A protective diaper, the structure of which, from top to bottom, includes an antibacterial top layer, a diversion layer, an absorbent core, and a breathable bottom layer.

[0058] In this embodiment, the antibacterial surface layer is made by the following steps: S101. Mix 1 part by mass of 3-aminopyridine, 1.2 parts by mass of 4-pyridinecarboxaldehyde, 1.3 parts by mass of cyanoacetic acid, 0.8 parts by mass of p-toluenesulfonic acid, and 20 parts by mass of N,N-dimethylformamide and react at 100℃ for 4 hours. After the reaction is completed, pour the reaction solution into deionized water to precipitate. After filtering and separating the precipitate, wash the precipitate with deionized water and dry it to obtain the surface treatment agent. S102. Mix 1.5 parts by mass of surface treatment agent, 10 parts by mass of tetragonal barium titanate, and 150 parts by mass of anhydrous ethanol and react at 80°C for 8 hours. After the reaction is completed, filter to separate the solid and wash the obtained solid with anhydrous ethanol and deionized water in sequence and dry to constant weight to obtain modified barium titanate. S103. Mix 100 parts by weight of polyethylene terephthalate, 5 parts by weight of modified barium titanate, 0.4 parts by weight of antioxidant 1076, 0.4 parts by weight of antioxidant 168, and 0.5 parts by weight of ethylene bis-stearamide, and add the mixture to a screw extruder. Set the screw extruder temperature as follows: Zone 1 270℃, Zone 2 280℃, Zone 3 285℃, and Die head temperature 290℃. After melt extrusion, spin the mixture at a spinning speed of 1200m / min, a side blowing temperature of 15℃, and a draw ratio of 3.5 to obtain PET yarn. S104. 100 parts by weight of PET yarn, 1.2 parts by weight of n-dodecyl bromide, and 500 parts by weight of acetonitrile were mixed and reacted at 90℃ for 6 hours. After the reaction, the yarn was separated by filtration and washed successively with anhydrous ethanol and deionized water, then dried to obtain antibacterial yarn. The antibacterial yarn was then weft-knitted at a loop length of 2.0 mm and a knitting speed of 100 r / min to obtain a surface density of 25 g / m². 2 Antibacterial surface layer.

[0059] In this embodiment, the flow guiding layer is an ES fiber hot air nonwoven fabric, and the areal density of the flow guiding layer is 20 g / m². 2 .

[0060] In this embodiment, the absorbent core is a mixture of fluff pulp and superabsorbent resin, wherein the mass fraction of superabsorbent resin is 40%, and the areal density of the absorbent core is 450 g / m³. 2 .

[0061] In this embodiment, the breathable bottom layer is a composite layer of a breathable membrane and SMS nonwoven fabric. The water vapor transmission rate of the breathable membrane is 3200 g / (m2·24h), and the areal density of the breathable bottom layer is 45 g / m2. 2 .

[0062] A method for preparing a protective diaper includes the following steps: The antibacterial top layer, the flow-guiding layer, the absorbent core, and the breathable bottom layer are stacked in that order from top to bottom. Hot melt adhesive is applied between adjacent layers at a temperature of 170℃ using a spiral application method, with an interlayer adhesive application rate of 2.5 g / m². 2 After applying the adhesive, the diapers are pressed together at a temperature of 45°C, a linear pressure of 0.6 MPa, and a lamination speed of 350 m / min. After pressing, the diapers are cooled to room temperature and then slit and shaped to obtain protective diapers.

[0063] Comparative Example 1 The difference between this comparative example and Example 2 is that the PET yarn is not treated with antibacterial finishing.

[0064] A protective diaper, the structure of which, from top to bottom, includes an antibacterial top layer, a diversion layer, an absorbent core, and a breathable bottom layer.

[0065] In this comparative example, the antibacterial surface layer was prepared by the following steps: S101. Mix 1 part by mass of 3-aminopyridine, 1.2 parts by mass of 4-pyridinecarboxaldehyde, 1.2 parts by mass of cyanoacetic acid, 0.65 parts by mass of p-toluenesulfonic acid, and 18 parts by mass of N,N-dimethylformamide and react at 80°C for 6 hours. After the reaction is completed, pour the reaction solution into deionized water to precipitate. After filtering and separating the precipitate, wash the precipitate with deionized water and dry it to obtain the surface treatment agent. S102. Mix 1 part by mass of surface treatment agent, 10 parts by mass of tetragonal barium titanate and 125 parts by mass of anhydrous ethanol and react at 70°C for 16 h. After the reaction is completed, filter to separate the solid and wash the obtained solid with anhydrous ethanol and deionized water in sequence and dry to constant weight to obtain modified barium titanate. S103. Mix 100 parts by weight of polyethylene terephthalate, 4 parts by weight of modified barium titanate, 0.4 parts by weight of antioxidant 1035, 0.25 parts by weight of antioxidant 168, and 0.35 parts by weight of pentaerythritol stearate, and add the mixture to a screw extruder. Set the screw extruder temperature as follows: Zone 1 265℃, Zone 2 275℃, Zone 3 280℃, and Die head temperature 285℃. After melt extrusion, spin the mixture at a spinning speed of 1000m / min, a side blowing temperature of 20℃, and a draw ratio of 3.0 to obtain PET yarn. S104. Using weft knitting technology, PET yarn is woven to obtain a surface density of 30 g / m² under the conditions of a loop length of 2.5 mm and a knitting speed of 200 r / min. 2 Antibacterial surface layer.

[0066] In this comparative example, the flow guiding layer is an ES fiber hot air nonwoven fabric, and the areal density of the flow guiding layer is 25 g / m². 2 .

[0067] In this comparative example, the absorbent core is a mixture of fluff pulp and superabsorbent polymer (SAP), wherein the SAP mass fraction is 50%, and the areal density of the absorbent core is 350 g / m³. 2 .

[0068] In this comparative example, the breathable bottom layer is a composite layer of a breathable membrane and SMS nonwoven fabric. The water vapor permeability of the breathable membrane is 2800 g / (m2·24h), and the areal density of the breathable bottom layer is 35 g / m2. 2 .

[0069] A method for preparing a protective diaper includes the following steps: The antibacterial top layer, the flow-guiding layer, the absorbent core, and the breathable bottom layer are stacked in order from top to bottom. Hot melt adhesive is applied between adjacent layers at a temperature of 160℃ using a spiral application method, with an interlayer adhesive application rate of 2g / m². 2 After applying the adhesive, the diapers are pressed together at a temperature of 35°C, a linear pressure of 0.4 MPa, and a lamination speed of 250 m / min. After pressing, the diapers are cooled to room temperature and then slit and shaped to obtain protective diapers.

[0070] Comparative Example 2 The difference between this comparative example and Example 2 is that barium titanate is not modified by loading, but commercially available quaternary ammonium salt antibacterial agent benzalkonium chloride is added to the raw materials for preparing PET yarn.

[0071] A protective diaper, the structure of which, from top to bottom, includes an antibacterial top layer, a diversion layer, an absorbent core, and a breathable bottom layer.

[0072] In this comparative example, the antibacterial surface layer was prepared by the following steps: S101. Mix 100 parts by weight of polyethylene terephthalate, 4 parts by weight of barium titanate, 0.5 parts by weight of benzalkonium chloride, 0.4 parts by weight of antioxidant 1035, 0.25 parts by weight of antioxidant 168, and 0.35 parts by weight of pentaerythritol stearate, and add the mixture to a screw extruder. Set the screw extruder temperature as follows: Zone 1 265℃, Zone 2 275℃, Zone 3 280℃, and Die head temperature 285℃. After melt extrusion, spin the mixture at a spinning speed of 1000m / min, a side blowing temperature of 20℃, and a draw ratio of 3.0 to obtain PET yarn. S102. Using weft knitting technology, PET yarn is woven to obtain a surface density of 30 g / m² under the conditions of a loop length of 2.5 mm and a knitting speed of 200 r / min. 2 Antibacterial surface layer.

[0073] In this comparative example, the flow guiding layer is an ES fiber hot air nonwoven fabric, and the areal density of the flow guiding layer is 25 g / m². 2 .

[0074] In this comparative example, the absorbent core is a mixture of fluff pulp and superabsorbent polymer (SAP), wherein the SAP mass fraction is 50%, and the areal density of the absorbent core is 350 g / m³. 2 .

[0075] In this comparative example, the breathable bottom layer is a composite layer of a breathable membrane and SMS nonwoven fabric. The water vapor permeability of the breathable membrane is 2800 g / (m2·24h), and the areal density of the breathable bottom layer is 35 g / m2. 2 .

[0076] A method for preparing a protective diaper includes the following steps: The antibacterial top layer, the flow-guiding layer, the absorbent core, and the breathable bottom layer are stacked in order from top to bottom. Hot melt adhesive is applied between adjacent layers at a temperature of 160℃ using a spiral application method, with an interlayer adhesive application rate of 2g / m². 2 After applying the adhesive, the diapers are pressed together at a temperature of 35°C, a linear pressure of 0.4 MPa, and a lamination speed of 250 m / min. After pressing, the diapers are cooled to room temperature and then slit and shaped to obtain protective diapers.

[0077] Experimental Example 1 The antibacterial surface layer of the diapers in Examples 1-3 and Comparative Examples 1-2 were subjected to performance tests. The inhibition rates of each component sample against *Escherichia coli* and *Staphylococcus aureus* were tested according to the national standard GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles - Part 3: Shaking Method". The culture conditions were 37±1℃ and shaking culture time was 18h. The blank control was a pure PET surface layer. The test was repeated after 10 washes. The test results are shown in Table 1. Table 1 As shown in Table 1, the antibacterial surface layer of the diapers obtained in Examples 1-3 exhibits good antibacterial properties and maintains these properties even after washing. Although commercially available quaternary ammonium salt antibacterial agents were also added in Comparative Example 2, the high processing temperature of PET led to the extensive decomposition of benzalkonium chloride, resulting in an inability to maintain a complete antibacterial structure. Furthermore, the unmodified barium titanate still exhibited poor compatibility during processing, leading to agglomeration and uneven dispersion. Therefore, the antibacterial efficiency was actually lower than that of Comparative Example 1, which did not contain any additional antibacterial agents or undergo antibacterial finishing.

[0078] Experimental Example 2 The surface treatment agent obtained in Example 3 was mixed and ground with potassium bromide powder and then pressed into a transparent sheet. The infrared spectrum was obtained by scanning with a Nexus 670 Fourier transform infrared spectroscopy system (Thermo Nicolet, USA) equipped with a DTGS detector.

[0079] like Figure 3 As shown, at 3392cm -1 An absorption peak of NH stretching vibration was observed at 3021 cm⁻¹. -1 An absorption peak for the CH stretching vibration on the pyridine ring was observed at [location missing]. This is because the carboxyl group formed a dimer, and the OH [group missing] [is also missing]. - The stretching vibration absorption peak shifts to lower wavenumbers, around 2792 cm⁻¹. -1 Location, 2717cm -1 Location, 2653cm -1 Multiple OH groups were observed at the location. - The stretching vibration absorption peak is at 2228 cm⁻¹. -1 The CN stretching vibration absorption peak was observed at 1698 cm⁻¹. -1 Location, 1682cm -1 An absorption peak of C=O stretching vibration on the carboxyl group was observed, indicating that the surface treatment agent required by the present invention has been successfully prepared.

[0080] The above description is merely a preferred embodiment of this application, but the scope of protection of this application is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in this application, based on the technical solution and inventive concept of this application, should be included within the scope of protection of this application.

Claims

1. A protective diaper, characterized in that, The structure, from top to bottom, includes an antibacterial top layer, a diversion layer, an absorbent core, and a breathable bottom layer. The antibacterial surface layer is made by the following steps: Step 1: Mix 3-aminopyridine, 2-pyridinecarboxaldehyde or 4-pyridinecarboxaldehyde, and cyanoacetic acid and react them to obtain a surface treatment agent; The second step is to load a surface treatment agent onto the surface of barium titanate to modify the barium titanate and obtain modified barium titanate. The third step involves mixing polyethylene terephthalate, modified barium titanate, antioxidants, and lubricants, then adding the mixture to a screw extruder and melt spinning it to obtain PET yarn. Step 4: After applying n-dodecyl bromide to the PET yarn for antibacterial treatment, antibacterial yarn is obtained. The antibacterial yarn is then spun into an antibacterial surface layer.

2. The protective diaper according to claim 1, characterized in that, The barium titanate is tetragonal barium titanate, the antioxidant is at least one of antioxidant 1010, antioxidant 1035, antioxidant 1076, and antioxidant 168, and the lubricant is at least one of pentaerythritol stearate and ethylene bis-stearamide.

3. A protective diaper according to claim 1, characterized in that, The loading modification conditions are as follows: 0.5-1.5 parts by mass of surface treatment agent, 10 parts by mass of barium titanate, and 100-150 parts by mass of anhydrous ethanol are mixed and reacted at a temperature of 60-80℃ for 8-24 hours. After the reaction is completed, the solid is filtered to separate the solid and the obtained solid is washed with anhydrous ethanol and deionized water in sequence and then dried to constant weight to obtain modified barium titanate.

4. A protective diaper according to claim 1, characterized in that, The conditions for melt spinning are as follows: screw extruder temperature: zone 1 260-270℃, zone 2 270-280℃, zone 3 275-285℃, die head temperature 280-290℃, spinning speed 800-1200m / min, side blowing temperature 15-25℃, and drawing ratio 2.0-3.

5.

5. A protective diaper according to claim 1, characterized in that, The antibacterial finishing conditions are as follows: 100 parts by weight of PET yarn, 0.5 to 1.2 parts by weight of n-dodecyl bromide, and 400 to 500 parts by weight of acetonitrile are mixed and reacted at a temperature of 70 to 90°C for 6 to 12 hours. After the reaction is completed, the yarn is filtered and separated, and then washed with anhydrous ethanol and deionized water in sequence and dried to obtain antibacterial yarn.

6. A protective diaper according to claim 1, characterized in that, The conditions for textile forming are as follows: using weft knitting process, with a loop length of 2.0 to 3.0 mm and a knitting speed of 100 to 300 r / min, an antibacterial surface layer with an areal density of 25 to 40 g / m2 is obtained.

7. A protective diaper according to claim 1, characterized in that, The flow guiding layer is made of ES fiber hot air nonwoven fabric, and the areal density of the flow guiding layer is 20-30 g / m². 2 The absorbent core is a mixture of fluff pulp and superabsorbent resin, wherein the mass fraction of superabsorbent resin is 40-55%, and the areal density of the absorbent core is 250-450 g / m³. 2 The breathable bottom layer is a composite layer of a breathable membrane and SMS nonwoven fabric, and the water vapor permeability of the breathable membrane is 2400-3200 g / (m²). 2 •24h), and the areal density of the breathable bottom layer is 25~45g / m². 2 .

8. A method for preparing a protective diaper as described in any one of claims 1 to 7, characterized in that, Includes the following steps: The antibacterial top layer, the diversion layer, the absorbent core, and the breathable bottom layer are stacked in order from top to bottom. Hot melt adhesive is applied between adjacent layers and they are pressed together and then cooled to room temperature. The layers are then cut and shaped to obtain a protective diaper.

9. The method for preparing a protective diaper according to claim 8, characterized in that, The hot melt adhesive is applied at a temperature of 150–170°C using a spiral application method, with an interlayer application rate of 1.5–2.5 g / m². 2 .

10. The method for preparing a protective diaper according to claim 8, characterized in that, The pressing conditions are: pressing roller temperature 25-45℃, linear pressure 0.2-0.6MPa, and compounding speed 150-350m / min.