A silica-alumina sol and its preparation method
By employing low-temperature co-hydrolysis and segmented temperature-controlled reflux aging processes, the problems of uniformity and stability of silicon-aluminum composites in the preparation of silicon-aluminum sols were solved, resulting in silicon-aluminum sols with narrow particle size distribution and stable storage, which are suitable for applications such as catalyst supports and high-temperature ceramic precursors.
Patent Information
- Application Number
- CN202611480378.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
In existing methods for preparing silicon-aluminum sol, there are temporal differences in the nucleation and condensation processes of silicon and aluminum components, which leads to a decrease in the uniformity of silicon-aluminum composites, making it easy to produce local component enrichment and particle agglomeration. Furthermore, high-temperature reactions accelerate the hydrolysis and condensation reaction rates of alkoxides, making it difficult to form a molecularly uniform composite structure.
A low-temperature co-hydrolysis strategy was adopted, in which silicon source and acid-catalyzed aqueous solution were simultaneously and uniformly added to aluminum source precursor liquid. Combined with a segmented temperature-controlled reflux aging process, the addition time and hydrolysis temperature were adjusted to ensure that the silicon-aluminum sol particle size distribution was 5-50nm within the range of silicon-aluminum molar ratio of 1:0.02-1:5.
A clear, transparent silica-alumina sol with a narrow particle size distribution and excellent storage stability was prepared, which is suitable for multiple applications. The problem of easy agglomeration and phase separation of silica-alumina sol was solved, and efficient silica-alumina composite uniformity and long-term stability were achieved.
Smart Images

Figure CN123102251A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of inorganic sol materials technology, specifically to a silica-alumina sol and its preparation method. Background Technology
[0002] Silica-alumina sol is an inorganic colloidal material that combines the excellent weather resistance and light transmittance of silica with the high activity, high temperature resistance, and high adhesion of alumina. Due to its molecularly uniform silica-alumina composite network structure, it is widely used in many fields such as catalyst supports, high-temperature ceramic precursors, optical coatings, inorganic modified coatings, and molecular sieve synthesis. Compared to single silica sols or alumina sols, silica-alumina sols effectively avoid the defects of single-component colloids, such as poor thermal stability, insufficient cross-linking activity, and poor film density, making them a core precursor for high-performance inorganic functional materials.
[0003] Existing methods for preparing silica-alumina sol, such as the method for preparing high-purity silica-alumina sol disclosed in CN108854870A, have the following problems: 1. The aluminum source undergoes hydrolysis, nucleation, and forms a stable colloidal particle structure in advance, followed by the introduction of pre-hydrolyzed silicon components. This feeding and compounding method results in a significant temporal difference between the nucleation and condensation processes of the silicon and aluminum components. The silicon component tends to adhere to the surface of the already formed aluminum sol particles for condensation reactions, which easily leads to a decrease in the uniformity of the silicon-aluminum composite. The system is more prone to local component enrichment, which in turn induces slight particle agglomeration and a certain tendency for phase separation, making it difficult to form a molecularly uniform silicon-aluminum network structure.
[0004] 2. The overall reaction temperature is relatively high, with the hydrolysis temperature of aluminum sol reaching 85–92℃, while the pre-hydrolysis and composite processes of silicon source are maintained at around 70℃. Higher reaction temperatures accelerate the reaction rates of alkoxide hydrolysis and condensation, reducing the controllability of the nucleation and growth process to some extent, making the system more prone to uneven nucleation and wide particle size distribution. Summary of the Invention
[0005] This invention provides a silica-alumina sol and its preparation method to solve the technical problems mentioned in the background.
[0006] To solve the above-mentioned technical problems, this invention discloses a method for preparing silica-alumina sol, comprising: S1: Add the aluminum source and anhydrous ethanol in a molar ratio of 1:3-1:15. Add the anhydrous ethanol to the reaction vessel, then add the aluminum source. Stir at room temperature and 200-500 r / min for 0.5-3 h until the aluminum source is completely dissolved to obtain the aluminum source precursor liquid. S2: Determine the amount of silicon source to be fed according to the silicon-aluminum molar ratio of 1:0.02-1:5; S3: Determine the amount of deionized water according to the molar ratio of silicon source to deionized water of 1:4-1:200. Mix deionized water and anhydrous ethanol at a volume ratio of 1:0.1-1:3. Add 5%-20% acid solution by mass under stirring at room temperature to adjust the pH of the mixture of deionized water, anhydrous ethanol and acid solution to 2.5-4.5 to obtain an acid-catalyzed aqueous solution. S4: Control the stirring speed to 300-800 r / min and the water bath temperature to 5-20℃. Drop the silicon source and acid catalytic aqueous solution into the aluminum source precursor liquid. During the process, keep the silicon source and acid catalytic aqueous solution added synchronously and at a uniform rate, and keep the start and end times of the addition consistent. When the silicon-aluminum molar ratio is 1:0.02-1:2, the addition time of the silicon source and acid catalytic aqueous solution is controlled at 0.5-5 h. When the silicon-aluminum molar ratio is 1:2-1:5, the addition time of the silicon source and acid catalytic aqueous solution is controlled at 3-12 h. S5: Raise the water bath temperature to 30-75℃, stir and reflux for 0.5-10h, cool to room temperature after the reaction is complete, and continue stirring and aging for 0.5-3h to finally obtain a silica-alumina sol with a pH of 3-5 and a particle size of 5-50nm.
[0007] Preferably, the aluminum source includes either aluminum isopropoxide or aluminum sec-butoxide.
[0008] Preferably, the acid solution includes any one of nitric acid, hydrochloric acid, and sulfuric acid.
[0009] Preferably, the silicon source includes either methyl silicate or ethyl silicate.
[0010] Preferably, in step S4, the water bath temperature is raised to 40-65°C.
[0011] Preferably, the acid solution with a mass fraction of 5%-20% is nitric acid with a mass fraction of 5%.
[0012] The present invention also discloses a silica-alumina sol, which is prepared by the aforementioned method for preparing a silica-alumina sol.
[0013] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments.
[0014] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention employs a co-hydrolysis strategy involving the simultaneous and uniform dropwise addition of a silicon source and an acid-catalyzed aqueous solution to an aluminum source precursor liquid. Under low-temperature water bath conditions, the hydrolysis-condensation rates of the silicon and aluminum sources are matched to avoid excessive and rapid hydrolysis of any single component. Comparative Examples 1-4 demonstrate that when the dropwise rate is too fast, the hydrolysis temperature is too high, the system pH is outside the range of this invention, or the alcohol-water solvent ratio is unbalanced, the sol system exhibits significant agglomeration, turbidity, precipitation, and stratification. The silica-alumina sol prepared using the process conditions of this invention, as shown in Examples 1-4, yields clear, stratified sol products without particle agglomeration, overcoming the problems of phase separation and precipitation that easily occur during the co-hydrolysis of silica-alumina alkoxides.
[0015] 2. This invention can prepare silicon-aluminum sol in a silicon-aluminum molar ratio of 1:0.02-1:5. By adjusting process parameters such as dropping time, hydrolysis temperature, and aging temperature, the average particle size of the sol can be controlled within the range of 5-50 nm. In Example 1, a narrow-distribution sol with an average particle size of 12.5 nm and a PDI as low as 0.08 was obtained. Even with an increased silicon content, the PDI of the products in all examples was ≤0.14. In contrast, the comparative product with a PDI as high as 0.45, exceeding the process parameters of this invention, exhibited a wide particle distribution. This invention is adaptable to different composition requirements from high-aluminum and low-silicon to high-silicon, and is suitable for applications such as coating, catalyst support, and ceramic precursor.
[0016] 3. This invention utilizes a process combining low-temperature co-hydrolysis with staged heating and reflux aging, followed by room-temperature aging, to obtain a silica-alumina sol with a stable pH in the 3-5 range. Example 1 shows a stable storage period of up to 6 months at room temperature, while Examples 2-4 show a stable storage period of 3-5 months, with no precipitation, gelation, or significant increase in particle size during storage. In contrast, the comparative samples, after deviating from the process parameters, exhibited turbidity, precipitation, or gel failure within a short period (hours to 15 days), demonstrating that the process conditions of this invention play a crucial role in maintaining the long-term stability of the colloid. Attached Figure Description
[0017] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used in conjunction with embodiments of the invention to explain the invention and do not constitute a limitation thereof. In the drawings: Figure 1 This is a flowchart of the method of the present invention. Detailed Implementation
[0018] The preferred embodiments of the present invention will be described below with reference to the accompanying drawings. It should be understood that the preferred embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.
[0019] Furthermore, in this invention, the use of terms such as "first" and "second" is for descriptive purposes only and does not specifically refer to any order or sequence, nor is it intended to limit the invention. They are merely used to distinguish components or operations described using the same technical terms and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined with "first" or "second" may explicitly or implicitly include at least one of those features. Additionally, the technical solutions and features of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. If a combination of technical solutions is contradictory or impossible to implement, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection claimed by this invention.
[0020] This invention provides a method for preparing silica-alumina sol, such as... Figure 1 ,include: 1. Preparation of aluminum source precursor solution: Add the aluminum source (aluminum isopropoxide, aluminum sec-butoxide) to anhydrous ethanol at a molar ratio of 1:3-1:15 (preferably 1:5-1:8). Add the anhydrous ethanol to the reaction vessel, then add the aluminum source. Stir at room temperature and 200-500 rpm for 0.5-3 hours until the aluminum source is completely dissolved, yielding a clear and transparent aluminum source precursor solution. 2. Silicon source (methyl silicate, ethyl silicate): The amount of silicon source to be fed should be determined according to the silicon-aluminum molar ratio of 1:0.02-1:5 (preferably 1:0.02-1:3).
[0021] 3. Preparation of acid catalytic aqueous solution: The molar ratio of silicon source to deionized water is 1:4-1:200 (preferably 1:20-1:100). Determine the amount of deionized water to be used. Mix deionized water and anhydrous ethanol at a volume ratio of 1:0.1-1:3 (preferably 1:0.5-1:1.5) until homogeneous. Slowly add 5%-20% by mass of nitric acid, hydrochloric acid, or sulfuric acid (preferably 5% nitric acid) under stirring at room temperature. Stir at a constant speed throughout the process and adjust the pH of the system to 2.5-4.5 (preferably 3-4.2) to obtain a homogeneous, transparent, and non-stratified acid catalytic aqueous solution for later use.
[0022] 4. Co-hydrolysis and polycondensation: Control the stirring speed at 300-800 r / min and the water bath temperature at 5-20℃, preferably 10-15℃. Slowly add the silicon source and acid-catalyzed aqueous solution dropwise into the aluminum source precursor liquid. During the process, keep the silicon source and acid-catalyzed aqueous solution added synchronously and at a uniform rate, and keep the start and end times of the addition consistent. Strictly control the addition time according to the silicon-aluminum molar ratio to control the hydrolysis and polymerization rate of silicon and aluminum: when the silicon-aluminum molar ratio is 1:0.02-1:2, the addition time of silicon source and acid-catalyzed aqueous solution is controlled at 0.5-5h; when the silicon-aluminum molar ratio is 1:2-1:5, the addition time of silicon source and acid-catalyzed aqueous solution is controlled at 3-12h.
[0023] 5. Heating and aging: Raise the water bath temperature to 30-75℃ (preferably 40-65℃), stir and reflux for 0.5-10h to promote further reaction, make the system components uniform, and improve the stability of the sol. After the reaction is completed, cool to room temperature and continue stirring and aging for 0.5-3h to finally obtain a narrow distribution non-agglomerated silica-alumina sol with a pH of 3-5 and a particle size of 5-50nm.
[0024] Example 1 (High aluminum, low silicon system, aluminum-silicon molar ratio Al:Si=1:0.02). Experimental setup: 0.2 mol aluminum isopropoxide was used as the aluminum source, and a 500 mL jacketed closed glass reactor was used. The entire process was carried out under a dry nitrogen atmosphere to avoid the alkoxide precursor absorbing moisture and hydrolyzing.
[0025] S1. Preparation of aluminum source precursor solution: Add aluminum source and anhydrous ethanol at a molar ratio of 1:6: 0.2 mol of aluminum isopropoxide (molar mass 204.24 g / mol), corresponding to a mass of 40.85 g; 1.2 mol of anhydrous ethanol, corresponding to a volume of approximately 70 mL.
[0026] Dry nitrogen gas was introduced into a 500mL sealed reactor to purge air, and 70mL of anhydrous ethanol was added. The stirring was started and the stirring speed was kept stable at 350r / min. 40.85g of aluminum isopropoxide was added at room temperature and the mixture was stirred continuously for 1.5h until the aluminum source was completely dissolved, resulting in a clear and transparent aluminum source precursor liquid. The system was kept sealed throughout the process.
[0027] S2. Prepare the silicon source: Weigh precisely according to the overall formula aluminum-silicon molar ratio Al:Si=1:0.02: 0.004mol of ethyl silicate, which corresponds to a volume of approximately 0.89mL.
[0028] Measure 0.89 mL of ethyl silicate under dry conditions, seal it and place it in a desiccator at room temperature for later use. Keep it dry and sealed throughout the process to prevent the silicon source from prematurely becoming damp and hydrolyzing.
[0029] S3. Preparation of acid-catalyzed aqueous solution: The amount of deionized water used is determined according to a silicon source to deionized water molar ratio of 1:50: 0.2 mol of deionized water is added, corresponding to a volume of 3.6 mL; and 3.6 mL of anhydrous ethanol is added according to a deionized water to anhydrous ethanol volume ratio of 1:1.
[0030] Add 3.6 mL of deionized water and 3.6 mL of anhydrous ethanol to a beaker and stir at room temperature until homogeneous. While stirring at a constant speed, slowly add 5% (w / w) dilute nitric acid solution dropwise using a microburette, monitoring the pH of the system in real time until the pH stabilizes at 3.5, resulting in a homogeneous, transparent, and non-layered acid-catalyzed aqueous solution, which is then sealed for later use.
[0031] S4, co-hydrolysis condensation: The reactor was connected to a constant-temperature water bath system, with the water bath temperature set at 12℃. The stirring was started and the rotation speed stabilized at 500 r / min. Two synchronous peristaltic pumps were used to simultaneously and uniformly drip the silicon source and acid-catalyzed aqueous solution into the aluminum source precursor liquid, respectively. The start and end times of the two dripping streams were exactly the same, and the total dripping time was controlled to be 2.5 h. The entire dripping process was sealed and a small amount of dry nitrogen was introduced to avoid excessively high local concentrations that could cause precipitation.
[0032] S5, Temperature-Induced Aging and Aging After the addition is complete, the temperature of the constant temperature water bath is raised to 50℃, the stirring speed is maintained at 500r / min, and the stirring and reflux reaction is carried out for 5 hours to promote further reaction, make the system components uniform, and improve the stability of the sol. After the reaction is completed, the heating is turned off, the water bath is allowed to cool naturally to room temperature, and stirring and aging are continued for 1.5 hours to finally obtain the finished silica-alumina sol.
[0033] Finished product performance parameters: Appearance: Clear and transparent liquid, without sediment or layering. pH value: 3.6 (measured directly at 25℃ using a precision pH meter) Particle size and distribution: Average particle size 12.5 nm, Particle size distribution index (PDI) = 0.08 (measured at 25 °C using dynamic light scattering (DLS) method, after diluting the sol to approximately 0.1% solid content). Dispersed state: No particle aggregation Storage stability: Stable period of ≥6 months when stored at room temperature in a sealed container, during which there is no precipitation, no gelation, and no significant increase in particle size.
[0034] Example 2 (low-to-medium aluminum system, silicon-to-aluminum molar ratio 1:1; aluminum source 0.2 mol sec-butoxide aluminum) Experimental setup: 0.2 mol sec-butoxide aluminum was used as the aluminum source, and a 500 mL jacketed closed glass reactor was used. The entire process was carried out under a dry nitrogen atmosphere to avoid the alkoxide precursor absorbing moisture and hydrolyzing.
[0035] S1. Preparation of aluminum source precursor solution: Select aluminum sec-butoxide as aluminum source, take 0.2 mol aluminum sec-butoxide (49.26 g); the molar ratio of aluminum source to anhydrous ethanol is 1:7, corresponding to 1.4 mol of anhydrous ethanol, with a volume of about 81.7 mL; Dry nitrogen gas was introduced into a 500 mL sealed reactor to purge the air. 81.7 mL of anhydrous ethanol was added, and the stirring was started and kept at a stable speed of 400 r / min. 49.26 g of aluminum sec-butoxide was added at room temperature, and the mixture was stirred continuously for 2 h until the aluminum source was completely dissolved, resulting in a clear and transparent aluminum source precursor liquid. The system was kept sealed throughout the process.
[0036] S2. Prepare the silicon source: Weigh 0.2 mol of ethyl silicate (41.67 g) according to the silicon-aluminum molar ratio of 1:1, and set aside.
[0037] Weigh 41.67g of ethyl silicate under dry conditions, seal it in a desiccator and let it stand at room temperature for later use. Keep it dry and sealed throughout the process to prevent the silicon source from being prematurely hydrolyzed by moisture.
[0038] S3. Prepare acid-catalyzed aqueous solution: the molar ratio of silicon source to deionized water is 1:60, corresponding to 12 mol (216 mL) of deionized water; the volume ratio of deionized water to anhydrous ethanol is 1:1.2, corresponding to 259.2 mL of anhydrous ethanol. Add 216 mL of deionized water and 259.2 mL of anhydrous ethanol to a beaker and stir at room temperature until homogeneous. While stirring at a constant speed, slowly add 5% dilute nitric acid solution dropwise using a microburette, monitoring the pH of the system in real time until the pH stabilizes at 3.8, resulting in a homogeneous, transparent, and non-layered acid-catalyzed aqueous solution, which is then sealed for later use.
[0039] S4. Co-hydrolysis and polycondensation: Connect the reactor to a constant temperature water bath system, set the water bath temperature to 10℃, start the stirrer and stabilize the speed at 600 r / min; use two synchronous peristaltic pumps to simultaneously and uniformly drop the silicon source and acid-catalyzed aqueous solution into the aluminum source precursor liquid, with the start and end times of the two drops being exactly the same, and the total dropping time controlled to 3 hours. The entire dropping process is sealed and a small amount of dry nitrogen is introduced to avoid excessively high local concentrations that may cause precipitation.
[0040] S5. Heating and aging: After the addition is completed, the temperature of the constant temperature water bath is raised to 55℃, the stirring speed is maintained at 600r / min, and the stirring and reflux reaction is carried out for 6 hours to promote further reaction, make the system components uniform, and improve the stability of the sol. After the reaction is completed, the heating is turned off, the water bath is naturally cooled to room temperature, and stirring and aging are continued for 2 hours to finally obtain the finished silica-alumina sol.
[0041] Finished product parameters: clear and transparent appearance; pH=3.9 (directly measured at 25℃ using a precision pH meter); average particle size 15.2nm, particle size distribution index PDI=0.10 (measured at 25℃ using dynamic light scattering (DLS) method, diluted to approximately 0.1% solid content by cumulative analysis); no agglomeration, no flocculent matter; stable at room temperature for ≥5 months, during which no precipitation, no gelation, and no significant increase in particle size occur.
[0042] Example 3 (medium-high aluminum system, silicon-aluminum molar ratio 1:3; aluminum source 0.2 mol aluminum isopropoxide) Experimental setup: 0.2 mol aluminum isopropoxide was used as the aluminum source, and a 500 mL jacketed closed glass reactor was used. The entire process was carried out under a dry nitrogen atmosphere to avoid the alkoxide precursor absorbing moisture and hydrolyzing.
[0043] S1. Preparation of aluminum source precursor solution: Select aluminum isopropoxide as the aluminum source, take 0.2 mol aluminum isopropoxide (40.85 g); the molar ratio of aluminum source to anhydrous ethanol is 1:5, corresponding to 1.0 mol of anhydrous ethanol, with a volume of about 58.4 mL.
[0044] Dry nitrogen gas was introduced into a 500mL sealed reactor to purge air, and 58.4mL of anhydrous ethanol was added. The stirring was started and the stirring speed was kept stable at 450r / min. 40.85g of aluminum isopropoxide was added at room temperature and the mixture was stirred continuously for 1h until the aluminum source was completely dissolved, resulting in a clear aluminum source precursor liquid. The system was kept sealed throughout the process.
[0045] S2. Preparation of silicon source: Weigh precisely according to the overall formula silicon-aluminum molar ratio of 1:3: 0.0667mol of methyl silicate, corresponding to a mass of 10.15g.
[0046] Weigh 10.15g of methyl silicate under dry conditions, seal it and place it in a desiccator at room temperature for later use. Keep it dry and sealed throughout the process to prevent the silicon source from being prematurely hydrolyzed by moisture.
[0047] S3. Preparation of acid-catalyzed aqueous solution: The amount of deionized water used was determined according to a silicon source to deionized water molar ratio of 1:80: 5.336 mol of deionized water was added, corresponding to a volume of 96.0 mL; and 76.8 mL of anhydrous ethanol was added according to a deionized water to anhydrous ethanol volume ratio of 1:0.8.
[0048] Add 96.0 mL of deionized water and 76.8 mL of anhydrous ethanol to a beaker and stir at room temperature until homogeneous. While stirring at a constant speed, slowly add 5% (w / w) dilute nitric acid solution dropwise using a microburette, monitoring the pH of the system in real time until the pH stabilizes at 3.2, resulting in a homogeneous, transparent, and non-layered acid-catalyzed aqueous solution, which is then sealed for later use.
[0049] S4, co-hydrolysis condensation: The reactor was connected to a constant-temperature water bath system, with the water bath temperature set at 15℃. The stirring was started and the rotation speed stabilized at 700 r / min. Two synchronous peristaltic pumps were used to simultaneously and uniformly drip the silicon source and acid-catalyzed aqueous solution into the aluminum source precursor liquid, respectively. The start and end times of the two dripping streams were exactly the same, and the total dripping time was controlled to be 6 hours. The entire dripping process was sealed and a small amount of dry nitrogen was introduced to avoid excessively high local concentrations that could cause precipitation.
[0050] S5, Temperature-Induced Aging and Aging After the addition is complete, the temperature of the constant temperature water bath is raised to 60℃, the stirring speed is maintained at 700r / min, and the stirring and reflux reaction is carried out for 8 hours to promote further reaction, make the system components uniform, and improve the stability of the sol. After the reaction is completed, the heating is turned off, the water bath is allowed to cool naturally to room temperature, and stirring and aging are continued for 2.5 hours to finally obtain the finished silica-alumina sol.
[0051] Finished product performance parameters: Appearance: Uniform, transparent liquid, without sediment or layering. pH value: 3.4 (measured directly at 25℃ using a precision pH meter) Particle size and distribution: Average particle size 18.6 nm, Particle size distribution index (PDI) = 0.12 (measured by dynamic light scattering (DLS) at 25 °C, after diluting the sol to approximately 0.1% solid content using the cumulative analysis method). Dispersion state: No aggregated particles; Storage stability: Stable period of ≥4 months when stored at room temperature in a sealed container, during which there is no precipitation, no gelation, and no significant increase in particle size.
[0052] Example 4 (High-alumina limiting system, silicon-aluminum molar ratio 1:5; aluminum source 0.2 mol sec-butoxide aluminum) Experimental setup: 0.2 mol sec-butoxide aluminum was used as the aluminum source, and a 500 mL jacketed closed glass reactor was used. The entire process was carried out under a dry nitrogen atmosphere to avoid the alkoxide precursor absorbing moisture and hydrolyzing.
[0053] S1. Preparation of aluminum source precursor solution: Select aluminum sec-butoxide as the aluminum source, take 0.2 mol aluminum sec-butoxide (49.26 g); the molar ratio of aluminum source to anhydrous ethanol is 1:8, corresponding to 1.6 mol of anhydrous ethanol, with a volume of about 93.3 mL.
[0054] Dry nitrogen gas was introduced into a 500 mL sealed reactor to purge air, and 93.3 mL of anhydrous ethanol was added. The stirring was started and the speed was kept stable at 300 r / min. 49.26 g of aluminum sec-butoxide was added at room temperature, and the mixture was stirred continuously for 2.5 h until the aluminum source was completely dissolved, resulting in a clear and transparent aluminum source precursor liquid. The system was kept sealed throughout the process.
[0055] S2. Preparation of silicon source: Weigh precisely according to the overall formula silicon-aluminum molar ratio of 1:5: 0.04mol of ethyl silicate, corresponding to a mass of 8.33g.
[0056] Weigh 8.33g of ethyl silicate under dry conditions, seal it in a desiccator and let it stand at room temperature for later use. Keep it dry and sealed throughout the process to prevent the silicon source from being prematurely hydrolyzed by moisture.
[0057] S3. Preparation of acid-catalyzed aqueous solution: The amount of deionized water used was determined according to a silicon source to deionized water molar ratio of 1:100: 4 mol of deionized water was added, corresponding to a volume of 72.0 mL; 108.0 mL of anhydrous ethanol was added according to a deionized water to anhydrous ethanol volume ratio of 1:1.5.
[0058] Add 72.0 mL of deionized water and 108.0 mL of anhydrous ethanol to a beaker and stir at room temperature until homogeneous. While stirring at a constant speed, slowly add 5% dilute nitric acid solution dropwise using a microburette, monitoring the pH of the system in real time until the pH stabilizes at 4.0, resulting in a homogeneous, transparent, and non-stratified acid-catalyzed aqueous solution, which is then sealed for later use.
[0059] S4, co-hydrolysis condensation: The reactor was connected to a constant-temperature water bath system, with the water bath temperature set at 13℃. The stirring was started and the rotation speed stabilized at 800 r / min. Two synchronous peristaltic pumps were used to simultaneously and uniformly drip the silicon source and acid-catalyzed aqueous solution into the aluminum source precursor liquid, respectively. The start and end times of the two dripping streams were exactly the same, and the total dripping time was controlled to be 10 hours. The entire dripping process was sealed and a small amount of dry nitrogen was introduced to avoid excessively high local concentrations that could cause precipitation.
[0060] S5, Temperature-Induced Aging and Aging After the addition is complete, the temperature of the constant temperature water bath is raised to 65℃, the stirring speed is maintained at 800r / min, and the stirring and reflux reaction is carried out for 9 hours to promote further reaction, make the system components uniform, and improve the stability of the sol. After the reaction is completed, the heating is turned off, the water bath is allowed to cool naturally to room temperature, and stirring and aging are continued for 3 hours to finally obtain the high-alumina silica-alumina sol product.
[0061] Finished product performance parameters: Appearance: Slightly transparent liquid, no sediment, no stratification. pH value: 4.1 (measured directly at 25℃ using a precision pH meter) Particle size and distribution: Average particle size 22.3 nm, Particle size distribution index (PDI) = 0.14 (measured by dynamic light scattering (DLS) at 25 °C, after diluting the sol to approximately 0.1% solid content using the cumulative analysis method). Dispersed state: No obvious aggregation Storage stability: Stable period of ≥3 months when stored at room temperature in a sealed container, during which there is no precipitation, no gelation, and no significant increase in particle size.
[0062] Comparative Example 1 The overall process is completely consistent with Example 4, with the only difference being: the silicon-aluminum molar ratio is 1:5 (high-aluminum system), and the slow dripping time of 3-12 hours is not used; only the dripping time is controlled to 2 hours. The remaining raw material ratios, temperature, rotation speed, pH, and aging parameters are all consistent with Example 4.
[0063] Finished product parameters: The system is turbid with white flocculent precipitate; pH=4.2; average particle size 58.7nm; PDI=0.42; severe agglomeration and extremely wide particle size distribution; stratification and gelation occur after standing at room temperature for 72h, with no storage stability.
[0064] Defect Description: The high-alumina system has extremely strong hydrolytic activity. Rapid dropwise addition causes instantaneous and localized excessive hydrolysis of the aluminum source, making it unable to co-condense with the silicon source, resulting in the formation of aluminum hydroxide agglomerates and disrupting the uniformity of the sol.
[0065] Comparative Example 2 The overall process is completely consistent with Example 2, with the only difference being that the co-hydrolysis condensation water bath temperature is increased to 28°C (exceeding the 5-20°C limit range of this invention), while all other parameters remain unchanged.
[0066] Finished product parameters: The system is slightly turbid with trace amounts of suspended particles; pH=4.0; average particle size 36.4nm; PDI=0.35; localized agglomeration is obvious; precipitation begins to appear after 15 days of storage at room temperature.
[0067] Defect Description: Excessive temperature accelerates the uncontrolled hydrolysis of aluminum alkoxides, resulting in an excessively fast nucleation rate, rapid particle growth and secondary aggregation, and an inability to form a narrow-distribution sol.
[0068] Comparative Example 3 The overall process is completely consistent with Example 3, with the only difference being that the pH of the acid-catalyzed aqueous solution is adjusted to 2.2 (lower than the lower limit of 2.5-4.5 of this invention), while the other raw material ratios and process parameters remain unchanged.
[0069] Finished product parameters: clear appearance but extremely low viscosity; pH=2.3; average particle size 9.8nm; PDI=0.38; thinning and instability occurs after 1 month of storage at room temperature.
[0070] Defect Description: H in a strong acid environment + Excessive concentration significantly inhibits the condensation reaction of silicon and aluminum species, promotes further reactions, makes the system components uniform, and improves the stability of the sol. However, it cannot grow completely, has a wide particle size distribution, unstable structure, and is prone to failure.
[0071] Comparative Example 4 The overall process is completely consistent with Example 1, with the only difference being that the volume ratio of deionized water to anhydrous ethanol in the acid-catalyzed aqueous solution is 1:0.05 (lower than the lower limit of 1:0.1 in this invention), resulting in extremely poor solvent compatibility. All other parameters remain unchanged.
[0072] Finished product parameters: The system shows obvious stratification, with a clear upper layer and a white turbid lower layer; pH=3.7; average particle size 49.2nm; PDI=0.45; large amount of agglomerate and precipitate; unable to form a homogeneous silica-alumina sol.
[0073] Defect Description: Insufficient ethanol solvent, poor compatibility between water and oil phases, local phase separation of the precursor during the dropwise addition process, inability to carry out synchronous silicon-aluminum hydrolysis, resulting in phase separation precipitation and complete loss of sol properties.
[0074] This invention optimizes the raw material ratio, hydrolysis kinetics, and aging process. Through a synergistic process of low-temperature reverse dripping and segmented temperature-controlled polycondensation aging, the particle size, solid content, and cross-linking structure of the silica-alumina sol are precisely controlled. The resulting silica-alumina sol is clear and transparent, with a narrow particle size distribution, no agglomeration, and excellent storage stability. It can meet the differentiated application needs of multiple fields. At the same time, the process is simple, the parameters are controllable, and the batch repeatability is good, making it suitable for large-scale production.
[0075] The beneficial effects of the above technical solution are as follows: 1. This invention employs a co-hydrolysis strategy involving the simultaneous and uniform dropwise addition of a silicon source and an acid-catalyzed aqueous solution to an aluminum source precursor liquid. Under low-temperature water bath conditions, the hydrolysis-condensation rates of the silicon and aluminum sources are matched to avoid excessive and rapid hydrolysis of any single component. Comparative Examples 1-4 demonstrate that when the dropwise rate is too fast, the hydrolysis temperature is too high, the system pH is outside the range of this invention, or the alcohol-water solvent ratio is unbalanced, the sol system exhibits significant agglomeration, turbidity, precipitation, and stratification. The silica-alumina sol prepared using the process conditions of this invention, as shown in Examples 1-4, yields clear, stratified sol products without particle agglomeration, overcoming the problems of phase separation and precipitation that easily occur during the co-hydrolysis of silica-alumina alkoxides.
[0076] 2. This invention can prepare silicon-aluminum sol in a silicon-aluminum molar ratio of 1:0.02-1:5. By adjusting process parameters such as dropping time, hydrolysis temperature, and aging temperature, the average particle size of the sol can be controlled within the range of 5-50 nm. In Example 1, a narrow-distribution sol with an average particle size of 12.5 nm and a PDI as low as 0.08 was obtained. Even with an increased silicon content, the PDI of the products in all examples was ≤0.14. In contrast, the comparative product with a PDI as high as 0.45, exceeding the process parameters of this invention, exhibited a wide particle distribution. This invention is adaptable to different composition requirements from high-aluminum and low-silicon to high-silicon, and is suitable for applications such as coating, catalyst support, and ceramic precursor.
[0077] 3. This invention utilizes a process combining low-temperature co-hydrolysis with staged heating and reflux aging, followed by room-temperature aging, to obtain a silica-alumina sol with a stable pH in the 3-5 range. Example 1 shows a stable storage period of up to 6 months at room temperature, while Examples 2-4 show a stable storage period of 3-5 months, with no precipitation, gelation, or significant increase in particle size during storage. In contrast, the comparative samples, after deviating from the process parameters, exhibited turbidity, precipitation, or gel failure within a short period (hours to 15 days), demonstrating that the process conditions of this invention play a crucial role in maintaining the long-term stability of the colloid.
[0078] In a preferred embodiment, before mass production, a preset combination of process parameters for the current raw material formula is obtained; during the mass production process, a mass production verification and adjustment process is first executed, which includes: S1-S4: Based on the preset process parameter combination of the current raw material formula, execute S1-S4, and detect the actual pH of the aluminum source precursor liquid before S4 addition and the actual pH of the reaction mixture after S4 addition to determine the actual pH change. Based on the actual pH change and the preset pH change, pre-correct the preset reflux time of S5 corresponding to the current raw material formula to obtain the pre-corrected reflux time of S5 corresponding to the current raw material formula. S5: Raise the water bath temperature to the preset water bath temperature corresponding to S5 of the current raw material formula, stir and reflux for the pre-corrected reflux time of S5 corresponding to the current raw material formula, cool to room temperature after stirring and reflux reaction is completed, detect the actual pH of the reaction material after cooling to room temperature after reflux, and determine the actual reflux pH change. The pre-corrected aging time of S5 corresponding to the current raw material formula is determined based on the actual pH change during addition and the actual pH change during reflux. The pre-corrected aging time of S5 corresponding to the current raw material formula is continued to be stirred and aged, and finally agglomerated silica-alumina sol with pH of 3-5 and particle size of 5-50nm is obtained.
[0079] (1) Before mass production, based on the fixed formula (specific raw materials and ratios) corresponding to mass production, the preset process parameter combination that meets the qualified production of silica-alumina sol is determined through experiments; here, qualified production requirements refer to the fact that the colloidal particle size (5-50nm), pH is 3-5, PDI (can be less than or equal to 0.25), no agglomeration and precipitation, etc. all meet the preset product acceptance indicators.
[0080] The preset process parameter combinations include: preset stirring speed for S1, preset pH of the acid-catalyzed aqueous solution for S3, preset stirring speed and preset water bath temperature for S4, preset dropping rate and preset dropping time of the silicon source and acid-catalyzed aqueous solution for S4, and preset water bath temperature, preset stirring reflux time, and preset aging time for S5. All of the above preset parameters (which can be fixed parameters or parameter ranges depending on the actual situation) satisfy the parameter range described in Example 1 above (S1 stirring at room temperature, 200-500 r / min, S3 acid-catalyzed aqueous solution...). The target pH is 2.5-4.5; for S4, the stirring speed is 300-800 r / min and the water bath temperature is 5-20℃. The silicon source and acid-catalyzed aqueous solution for S4 are added simultaneously and uniformly. When the silicon-aluminum molar ratio is 1:0.02-1:2, the addition time is controlled at 0.5-5 h; when the silicon-aluminum molar ratio is 1:2-1:5, the addition time is controlled at 3-12 h. The start and end times of the addition process are consistent. For S5, the preset water bath temperature is 30-75℃, the stirring and reflux time is 0.5-10 h, and the aging time is 0.5-3 h. For slight fluctuations in the system caused by raw material purity and trace impurities (differences between the raw material state and the experimentally determined preset process parameter combination), only minor adjustments to the stirring reflux time and aging time are allowed in step S5. The product is considered qualified if it meets the acceptance criteria after adjustment. Steps S1-S4 are executed according to the preset process parameters without parameter adjustments. If the product still fails to meet the acceptance criteria even after adjustments to the boundary of the fine-tuning fluctuation range, the raw material batch is deemed abnormal.
[0081] (2) Before mass production, based on the predetermined combination of process parameters for the current raw material formulation, a verification experiment is conducted using the predetermined combination of process parameters and the corresponding verification raw material batch (the raw material batch used when determining the predetermined combination of process parameters). The change in pH during addition and the change in pH during reflux are measured in the verification experiment. The change in pH during addition measured in this set of verification experiments is recorded as the predetermined change in pH during addition, and the change in pH during reflux measured in this set of verification experiments is recorded as the predetermined change in pH during reflux. The predetermined change in pH during addition and the predetermined change in pH during reflux are obtained by taking the average of the valid test results from multiple parallel verification experiments under the same verification raw material batch, and are used as a reference benchmark.
[0082] It should be noted that the preset pH change amount and preset reflux pH change amount are a set of reference recorded values obtained from the verification experiment, which are used as a reference benchmark and are not used as the qualification criteria for subsequent mass production.
[0083] (3) Actual pH change after dripping = Actual pH of the reaction mixture obtained after S4 dripping - Actual pH of the aluminum source precursor solution before S4 dripping; Determine: pH change ratio = actual pH change ÷ preset pH change; The actual pH change during the dropwise addition can serve as an empirical monitoring indicator of the reaction state during the dropwise addition stage. It has an empirical correlation with the overall progress of hydrolysis and pre-condensation of the system and the state of the primary colloidal core entering the reflux stage, and can be used to predict the relative deviation of the reaction progress. A slight deviation of the actual pH change from the preset pH change indicates a relatively slight reaction disturbance caused by factors such as the batch of raw materials. By adjusting the reflux time in advance, excessive aggregation or insufficient condensation during the reflux stage can be avoided.
[0084] Based on the pH change ratio during dropping, the pre-corrected reflux time for S5 corresponding to the current raw material formulation is determined as follows: This embodiment only addresses minor fluctuations caused by the raw materials, and the effective working range for the pH change ratio during addition is controlled between 0.95 and 1.05. If the pH change ratio during addition exceeds this range, it indicates that the deviation has exceeded the compensation range of the reflux process, and the raw material batch is directly determined to be abnormal, without further time correction.
[0085] Fine-tuning was performed within the small deviation range of 0.95-1.08. The pH change ratio during the dropwise addition was between (1.03, 1.08). The degree of hydrolysis and pre-condensation during the dropwise addition stage was slightly higher than the state corresponding to the preset reflux time. The reflux time after pre-correction was shortened by 1%-2% compared to the preset reflux time. When the pH change ratio during the dropwise addition is in the range of 0.90-0.95, the degree of hydrolysis and pre-condensation during the dropwise addition stage is slightly lower than the state corresponding to the preset reflux time. After pre-correction, the reflux time is extended by 1%-2% compared to the preset reflux time. The pH change ratio is between [0.95, 1.03], and the pre-corrected reflux time is directly used without adjustment.
[0086] (4) Actual reflux pH change = pH of the reaction mixture after cooling to room temperature after reflux - actual pH of the reaction mixture after S4 addition; Determine the reflux pH change ratio = actual reflux pH change ÷ preset reflux pH change; Based on the reflux pH change ratio and the dropwise pH change ratio, the pre-corrected aging time for S5 corresponding to the current raw material formulation is determined as follows: The effective working range for the reflux pH change ratio is controlled between 0.93 and 1.06. If the reflux pH change ratio exceeds this range, the disturbance exceeds the compensation capacity of the aging process, and the raw material batch is directly judged to be abnormal, and the aging time correction is not performed.
[0087] The pH change ratio during addition is only used to determine the direction of the reaction deviation. The adjustment range of the aging time is determined based on the range of the reflux pH change ratio. At the same time, the adjustment range is also determined by whether the directions of the pH change ratio during addition and the reflux pH change ratio are consistent.
[0088] pH change range for drop addition: [0.90-0.95] is negative deviation; (1.03, 1.08] is positive deviation; [0.95, 1.03] is the baseline range.
[0089] The reflux pH change range is as follows: (1.02, 1.06) indicates a positive deviation, with the condensation progress higher than the baseline; [0.93, 0.97) indicates a negative deviation, with the condensation progress lower than the baseline; and [0.97, 1.02] is the baseline range.
[0090] When the deviation direction of the pH change ratio during dropwise addition is consistent with the deviation direction of the pH change ratio during reflux, the activity of the gel core matches the reaction progress trend during the reflux stage, and the full adjustment range corresponding to the pH change ratio during reflux is directly adopted: When the reflux pH change is within the range of (1.02, 1.06), the aging time is shortened by 2%-4% compared to the preset aging time; The reflux pH change was within the range of [0.93, 0.97], and the aging time was 2%-4% longer than the preset aging time.
[0091] When the direction of pH change during addition is opposite to that during reflux, the activity of the gel core does not match the reaction progress trend during reflux. The aging effects brought by the two stages will antagonize each other. Therefore, the above-mentioned complete adjustment range is reduced, and the actual aging time adjustment range is controlled within 1-3%.
[0092] The pH change ratio during addition and the pH change ratio during reflux were both within the corresponding baseline range, so the preset aging time was used directly without adjustment.
[0093] The revised aging time should not fluctuate by more than ±6% of the preset value, and should not exceed the basic process range of 0.5-3 hours. If the product still fails to meet the acceptance criteria for particle size, PDI, and absence of agglomeration and sedimentation after adjustment to the boundary, the raw material batch is deemed abnormal. This correction only applies to minor reaction fluctuations caused by raw material batches; abnormalities caused by process parameter deviations or operational errors are not covered by this compensation. Mechanism of pH deviation correction for reflux time The dropping stage is the initial hydrolysis and pre-condensation stage of the silicon-aluminum source. By the end of the dropping stage, a large number of primary oligomers and nanoscale colloidal cores have been formed in the system. The degree of reaction in this stage directly determines the "initial base" of colloidal particle growth in the reflux stage. A pH change ratio greater than 1 (actual change greater than preset value) indicates a higher degree of hydrolysis and pre-condensation during the dropwise addition stage, resulting in more primary colloidal nuclei and higher surface activity. If the preset reflux time is continued, the risk of excessive particle growth and soft / hard agglomeration will increase significantly. Therefore, it is necessary to shorten the reflux time and control the total particle growth time to help the final particle size and dispersibility approach the target level.
[0094] A pH change ratio of <1 (actual change < preset value) indicates that the degree of hydrolysis and pre-condensation during the dropwise addition stage is low, resulting in a small number of primary colloidal nuclei and insufficient reactivity. If the preset reflux time is continued, the final particle size will be too small, the degree of cross-linking will be insufficient, and the colloidal storage stability will be poor. Therefore, it is necessary to extend the reflux time to supplement the condensation reaction time, which will help the colloidal particles develop towards the target particle size and degree of cross-linking.
[0095] 3. Mechanism of reflux pH deviation correcting aging time The reflux stage is the core stage for particle growth and bulk cross-linking. After reflux, the particle size distribution framework of the colloidal particles is basically formed. The role of the aging stage is to allow the remaining hydroxyl groups on the surface of the colloidal particles to continue to slowly condense, thereby improving the degree of cross-linking and storage stability of the colloid, while optimizing the uniformity of particle size distribution. A reflux pH change ratio > 1 (actual change > preset value) indicates a higher degree of condensation reaction during the reflux stage, a higher degree of cross-linking in the main body of the particles, and fewer remaining hydroxyl groups on the surface. If the preset aging time is continued, the particles may become over-cross-linked and aggregate. Therefore, it is necessary to shorten the aging time, control the degree of condensation in the later stage, and avoid the risk of aggregation.
[0096] A reflux pH change ratio < 1 (actual change < preset value) indicates insufficient condensation during the reflux stage, resulting in numerous residual hydroxyl groups on the particle surface, an incomplete colloidal network structure, and a tendency to settle during storage. Therefore, extending the aging time allows for more condensation opportunities for the remaining hydroxyl groups, which is beneficial for improving the degree of crosslinking and long-term stability of the colloidal particles.
[0097] Mechanism of the difference in adjustment magnitude between the same and opposite directions of the deviation: The aging time correction takes into account the deviations in both the dropping and reflux stages, and adjusts the magnitude based on whether the deviation directions are consistent. Essentially, it is the superposition and mutual antagonism of the effects of the two stages of reaction. Consistent deviation direction: If the reaction progress in both the dropping and reflux stages is simultaneously too high or too low, the effects of the two stages on the final degree of condensation are superimposed, resulting in a larger total deviation. For example, if both stages are too high, it indicates that the entire reaction from pre-condensation to particle growth is faster than the baseline, and the total deviation in the final degree of condensation is more prominent. Therefore, a full adjustment range is required to accommodate this accumulated total deviation.
[0098] The deviations are in opposite directions: the reaction progress in the two stages is high and low, and their effects on the final degree of condensation will antagonize each other. For example, if the reaction is faster in the dropping stage (more gel cores) and slower in the reflux stage (slower growth), the total deviation of the overall degree of condensation will be smaller than the deviation of a single stage. Therefore, it is necessary to attenuate the adjustment range to avoid over-correction that would cause the final product indicators to deviate in the opposite direction.
[0099] Applying the aforementioned phased correction process in large-scale production can compensate for deviations in reaction intensity caused by minor fluctuations in raw material purity and activity, reducing the risk of product non-conformity due to such raw material fluctuations. Multiple pilot-scale production trials have verified that, within the range of normal raw material fluctuations, issues such as particle size and dispersibility exceeding tolerances caused by slight raw material variations are significantly suppressed. The proportion of non-conforming batches due to this reason is significantly lower than when the correction process was not used, reducing production rework and improving process stability and production efficiency in the mass production stage.
[0100] The beneficial effects of the above technical solution are as follows: This solution addresses the issue of reaction behavior deviations caused by subtle differences in raw materials during mass production by establishing a phased and target-specific process fine-tuning approach. The solution maintains all process conditions for steps S1-S4 unchanged, utilizing pH changes at two key nodes to play different regulatory roles: the pH change during the dropping stage is primarily used to pre-correct the S5 reflux time, adapting to the actual state of the primary gel cores formed after dropping; the pH change during the reflux stage is primarily used to correct the subsequent aging time, adapting to the condensation basis of the system after particle growth and cross-linking are complete.
[0101] The indicators in the dropping stage reflect the degree of deviation in the nucleation process, allowing for adaptive adjustments to the reflux time during the particle growth stage. The indicators in the reflux stage reflect the actual state of the colloidal particles after cross-linking and growth. Combined with the deviation direction from the preceding dropping stage, the aging time is constrained and adjusted. When the deviation directions of the two stages are consistent, a full aging adjustment range is used to accommodate the reaction deviation caused by the cumulative effect of the two stages. When the deviation directions of the two stages are opposite, the aging adjustment range is narrowed to avoid overcorrection caused by a single indicator, which could introduce new colloidal performance deviations. At the same time, a floating boundary for the aging time is set, ensuring that the adjusted time remains within the original process window, thus constraining the degree of freedom in adjustment.
[0102] Simultaneously, a disturbance differentiation mechanism is set up. For slight fluctuations in raw material indicators within the adjustable range, the process is adapted through the aforementioned time adjustment. If the indicators exceed the adjustable range, it indicates that the raw material batch is abnormal, and the compensation adjustment is terminated. This avoids directly discarding raw materials under minor disturbances and also prevents ineffective production input from continuing to process abnormal raw materials, thus adapting to the needs of industrial quality control.
[0103] By adapting and adjusting the reflux time and aging time separately, the particle growth process and the later hydroxyl condensation aging process can be appropriately guided, which helps the colloidal particle size, PDI, pH and other indicators to approach the target range, improves the controllability of the colloidal crosslinking state and optimizes the colloidal storage stability.
[0104] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.
Claims
1. A method for preparing a silica-alumina sol, characterized in that: include: S1: Add the aluminum source and anhydrous ethanol in a molar ratio of 1:3-1:
15. Add the anhydrous ethanol to the reaction vessel, then add the aluminum source. Stir at room temperature and 200-500 r / min for 0.5-3 h until the aluminum source is completely dissolved to obtain the aluminum source precursor liquid. S2: Determine the amount of silicon source to be fed according to the silicon-aluminum molar ratio of 1:0.02-1:5; S3: Determine the amount of deionized water according to the molar ratio of silicon source to deionized water of 1:4-1:
200. Mix deionized water and anhydrous ethanol at a volume ratio of 1:0.1-1:
3. Add 5%-20% acid solution by mass under stirring at room temperature to adjust the pH of the mixture of deionized water, anhydrous ethanol and acid solution to 2.5-4.5 to obtain an acid-catalyzed aqueous solution. S4: Control the stirring speed to 300-800 r / min and the water bath temperature to 5-20℃. Drop the silicon source and acid catalytic aqueous solution into the aluminum source precursor liquid. During the process, keep the silicon source and acid catalytic aqueous solution added synchronously and at a uniform rate, and keep the start and end times of the addition consistent. When the silicon-aluminum molar ratio is 1:0.02-1:2, the addition time of the silicon source and acid catalytic aqueous solution is controlled at 0.5-5 h. When the silicon-aluminum molar ratio is 1:2-1:5, the addition time of the silicon source and acid catalytic aqueous solution is controlled at 3-12 h. S5: Raise the water bath temperature to 30-75℃, stir and reflux for 0.5-10h, cool to room temperature after the reaction is complete, and continue stirring and aging for 0.5-3h to finally obtain a silica-alumina sol with a pH of 3-5 and a particle size of 5-50nm.
2. The method for preparing a silica-alumina sol according to claim 1, characterized in that: The aluminum source includes either aluminum isopropoxide or aluminum sec-butoxide.
3. The method for preparing a silica-alumina sol according to claim 1, characterized in that: The acid solution includes any one of nitric acid, hydrochloric acid, and sulfuric acid.
4. The method for preparing a silica-alumina sol according to claim 1, characterized in that: The silicon source includes either methyl silicate or ethyl silicate.
5. The method for preparing a silica-alumina sol according to claim 1, characterized in that: In S4, the water bath temperature is raised to 40-65℃.
6. The method for preparing a silica-alumina sol according to claim 1, characterized in that: Acid solutions with a mass fraction of 5%-20% are nitric acid solutions with a mass fraction of 5%.
7. A silica-alumina sol, characterized in that: Prepared by any one of the methods for preparing silica-alumina sol as described in any one of claims 1-6.
Citation Information
Patent Citations
Preparation method of high-purity silica alumina sol
CN108854870A