By adding nanoporous materials to the silica aerogel and performing specific treatment, the problems of poor brittleness and thermal insulation properties of silica aerogel are solved, and higher mechanical and thermal insulation properties are achieved, suitable for large Scale application.

CN119038944APending Publication Date: 2024-11-29GUANGZHOU UNIVERSITY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411152751.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Due to poor brittleness and mechanical properties of silica aerogels, they have damaged their functions in large-scale applications, and the uneven dispersion of inorganic particles in the aerogels leads to low thermal insulation performance.

Method used

Nanoporous materials are used as reinforced phase and fully mixed with the silicon source precursor solution, adjust the pH value through acid and alkali catalysts, form a wet gel, and aged and dried under normal pressure to avoid agglomeration and shrinkage, and improve composite aerosol Glue uniformity and thermal insulation properties.

Benefits of technology

It improves the mechanical and thermal insulation properties of composite aerogels, ensures its stability and thermal insulation properties under medium and high temperature conditions, reduces the replacement rate of thermal insulation materials, and is simple in process and low in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038944A_ABST
    Figure CN119038944A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of silicon dioxide aerogel, in particular to nano porous material-silicon dioxide composite aerogel and a preparation method thereof. The specific preparation method comprises the following steps: taking a nano-porous material as a reinforcing phase, and fully mixing with a silicon source precursor solution to obtain a mixed solution; adjusting the pH value of the mixed solution to 4-5 by using an acid catalyst, and hydrolyzing to obtain silica sol; mixing the silica sol with a base catalyst, adjusting the pH value to 9-10, and standing to obtain wet gel; and after aging treatment and solvent replacement, drying to obtain the composite aerogel. On the basis of increasing the specific surface area and average pore size of the composite aerogel, the heat conductivity coefficient of the composite aerogel is reduced, and the heat insulation performance of the composite aerogel is improved. The problems that the mechanical property needs to be further improved due to the fact that the dispersion uniformity is difficult to control in the modification process of current silicon dioxide aerogel and the heat insulation performance is low due to local particle aggregation are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon dioxide aerogels, and in particular to a nanoporous material-silicon dioxide composite aerogel and a preparation method thereof. Background Art

[0002] Silica aerogel is a multifunctional nanomaterial with excellent properties such as light weight, low density, high specific surface area, high porosity, low dielectric constant and extremely low thermal conductivity. It has shown great application potential in many fields such as chemistry, thermal, acoustic, optical and electrical, especially in thermal insulation materials, adsorption materials, catalysts and their carriers. However, due to its great brittleness, poor mechanical properties and easy wear and breakage, the structure of silica aerogel is destroyed and its original function is lost, which seriously limits its potential in large-scale applications.

[0003] At present, the thermal insulation and mechanical properties of silica aerogels are mainly improved by modifying them. For example, some researchers have used inorganic fibers as reinforcement phases to prepare silica composite aerogels, which can significantly improve the mechanical properties of silica aerogels. However, the uniformity of the dispersion of inorganic fibers in aerogels is difficult to control, resulting in the need for further improvement in the mechanical properties of the composite materials.

[0004] In addition, in recent years, in order to enhance the properties of silica aerogel, some researchers have mixed inorganic particles into silica aerogel to improve the thermal insulation performance of silica aerogel. However, due to the problem of weak interface and uneven dispersion between inorganic particles and silica aerogel, local particle agglomeration can easily lead to excessive local density, and even inorganic particles may fall off during use, thereby reducing the thermal insulation performance of the composite material. Summary of the invention

[0005] In order to solve the problem that the dispersion uniformity of silica aerogel is difficult to control during the modification process, resulting in the need for further improvement in mechanical properties, and the problem that local particle agglomeration leads to low thermal insulation performance, the purpose of the present invention is to provide a nanoporous material-silica composite aerogel and a preparation method thereof.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows.

[0007] The first aspect of the present invention provides a method for preparing a nanoporous material-silicon dioxide composite aerogel, comprising the following steps:

[0008] A nanoporous material is used as a reinforcing phase and is fully mixed with a silicon source precursor solution to obtain a mixed solution; the nanoporous material is any one of zeolite, sepiolite, diatomite, vermiculite, porous calcium silicate, montmorillonite, hydrotalcite, MXene, ZIF-8, and halloysite;

[0009] The pH of the mixed solution is adjusted to 4-5 by using an acid catalyst, and silica sol is obtained by hydrolysis;

[0010] The silica sol is mixed with an alkali catalyst to adjust the pH to 9-10, and the mixture is allowed to stand to obtain a wet gel; after aging treatment and solvent replacement, the mixture is dried to obtain a composite aerogel.

[0011] The invention facilitates the uniform dispersion of the nanoporous material in the silicon source precursor solution through ultrasonic treatment, avoids agglomeration, ensures the uniformity of the composite material performance, and improves the thermal insulation performance.

[0012] The role of the acid catalyst is to adjust the pH to a certain acidic range and promote the hydrolysis reaction of the silicon source to generate silicic acid monomers or oligomers.

[0013] The role of the alkaline catalyst is to adjust the pH to a certain alkaline range, which is conducive to the polycondensation reaction between silicate monomers or oligomers to form a wet gel with a three-dimensional network structure.

[0014] The aging process helps to further stabilize and strengthen the internal structure of the wet gel and improve product performance. Use low surface tension solvents such as n-hexane to replace the moisture and residual solvent inside the wet gel to reduce shrinkage and cracking during the drying process.

[0015] Preferably, the nanoporous material is vermiculite.

[0016] Preferably, the particle size of the nanoporous material is 50 nm to 100 nm.

[0017] Preferably, the silicon source precursor solution is prepared by mixing a silicon source with a solvent; the solvent is a mixture of at least two of water, ethylene glycol methyl ether, and ethanol. Among them, ethanol is a good organic solvent.

[0018] More preferably, the mass ratio of the silicon source to the nanoporous material is 20.8-100:0.1-50, for example, 20.8:0.1, 20.8:3, 20.8:50, 100:0.1, 100:3, 100:50, etc.

[0019] More preferably, the silicon source is any one of water glass, fly ash and tetraethyl orthosilicate.

[0020] More preferably, the molar ratio of silicon source, water and ethylene glycol methyl ether is 0.1-0.48:0.5:0.1-0.13, for example, 0.1:0.5:0.1, 0.1:0.5:0.11, 0.1:0.5:0.12, 0.1:0.5:0.13, 0.48:0.5:0.13, etc.

[0021] Preferably, the hydrolysis conditions are: hydrolysis temperature is 45°C to 50°C, and hydrolysis time is 1.5h to 2h.

[0022] Preferably, the nanoporous material is used as the reinforcing phase and is fully mixed with the silicon source precursor solution by using ultrasound to fully mix the nanoporous material and the silicon source precursor solution.

[0023] Preferably, the aging treatment is to place the wet gel at room temperature under normal pressure for 12 hours to 24 hours; for example, 12 hours

[0024] The solvent used in the solvent replacement process is n-hexane, and the time of solvent replacement is 12h to 24h;

[0025] The drying is carried out at normal pressure, and the drying conditions are: the drying temperature is 120°C, and the drying time is 6h to 12h.

[0026] Preferably, the acid catalyst is any one of acetic acid solution, hydrochloric acid solution, and formic acid solution, and the concentration of the acid catalyst is 0.4 mol / L to 0.5 mol / L;

[0027] The base catalyst is any one of an aqueous ammonia solution and a sodium hydroxide solution, and the concentration of the base catalyst is 0.4 mol / L to 0.5 mol / L. Both the acid catalyst and the base catalyst are aqueous solution systems prepared with water.

[0028] The second aspect of the present invention provides a nanoporous material-silicon dioxide composite aerogel prepared by the preparation method described in the first aspect.

[0029] Preferably, the specific surface area of ​​the nanoporous material-silicon dioxide composite aerogel is 3349.15 m 2 / g~5698.30m 2 / g, average pore size is 1.35nm~3.35nm, thermal conductivity is 0.01w / m -1 k -1 ~0.04w / m -1 k -1 .

[0030] Beneficial effects of the present invention:

[0031] 1. The present invention mainly uses nanoporous materials as reinforcing phases and silicon dioxide as cross-linking phases, and utilizes nanoporous materials with larger pores to strengthen the skeleton structure of the composite aerogel and inhibit the shrinkage of the composite aerogel under medium and high temperature conditions. On the basis of increasing the specific surface area and average pore size of the composite aerogel, the thermal conductivity of the composite aerogel is reduced, and the thermal insulation performance of the composite aerogel is improved.

[0032] 2. The present invention adopts normal pressure drying, which is simple to operate, low in cost, and is conducive to large-scale promotion in the later stage.

[0033] 3. The composite aerogel prepared by the present invention can be used as a thermal insulation material to improve thermal insulation performance and reduce the replacement rate of thermal insulation materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Infrared spectra of the composite aerogel prepared in Example 3 and the silica aerogel prepared in Comparative Example 1.

[0035] Figure 2 These are nitrogen adsorption-desorption curves of the composite aerogels prepared in Examples 1 to 3 and the silica aerogel prepared in Comparative Example 1.

[0036] Figure 3 The pore size distribution curves of the composite aerogels prepared in Examples 1 to 3 and the silica aerogel prepared in Comparative Example 1 are shown.

[0037] Figure 4 This is a comparative bar chart of thermal conductivity of the composite aerogels prepared in Examples 1 to 3 and the silica aerogel prepared in Comparative Example 1. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0039] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.

[0040] Compared with the traditional preparation method of silica aerogel, under high temperature conditions, the nano three-dimensional network structure of silica aerogel will be severely damaged and the pores will collapse, resulting in a decrease in its specific surface area and a reduction in pore size, thereby reducing its thermal insulation performance.

[0041] Porous materials are materials with a network structure consisting of interconnected or closed pores, with the boundaries or surfaces of the pores composed of pillars. They have a large specific surface area and excellent flame retardant properties. When nanoporous materials are mixed into silica aerogels, their mechanical and thermal insulation properties are effectively improved.

[0042] The present invention aims to pre-add nanoporous materials to silicon source precursors and mix them thoroughly, thereby preparing nanoporous material-doped silica composite aerogels by a sol-gel method. Among them, silica is used as a cross-linking phase to obtain a three-dimensional network structure with high specific surface area and porosity; the nanoporous material is used as a reinforcing phase to enhance the skeleton structure of the composite aerogel and inhibit the shrinkage of the composite aerogel under medium and high temperature conditions.

[0043] In the present invention, the nanoporous material is any one of zeolite, sepiolite, diatomite, vermiculite, porous calcium silicate, montmorillonite, hydrotalcite, MXene, ZIF-8, and halloysite; the particle size of the nanoporous material is 50nm to 100nm; the nanoporous material is commercially available. Among them, the pore size of zeolite is less than 1nm, and the specific surface area is 1000m 2 / g. The specific surface area of ​​sepiolite is 900m 2 / g. The specific surface area of ​​diatomite is about 48m 2 / g. The average pore size of vermiculite is 2nm, and the specific surface area is 13m 2 / g. The content of CaSiO3·xH2O in porous calcium silicate accounts for more than 95%, with rich microporous structure and specific surface area of ​​152m 2 / g. Montmorillonite, Rojet K-10, with a specific surface area of ​​240m 2 / g. The specific surface area of ​​hydrotalcite is about 100m 2 / g. MXene is Ti3C2 nanosheet powder with a specific surface area of ​​20m 2 / g. ZIF-8 is 2-methylimidazole zinc salt, CAS number is 59061-53-9, pore size is 0.34nm~1.16nm, specific surface area>1400m 2 / g. Halloysite, specific surface area 35~87m 2 / g, from Chenxi County, Hunan Province.

[0044] In addition, the drying methods of silica aerogel include supercritical drying, freeze drying and ambient pressure drying. Supercritical drying has the problem of expensive equipment and complicated operation. Freeze drying allows the liquid in the pores to sublimate, but it is possible to destroy the aerogel network structure. When drying under ambient pressure, the capillary pressure difference in the gel pores is likely to exceed the elastic limit of the three-dimensional skeleton structure of silica, causing the internal structure to be destroyed. The above drying methods all have the problems of high energy consumption and difficulty in retaining the complete three-dimensional structure. The present invention adopts a normal pressure drying method to avoid the high energy consumption and high cost problems of methods such as supercritical drying and freeze drying, and can ensure that a complete three-dimensional network structure is obtained.

[0045] In the present invention, the silicon source precursor solution is prepared by mixing a silicon source with a solvent; the solvent is a mixture of at least two of water, ethylene glycol methyl ether, and ethanol. The silicon source is any one of water glass, fly ash, and tetraethyl orthosilicate. Among them, ethanol is a good organic solvent that can dissolve silanols, which are the hydrolysis products of tetraethyl orthosilicate. In addition, the addition of ethanol can also adjust the speed of the sol-gel process, and affect the gel time by changing the interaction between ethanol and silanols. In addition, the volatilization rate of ethanol also affects the pore structure of the aerogel. By controlling the evaporation rate of ethanol, the porosity and pore size distribution of the aerogel can be regulated to a certain extent.

[0046] The present invention uses nanoporous materials as reinforcing phases, dopes them into silica aerogels, and dries them under ambient pressure, with low production costs. The present invention combines the high porosity of silica aerogels with the heat insulation, high temperature resistance, and flame retardancy of nanoporous materials in a preparation method for composite aerogels, meeting the application needs of more fields.

[0047] The nanoporous material-silicon dioxide composite aerogel and its preparation method of the present invention are further described below by specific examples. The methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are all commercially available unless otherwise specified.

[0048] In the following embodiments, the nanoporous material is selected from any one of montmorillonite, MXene and vermiculite, and all are purchased. Among them, montmorillonite, Rojet K-10, has a specific surface area of ​​240m 2 / g. MXene is titanium carbide nanosheets, the main component of which is Ti3C2, with a purity of >95% and a specific surface area of ​​20m 2 / g, Heshi new material. The average pore size of vermiculite is about 2nm, and the specific surface area is about 13m 2 / g or so.

[0049] In the following examples, the standing time is between 1 h and 6 h.

[0050] Example 1

[0051] A method for preparing a nanoporous material-silicon dioxide composite aerogel comprises the following steps:

[0052] Step 1, using tetraethyl orthosilicate as a silicon source, adding 20.8 g of tetraethyl orthosilicate, 9 g of deionized water, and 10 g of ethylene glycol methyl ether into a 200 mL beaker, stirring at room temperature for 10 min to prepare a silicon source precursor solution; wherein the molar ratio of the silicon source, deionized water, and ethylene glycol methyl ether is 0.1:0.5:0.13.

[0053] Step 2, add 3g of montmorillonite to the silicon source precursor solution, ultrasonically disperse for 10min to mix the system evenly, cool to room temperature, use 0.5mol / L acetic acid solution as an acidic catalyst, add the acidic catalyst dropwise and adjust the solution pH to 4-5, react in a 50°C water bath for 2h to fully hydrolyze the silicon source to obtain silica sol.

[0054] Step 3, taking out the silica sol, cooling it to room temperature, using 0.5 mol / L sodium hydroxide solution as an alkaline catalyst, adding the alkaline catalyst dropwise and adjusting the solution pH to 9-10, mixing evenly, and letting it stand to obtain a wet gel.

[0055] Step 4: placing the wet gel at room temperature for 12 to 24 hours for aging. After aging, adding n-hexane for solvent replacement for 12 hours.

[0056] Step 5, drying the wet gel after solvent replacement at normal pressure and drying at 120° C. for 6 hours, and obtaining montmorillonite-silica composite aerogel after drying.

[0057] Example 2

[0058] A method for preparing a nanoporous material-silicon dioxide composite aerogel comprises the following steps:

[0059] Step 1, using tetraethyl orthosilicate as a silicon source, adding 20.8g of tetraethyl orthosilicate as a silicon source, 9g of deionized water, 10g of ethylene glycol methyl ether and 25g of anhydrous ethanol into a 200mL beaker, stirring at room temperature for 10 minutes, to prepare a silicon source precursor solution, wherein the molar ratio of the silicon source, deionized water and ethylene glycol methyl ether is 0.1:0.5:0.13.

[0060] Step 2: Add 3 g of MXene to the silicon source precursor solution, perform ultrasonic dispersion for 10 min to mix the system evenly, cool to room temperature, use 0.5 mol / L hydrochloric acid solution as an acidic catalyst, add the acidic catalyst dropwise and adjust the solution pH to 4-5, react in a 50 ° C water bath for 2 h to fully hydrolyze the silicon source to obtain silica sol.

[0061] Step 3, taking out the silica sol, cooling it to room temperature, using 0.5 mol / L sodium hydroxide solution as an alkaline catalyst, adding the alkaline catalyst dropwise and adjusting the solution pH to 9-10, mixing evenly, and letting it stand to obtain a wet gel.

[0062] Step 4: placing the wet gel at room temperature for 12 to 24 hours for aging. After aging, adding n-hexane for solvent replacement for 12 hours.

[0063] Step 5, drying the wet gel after solvent replacement at normal pressure and drying at 120° C. for 6 h. After drying, a MXene-silica composite aerogel is obtained.

[0064] Example 3

[0065] A method for preparing a nanoporous material-silicon dioxide composite aerogel comprises the following steps:

[0066] Step 1, using tetraethyl orthosilicate as a silicon source, adding 100g of tetraethyl orthosilicate as a silicon source, 9g of deionized water, and 10g of ethylene glycol methyl ether into a 200mL beaker, stirring at room temperature for 10 minutes, and preparing a silicon source precursor solution, wherein the molar ratio of the silicon source, deionized water, and ethylene glycol methyl ether is 0.48:0.5:0.13.

[0067] Step 2, add 3g of vermiculite to the silicon source precursor solution, ultrasonically disperse for 10min to mix the system evenly, cool to room temperature, use 0.5mol / L formic acid solution as an acidic catalyst, add the acidic catalyst dropwise and adjust the solution pH to 4-5, react in a 50°C water bath for 2h to fully hydrolyze the silicon source to obtain silica sol.

[0068] Step 3, taking out the silica sol, cooling it to room temperature, adding a 0.5 mol / L ammonia aqueous solution as an alkaline catalyst and adjusting the solution pH to 9-10, mixing well, and letting it stand to obtain a wet gel.

[0069] Step 4: placing the wet gel at room temperature for 12 to 24 hours for aging. After aging, adding n-hexane for solvent replacement for 12 hours.

[0070] Step 5, drying the wet gel after solvent replacement at normal pressure and drying at 120° C. for 6 hours, and after drying, obtaining vermiculite-silicon dioxide composite aerogel.

[0071] Example 4

[0072] A method for preparing a nanoporous material-silicon dioxide composite aerogel comprises the following steps:

[0073] Step 1, using tetraethyl orthosilicate as a silicon source, adding 20.8g of tetraethyl orthosilicate as a silicon source, 9g of deionized water, and 10g of ethylene glycol methyl ether into a 200mL beaker, stirring at room temperature for 10 minutes, and preparing a silicon source precursor solution, wherein the molar ratio of the silicon source, deionized water, and ethylene glycol methyl ether is 0.1:0.5:0.13.

[0074] Step 2, add 0.1g of vermiculite to the silicon source precursor solution, ultrasonically disperse for 10min to mix the system evenly, cool to room temperature, use 0.5mol / L acetic acid solution as an acidic catalyst, add the acidic catalyst dropwise and adjust the solution pH to 4-5, react in a 50°C water bath for 2h to fully hydrolyze the silicon source to obtain silica sol.

[0075] Step 3, taking out the silica sol, cooling it to room temperature, using 0.5 mol / L sodium hydroxide solution as an alkaline catalyst, adding the alkaline catalyst dropwise and adjusting the solution pH to 9-10, mixing evenly, and letting it stand to obtain a wet gel.

[0076] Step 4: placing the wet gel at room temperature for 12 to 24 hours for aging. After aging, adding n-hexane for solvent replacement for 12 hours.

[0077] Step 5, drying the wet gel after solvent replacement at normal pressure and drying at 120° C. for 6 hours, and obtaining montmorillonite-silica composite aerogel after drying.

[0078] Example 5

[0079] A method for preparing a nanoporous material-silicon dioxide composite aerogel comprises the following steps:

[0080] Step 1, using tetraethyl orthosilicate as a silicon source, adding 20.8g of tetraethyl orthosilicate as a silicon source, 9g of deionized water, and 10g of ethylene glycol methyl ether into a 200mL beaker, stirring at room temperature for 10 minutes, and preparing a silicon source precursor solution, wherein the molar ratio of the silicon source, deionized water, and ethylene glycol methyl ether is 0.1:0.5:0.13.

[0081] Step 2, add 10g of montmorillonite to the silicon source precursor solution, ultrasonically disperse for 10 minutes to mix the system evenly, cool to room temperature, use 0.5mol / L acetic acid solution as an acidic catalyst, add the acidic catalyst dropwise and adjust the solution pH to 4-5, react in a 50°C water bath for 2h to fully hydrolyze the silicon source to obtain silica sol.

[0082] Step 3, taking out the silica sol, cooling it to room temperature, using 0.5 mol / L sodium hydroxide solution as an alkaline catalyst, adding the alkaline catalyst dropwise and adjusting the solution pH to 9-10, mixing evenly, and letting it stand to obtain a wet gel.

[0083] Step 4: placing the wet gel at room temperature for 12 to 24 hours for aging. After aging, adding n-hexane for solvent replacement for 12 hours.

[0084] Step 5, drying the wet gel after solvent replacement at normal pressure and drying at 120° C. for 6 hours, and obtaining montmorillonite-silica composite aerogel after drying.

[0085] Example 6

[0086] A method for preparing a nanoporous material-silicon dioxide composite aerogel comprises the following steps:

[0087] Step 1, using tetraethyl orthosilicate as a silicon source, adding 100g of tetraethyl orthosilicate as a silicon source, 9g of deionized water, and 10g of ethylene glycol methyl ether into a 200mL beaker, stirring at room temperature for 10 minutes, and preparing a silicon source precursor solution, wherein the molar ratio of the silicon source, deionized water, and ethylene glycol methyl ether is 0.48:0.5:0.13.

[0088] Step 2, add 50g of montmorillonite to the silicon source precursor solution, ultrasonically disperse for 10min to mix the system evenly, cool to room temperature, use 0.5mol / L acetic acid solution as an acidic catalyst, add the acidic catalyst dropwise and adjust the solution pH to 4-5, react in a 50°C water bath for 2h to fully hydrolyze the silicon source to obtain silica sol.

[0089] Step 3, taking out the silica sol, cooling it to room temperature, using 0.5 mol / L sodium hydroxide solution as an alkaline catalyst, adding the alkaline catalyst dropwise and adjusting the solution pH to 9-10, mixing evenly, and letting it stand to obtain a wet gel.

[0090] Step 4: placing the wet gel at room temperature for 12 to 24 hours for aging. After aging, adding n-hexane for solvent replacement for 12 hours.

[0091] Step 5, drying the wet gel after solvent replacement at normal pressure and drying at 120° C. for 6 hours, and obtaining montmorillonite-silica composite aerogel after drying.

[0092] Comparative Example 1

[0093] A method for preparing a silica aerogel comprises the following steps:

[0094] Step 1, using tetraethyl orthosilicate as a silicon source, adding 20.8g of tetraethyl orthosilicate as a silicon source, 9g of deionized water, and 10g of ethylene glycol methyl ether into a 200mL beaker, stirring at room temperature for 10 minutes, and preparing a silicon source precursor solution, wherein the molar ratio of the silicon source, deionized water, and ethylene glycol methyl ether is 0.1:0.5:0.13.

[0095] Step 2: add 0.5 mol / L acetic acid solution as an acidic catalyst to the silicon source precursor solution, adjust the pH of the solution to 4-5, and react in a 50° C. water bath for 2 h to fully hydrolyze the silicon source to obtain silica sol.

[0096] Step 3, taking out the silica sol, cooling it to room temperature, using 0.5 mol / L sodium hydroxide solution as an alkaline catalyst, adding the alkaline catalyst dropwise and adjusting the solution pH to 9-10, mixing evenly, and letting it stand to obtain a wet gel.

[0097] Step 4: placing the wet gel at room temperature for 12 to 24 hours for aging. After aging, adding n-hexane for solvent replacement for 12 hours.

[0098] Step 5, drying the wet gel after solvent replacement at normal pressure and drying at 120° C. for 6 hours, and obtaining silica aerogel after drying.

[0099] The nanoporous material-silicon dioxide composite aerogel prepared in Examples 1 to 6 is referred to as composite aerogel for short; the composite aerogel prepared in Examples 1 to 6 and the silica aerogel prepared in Comparative Example 1 were used as samples to conduct infrared spectroscopy analysis, specific surface area and average pore size analysis, and thermal insulation performance analysis.

[0100] Table 1 Raw materials of each sample

[0101]

[0102] Note: “-” means not added.

[0103] Test 1: Infrared spectroscopy.

[0104] The composite aerogel prepared in Example 3 and the silica aerogel prepared in Comparative Example 1 were tested by infrared spectroscopy. The test results are shown in Figure 1 . Figure 1 Infrared spectra of the composite aerogel prepared in Example 3 and the silica aerogel prepared in Comparative Example 1.

[0105] Depend on Figure 1 The results show that the composite aerogel prepared in Example 3 and the silica aerogel prepared in Comparative Example 1 show similar characteristics in the infrared spectrum, indicating that the two have similarities in chemical structure or functional groups. The reinforcing phase added to the composite aerogel does not significantly change the main chemical structure of the silica matrix. Therefore, in the infrared spectrum, the characteristic absorption peak of the reinforcing phase may be weak or masked by the strong absorption peak of silica.

[0106] Test 2: Specific surface area and average pore size analysis.

[0107] The specific surface area and average pore size of the composite aerogels prepared in Examples 1 to 6 and the silica aerogel prepared in Comparative Example 1 were measured using a specific surface area and pore size analyzer according to the static volumetric nitrogen adsorption method. The results are shown in Figure 2 and Figure 3 As shown in Table 2.

[0108] Table 2 Specific surface area and average pore size of each sample

[0109] sample Specific surface area Average pore size Example 1 <![CDATA[3567.78m 2 / g]]> 1.90nm Example 2 <![CDATA[3349.15m 2 / g]]> 1.80nm Example 3 <![CDATA[4589.79m 2 / g]]> 1.68nm Example 4 <![CDATA[3400.34m 2 / g]]> 1.35nm Example 5 <![CDATA[5608.13m 2 / g]]> 2.15nm Example 6 <![CDATA[5698.30m 2 / g]]> 3.35nm Comparative Example 1 <![CDATA[1120.651m 2 / g]]> 1.537nm

[0110] Depend on Figure 2 and Figure 3 As can be seen from the results in Table 2, the nitrogen adsorption-desorption isotherms of the composite aerogels prepared in Examples 1 to 3 and the silica aerogel prepared in Comparative Example 1 all belong to type IV curves and present an H3 type hysteresis loop, indicating that these four different aerogels are typical mesoporous materials. Among them, compared with the specific surface area and average pore size of the silica aerogel in Comparative Example 1, the specific surface area and average pore size of the composite aerogel prepared in Example 3 are relatively large, which is mainly due to the doping of vermiculite in Example 3 and the more sufficient and stable hydrolysis condensation of the silicon source.

[0111] However, the specific surface areas and average pore sizes of Examples 1 and 2 are relatively small, and the smaller desorption pore size will lead to an increase in the flow resistance of gas molecules in the composite aerogel.

[0112] This shows that doping with vermiculite is more helpful to increase the specific surface area and average pore size of the composite aerogel.

[0113] From the data analysis of Examples 3 to 6, it can be seen that as the amount of vermiculite increases from 0.1g to 50g, the specific surface area and average pore size of the composite aerogel both show an increasing trend, which shows that the amount of ethyl orthosilicate in the range of 20.8g to 100g has little effect on the specific surface area and average pore size of the composite aerogel. The changes in the specific surface area and average pore size of the composite aerogel are positively correlated with the amount of nanoporous material used.

[0114] Test 3: Thermal insulation performance analysis.

[0115] The thermal insulation performance of the composite aerogels prepared in Examples 1 to 6 and the silica aerogel prepared in Comparative Example 1 was analyzed. The thermal insulation performance analysis was tested using a thermal conductivity measuring instrument. The results are as follows: Figure 4 And as shown in Table 3.

[0116] Table 3 Thermal conductivity of each sample

[0117] sample Thermal conductivity Example 1 <![CDATA[0.01w / m -1 k -1 ]]> Example 2 <![CDATA[0.021w / m -1 k -1 ]]> Example 3 <![CDATA[0.01w / m -1 k -1 ]]> Example 4 <![CDATA[0.04w / m -1 k -1 ]]> Example 5 <![CDATA[0.03w / m -1 k -1 ]]> Example 6 <![CDATA[0.03w / m -1 k -1 ]]> Comparative Example 1 <![CDATA[0.042w / m -1 k -1 ]]>

[0118] Note: The smaller the thermal conductivity, the better the thermal insulation performance.

[0119] from Figure 4 As can be seen from Table 3, compared with Comparative Example 1, the thermal conductivity of the composite aerogels prepared in Examples 1 to 6 is lower than that of Comparative Example 1, which shows that the composite aerogels prepared in Examples 1 to 6 of the present invention all have relatively low thermal conductivity, indicating that the addition of nanoporous materials can help improve the thermal insulation performance of the composite aerogels.

[0120] In Examples 1 to 3, doping with different nanoporous materials will lead to a decrease in thermal conductivity, while the thermal conductivity of the composite aerogel doped with vermiculite is relatively low. This is mainly because after doping with vermiculite, the vermiculite has larger pores and can support the three-dimensional pore structure without collapse, resulting in a lower thermal conductivity of the composite aerogel, thereby enhancing the thermal insulation performance of the composite silica aerogel.

[0121] In Examples 3 to 6, as the amount of vermiculite added increases from 0.1 g to 3 g, the thermal conductivity of the composite aerogel increases from 0.04 w / m -1 k -1 Reduced to 0.01w / m -1 k -1 When the amount of vermiculite increased from 3g to 10g, the thermal conductivity of the composite aerogel increased from 0.01w / m -1 k -1 Increase to 0.03w / m -1 k -1 ; Then, as the amount of vermiculite added increased to 50g, the thermal conductivity of the composite aerogel did not change. This shows that the optimal amount of vermiculite added is 0.1g to 10g. When the amount of vermiculite added is 3g, the thermal conductivity of the composite aerogel is the lowest, and the thermal insulation performance of the composite aerogel prepared at this time is the best.

[0122] The above analysis shows that the nanoporous material-silicon dioxide composite aerogel prepared by adding nanoporous materials such as vermiculite in the embodiment of the present invention can enhance the thermal insulation performance on the basis of increasing the specific surface area and average pore size of the composite aerogel. The composite aerogel prepared with nanoporous materials such as vermiculite as the reinforcing phase can be used as a thermal insulation material to improve the thermal insulation performance and reduce the replacement rate of thermal insulation materials.

[0123] It is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a nanoporous material-silicon dioxide composite aerogel, characterized in that: The following steps are involved: A nanoporous material is used as a reinforcing phase and is fully mixed with a silicon source precursor solution to obtain a mixed solution; the nanoporous material is any one of zeolite, sepiolite, diatomite, vermiculite, porous calcium silicate, montmorillonite, hydrotalcite, MXene, ZIF-8, and halloysite; The pH of the mixed solution is adjusted to 4-5 by using an acid catalyst, and silica sol is obtained by hydrolysis; The silica sol is mixed with an alkali catalyst to adjust the pH to 9-10 to obtain a wet gel; after aging treatment and solvent replacement, the gel is dried to obtain a composite aerogel.

2. The method for preparing the nanoporous material-silicon dioxide composite aerogel according to claim 1, characterized in that: The particle size of the nanoporous material is 50nm-100nm.

3. The method for preparing the nanoporous material-silicon dioxide composite aerogel according to claim 1, characterized in that: The silicon source precursor solution is prepared by mixing a silicon source with a solvent; the solvent is a mixture of at least two of water, ethylene glycol methyl ether and ethanol.

4. The method for preparing the nanoporous material-silicon dioxide composite aerogel according to claim 3, characterized in that: The mass ratio of the silicon source to the nanoporous material is 20.8-100:0.1-50.

5. The method for preparing the nanoporous material-silicon dioxide composite aerogel according to claim 3, characterized in that: The silicon source is any one of water glass, fly ash and tetraethyl orthosilicate.

6. The method for preparing the nanoporous material-silicon dioxide composite aerogel according to claim 3, characterized in that: The molar ratio of silicon source, water and ethylene glycol methyl ether is 0.1-0.48:0.5:0.1-0.

13.

7. The method for preparing the nanoporous material-silicon dioxide composite aerogel according to claim 1, characterized in that: The conditions for hydrolysis are: hydrolysis temperature is 45°C to 50°C, and hydrolysis time is 1.5h to 2h.

8. The method for preparing the nanoporous material-silicon dioxide composite aerogel according to claim 1, characterized in that: The aging treatment is to place the wet gel at normal pressure and room temperature for 12h to 24h; The solvent used in the solvent replacement process is n-hexane, and the time of solvent replacement is 12h to 24h; The drying is carried out under normal pressure, and the drying conditions are as follows: the drying temperature is 120°C, and the drying time is 6h to 12h.

9. The method for preparing the nanoporous material-silicon dioxide composite aerogel according to claim 1, characterized in that: The acid catalyst is any one of acetic acid solution, hydrochloric acid solution and formic acid solution, and the concentration of the acid catalyst is 0.4 mol / L to 0.5 mol / L; The alkali catalyst is any one of an aqueous ammonia solution and a sodium hydroxide solution, and the concentration of the alkali catalyst is 0.4 mol / L to 0.5 mol / L.

10. A nanoporous material-silicon dioxide composite aerogel prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Self-repairing vacuum insulation panel based on MOF-aerogel composite core material and preparation method of self-repairing vacuum insulation panel

    CN120116558A

  • Silicon dioxide aerogel with high resilience and low thermal conductivity as well as preparation method and application of silicon dioxide aerogel

    CN120440904A