An indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, its preparation method and application
By using indium-zirconium co-doped two-dimensional TiO2 nanosheets and carbon black composite photocatalysts, the problem of TiO2-based photocatalysts being easily poisoned and deactivated in the presence of H2S was solved, the photoresponse range was expanded, the selectivity and stability of methanol were improved, and the efficient resource utilization of CO2 in biogas was realized.
Patent Information
- Application Number
- CN202611334299.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing TiO2-based photocatalysts are easily poisoned and deactivated in H2S atmospheres, have low visible light utilization, severe recombination of photogenerated carriers, insufficient CO2 adsorption and activation capacity, and poor long-term stability, making it difficult to meet the needs of CO2 resource utilization in biogas.
A composite photocatalyst combining indium-zirconium co-doped two-dimensional TiO2 nanosheets and carbon black was constructed. By controlling the band gap width and surface electronic structure through indium-zirconium synergistic doping, and combining carbon black as an electron transport medium, a conductive network was built, optimizing the active crystal facets and adsorption activation capabilities.
It maintains high catalytic activity under hydrogen sulfide conditions, extends the photoresponse range to the visible light region, improves methanol selectivity and yield, enhances catalyst stability, and is suitable for the conversion of CO2 in anaerobic fermentation biogas without deep desulfurization.
Smart Images

Figure CN123102333A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photocatalytic materials and carbon resource utilization technology, and particularly relates to an indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, its preparation method and application. Background Technology
[0002] Anaerobic fermentation is a major biotechnological approach for treating organic waste and producing biogas. Biogas, as a renewable and clean energy source, mainly consists of CH4 and CO2, with CO2 typically comprising 30-45% by volume. In traditional biogas purification and utilization processes, this CO2 is often directly emitted or used only for low-value-added purposes, resulting in a waste of carbon resources and an increase in greenhouse gas emissions. In recent years, research on using photocatalysis to reduce CO2 to methanol has received widespread attention. Methanol not only has high energy density but can also be used directly as a liquid fuel or chemical feedstock, exhibiting good compatibility with existing energy infrastructure. Therefore, photocatalytic CO2 to methanol production is considered one of the ideal pathways for achieving carbon resource recycling.
[0003] Among existing photocatalytic CO2 reduction to methanol catalyst systems, TiO2-based materials have become the most widely studied main photocatalysts due to their advantages such as good chemical stability, non-toxicity, and relatively low cost. However, existing TiO2 photocatalytic systems face a series of unresolved technical bottlenecks when applied to practical biogas component scenarios.
[0004] First, actual biogas generally contains a certain concentration of H2S, typically ranging from 50 to 5000 ppm. The presence of H2S leads to a sharp decline in the activity of traditional TiO2-based photocatalysts, even causing irreversible deactivation. This is because H2S molecules undergo strong chemical adsorption or reaction with active sites on the catalyst surface, resulting in sulfur poisoning. This means that biogas without deep desulfurization treatment cannot be directly used in existing photocatalytic CO2 conversion systems, while the deep desulfurization process itself increases process complexity and operating costs. Second, TiO2 has a wide band gap, typically around 3.2 eV, and can only respond to ultraviolet light, which accounts for only about 4% of the solar spectrum, resulting in low solar energy utilization efficiency. Furthermore, the photogenerated electron-hole pair recombination rate of single TiO2 materials is relatively fast, resulting in unsatisfactory quantum efficiency. Simultaneously, its surface has limited adsorption and activation capacity for CO2, leading to poor product selectivity and the easy simultaneous generation of multiple byproducts such as CO, CH4, and HCOOH. The selectivity for methanol needs improvement. More importantly, most catalysts lack long-term stability under actual operating conditions, and the active components are prone to loss or aggregation, making it difficult to meet the needs of industrial applications.
[0005] In summary, the key technical problems that urgently need to be solved in order to realize the resource utilization of CO2 in biogas are how to maintain high catalytic activity in the presence of H2S, avoid sulfur poisoning and deactivation, expand the photoresponse range, suppress carrier recombination, improve methanol selectivity, and effectively couple the catalyst with the anaerobic fermentation biogas production process. Summary of the Invention
[0006] To address the problems of existing photocatalysts such as easy poisoning and deactivation in H2S atmosphere, low visible light utilization, severe recombination of photogenerated carriers, insufficient CO2 adsorption activation capacity, and poor long-term stability, this invention provides an indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, its preparation method, and its application.
[0007] The technical solution of this invention:
[0008] An indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst is disclosed. The composite photocatalyst uses two-dimensional TiO2 nanosheets as a substrate, wherein the lattice of the two-dimensional TiO2 nanosheets is doped with indium and zirconium, wherein the molar ratio of indium to titanium is 0.5~5:100, and the molar ratio of zirconium to titanium is 1~8:100; the surface of the two-dimensional TiO2 nanosheets is loaded with carbon black, and the loading amount of carbon black is 0.5~3.0 wt% based on the total mass of the composite photocatalyst.
[0009] Furthermore, the molar ratio of indium to titanium is 1~3:100, the molar ratio of zirconium to titanium is 3~6:100, and the loading of carbon black is 1.5wt%.
[0010] Furthermore, the two-dimensional TiO2 nanosheets have a thickness of 2~10 nm, a lateral dimension of 50~500 nm, and exposed {001} active crystal planes.
[0011] A method for preparing a composite photocatalyst includes the following steps:
[0012] Step 1: Titanium source, indium source and zirconium source are subjected to hydrothermal or solvothermal reaction at 160~240℃ in the presence of hydrofluoric acid for 8~72h to obtain indium-zirconium co-doped two-dimensional TiO2 nanosheets.
[0013] Step 2: Mix the obtained indium-zirconium co-doped two-dimensional TiO2 nanosheets with carbon black in a solvent, disperse them ultrasonically, evaporate the solvent, and calcine them at 250~500℃ for 2~4h under an inert atmosphere to obtain the composite photocatalyst.
[0014] Furthermore, the titanium source is tetrabutyl titanate, the indium source is indium nitrate or indium chloride, and the zirconium source is zirconium oxychloride or zirconium nitrate.
[0015] Furthermore, the hydrothermal or solvothermal reaction temperature in step one is 180~220℃, and the reaction time is 12~48h.
[0016] Furthermore, in step two, the solvent is anhydrous ethanol, the mass-to-volume ratio of the indium-zirconium co-doped two-dimensional TiO2 nanosheets, carbon black, and anhydrous ethanol is 1.0 g: 0.005~0.03 g: 100 mL, the ultrasonic dispersion time is 0.5~2 h, and the calcination temperature is 300~450 °C.
[0017] Application of a composite photocatalyst or a composite photocatalyst prepared by the method of the present invention in the photocatalytic reduction of CO2 to methanol.
[0018] Furthermore, the composite photocatalyst is dispersed in a reaction system containing H2O as a proton source, and the amount of the composite photocatalyst is 0.5~5 g / L. Under light conditions, biogas produced by anaerobic fermentation is introduced to carry out the photocatalytic reaction, the partial pressure of CO2 is 0.1~0.5 MPa, and methanol is collected after 2~12 h of reaction.
[0019] Furthermore, the illumination is simulated sunlight or visible light with a wavelength of not less than 420nm, the concentration of H2S in the biogas is 0~5000ppm, and the reaction temperature is 15~60℃.
[0020] The beneficial effects of this invention are:
[0021] This invention achieves a significant synergistic effect through the organic combination of indium-zirconium co-doping, two-dimensional nanosheet morphology control, and carbon black composite. Indium doping effectively narrows the band gap of titanium dioxide, extending the photoresponse range into the visible light region; zirconium doping introduces Lewis acid sites and oxygen vacancies that preferentially adsorb and convert hydrogen sulfide, protecting the active sites for carbon dioxide reduction from sulfur poisoning; carbon black, acting as an electron transport medium, constructs a conductive network, effectively suppressing photogenerated carrier recombination; and the highly active {001} crystal facets exposed by the two-dimensional nanosheets enhance the adsorption and activation capacity of carbon dioxide, improving methanol selectivity. Through the coupling of these multiple mechanisms, the composite photocatalyst of this invention maintains high catalytic activity and excellent sulfur resistance under hydrogen sulfide-containing conditions; the photoresponse range is extended to the visible light region, significantly improving solar energy utilization efficiency; methanol yield is greatly increased, and product distribution is controllable; the catalyst lattice structure stability is enhanced, and combined with the mechanical support and conductive network effect of carbon black, the activity decay is small under long-term continuous operation, demonstrating good reliability for industrial applications.
[0022] Performance verification experiments show that, under simulated sunlight irradiation, the optimal catalyst In / Zr-TNS-1.5 of this invention achieves a methanol yield of 28.5 μmol·g. -1 ·h -1The catalyst exhibited a 19-fold increase in activity compared to unmodified two-dimensional titanium dioxide nanosheets, and significantly outperformed single-component doped samples. After continuous reaction for 5 hours under 50 ppm hydrogen sulfide conditions, the catalyst retained 75% of its activity, far exceeding the 30% retention of pure titanium dioxide nanosheets. UV-Vis diffuse reflectance spectroscopy confirmed that the band gap decreased from 3.20 eV to 3.05 eV after co-doping, and the absorption edge red-shifted to 405–410 nm.
[0023] The photocatalyst provided by this invention can be directly used for the in-situ photocatalytic conversion of carbon dioxide in anaerobic fermentation biogas that has not undergone deep desulfurization, converting the carbon dioxide component in the biogas into methanol fuel. This achieves a closed-loop carbon cycle from organic waste through biogas to methanol and then to energy chemicals, aligning with the strategic needs of a circular economy and carbon neutrality. All raw materials used are non-precious metals, the preparation process is mature, and it has good prospects for industrial scale-up, providing a practical and feasible technical path for the resource utilization of carbon dioxide in biogas. Attached Figure Description
[0024] Figure 1 A bar chart comparing the methanol yields of different samples in Experiment Example 1;
[0025] Figure 2 The UV-Vis diffuse reflectance spectra and magnified views of 350-450 nm for different samples in Experiment Example 2 are shown.
[0026] Figure 3 This is a graph showing the relative activity of different samples in Experiment 3 as a function of reaction time under 50 ppm H2S conditions;
[0027] Figure 4 These are scanning electron microscope images of different samples in Example 4;
[0028] Figure 5 X-ray photoelectron spectra of different samples in Example 4;
[0029] Figure 6 The X-ray powder diffraction patterns are for different samples in Experiment Example 4. Detailed Implementation
[0030] The technical solution of the present invention will be further described below with reference to embodiments, but it is not limited thereto. Any modifications or equivalent substitutions to the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be covered within the protection scope of the present invention. In the following embodiments, the process equipment or apparatus not specifically specified are all conventional equipment or apparatus in the art. Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commercially available; unless otherwise specified, the technical means used in the embodiments of the present invention are all conventional means well known to those skilled in the art.
[0031] Example 1
[0032] This embodiment provides a method for preparing an indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, the steps of which are as follows:
[0033] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol. Indium nitrate hydrate (In(NO3)3·xH2O) and zirconium oxychloride hydrate (ZrOCl2·8H2O) are added as indium and zirconium sources, respectively, at a molar ratio of indium to titanium of 2:100 and a molar ratio of zirconium to titanium of 5:100. Stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while continuously stirring, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL polytetrafluoroethylene-lined high-pressure reactor, seal it, and place it in an oven for hydrothermal reaction at 200 °C for 24 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The white precipitate was collected by centrifugation and washed three times each with deionized water and anhydrous ethanol. The precipitate was then dried under vacuum at 80°C for 12 hours to obtain indium zirconium co-doped two-dimensional TiO2 nanosheets.
[0034] Step 2: Take 1.0 g of the indium-zirconium co-doped two-dimensional TiO2 nanosheets obtained in Step 1 and 0.015 g of carbon black, add them to 100 mL of anhydrous ethanol, and ultrasonically disperse for 2 h to form a uniform suspension. Stir the obtained suspension in an 80 °C water bath to evaporate the solvent, transfer the resulting solid powder to a tube furnace, and calcine it at a heating rate of 5 °C / min to 350 °C under nitrogen atmosphere protection for 3 h. After naturally cooling to room temperature, grind it to obtain the indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, denoted as In / Zr-TNS-1.5.
[0035] The composite photocatalyst obtained in this embodiment uses the two-dimensional TiO2 nanosheets prepared in step one as a substrate. The thickness of the two-dimensional TiO2 nanosheets is 2~10 nm, the lateral size is 50~500 nm, and they have highly exposed {001} active crystal planes. Indium and zirconium elements are introduced in situ into the lattice of the two-dimensional TiO2 nanosheets. The Lewis acid sites and oxygen vacancies introduced by zirconium doping can preferentially adsorb and oxidize H2S to elemental sulfur (S). 0Indium doping, or zirconium sulfate, fixes the CO2 reduction active sites on the catalyst surface in specific regions, thus protecting them from sulfur poisoning. Simultaneously, indium doping effectively narrows the band gap of TiO2, extending the photoresponse range from the ultraviolet region to the visible light region (absorbing up to 550 nm), which is beneficial for expanding the material's photoresponse range and improving the utilization of visible light. A considerable methanol yield can be achieved under visible light (λ≥420 nm) irradiation. Indium-zirconium synergistic doping regulates the surface electronic structure and active site distribution. At the same time, a tight interfacial contact and electron transport channel are formed between the two-dimensional TiO2 nanosheets and the carbon black loaded on their surface. The carbon black, acting as an electron transport medium, effectively suppresses carrier recombination, which is beneficial for promoting CO2 conversion to methanol and improving the selectivity of methanol formation.
[0036] Example 2
[0037] This embodiment provides a method for preparing an indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, the steps of which are as follows:
[0038] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol. Indium nitrate hydrate (In(NO3)3·xH2O) and zirconium oxychloride hydrate (ZrOCl2·8H2O) are added as indium and zirconium sources, respectively, at a molar ratio of indium to titanium of 2:100 and a molar ratio of zirconium to titanium of 5:100. Stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while continuously stirring, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL polytetrafluoroethylene-lined high-pressure reactor, seal it, and place it in an oven for hydrothermal reaction at 200 °C for 24 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The white precipitate was collected by centrifugation and washed three times each with deionized water and anhydrous ethanol. The precipitate was then dried under vacuum at 80°C for 12 hours to obtain indium zirconium co-doped two-dimensional TiO2 nanosheets.
[0039] Step 2: Take 1.0 g of the indium-zirconium co-doped two-dimensional TiO2 nanosheets obtained in Step 1 and 0.005 g of carbon black, add them to 100 mL of anhydrous ethanol, and ultrasonically disperse for 2 h to form a uniform suspension. Stir the obtained suspension in an 80 °C water bath to evaporate the solvent, transfer the resulting solid powder to a tube furnace, and calcine it at a heating rate of 5 °C / min to 350 °C under nitrogen atmosphere protection for 3 h. After naturally cooling to room temperature, grind it to obtain the indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, denoted as In / Zr-TNS-0.5.
[0040] Example 3
[0041] This embodiment provides a method for preparing an indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, the steps of which are as follows:
[0042] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol. Indium nitrate hydrate (In(NO3)3·xH2O) and zirconium oxychloride hydrate (ZrOCl2·8H2O) are added as indium and zirconium sources, respectively, at a molar ratio of indium to titanium of 2:100 and a molar ratio of zirconium to titanium of 5:100. Stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while continuously stirring, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL polytetrafluoroethylene-lined high-pressure reactor, seal it, and place it in an oven for hydrothermal reaction at 200 °C for 24 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The white precipitate was collected by centrifugation and washed three times each with deionized water and anhydrous ethanol. The precipitate was then dried under vacuum at 80°C for 12 hours to obtain indium zirconium co-doped two-dimensional TiO2 nanosheets.
[0043] Step 2: Take 1.0 g of the indium-zirconium co-doped two-dimensional TiO2 nanosheets obtained in Step 1 and 0.03 g of carbon black, add them to 100 mL of anhydrous ethanol, and ultrasonically disperse for 2 h to form a uniform suspension. Stir the obtained suspension in an 80 °C water bath to evaporate the solvent. Transfer the resulting solid powder to a tube furnace, heat it to 350 °C at a rate of 5 °C / min under nitrogen atmosphere protection, calcine it at this temperature for 3 h, and then grind it after naturally cooling to room temperature to obtain the indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, denoted as In / Zr-TNS-3.0.
[0044] Example 4
[0045] This embodiment provides a method for preparing an indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, the steps of which are as follows:
[0046] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol. Indium nitrate hydrate (In(NO3)3·xH2O) and zirconium oxychloride hydrate (ZrOCl2·8H2O) are added as indium and zirconium sources, respectively, at a molar ratio of indium to titanium of 0.5:100 and a molar ratio of zirconium to titanium of 1:100. Stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while continuously stirring, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL polytetrafluoroethylene-lined high-pressure reactor, seal it, and place it in an oven for hydrothermal reaction at 160 °C for 72 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The white precipitate was collected by centrifugation and washed three times each with deionized water and anhydrous ethanol. The precipitate was then dried under vacuum at 80°C for 12 hours to obtain indium zirconium co-doped two-dimensional TiO2 nanosheets.
[0047] Step 2: Take 1.0 g of the indium-zirconium co-doped two-dimensional TiO2 nanosheets obtained in Step 1 and 0.015 g of carbon black, add them to 100 mL of anhydrous ethanol, and ultrasonically disperse for 2 h to form a uniform suspension. Stir the obtained suspension in an 80 °C water bath to evaporate the solvent, transfer the resulting solid powder to a tube furnace, and calcine it at a heating rate of 5 °C / min to 250 °C under nitrogen atmosphere protection for 4 h. After naturally cooling to room temperature, grind to obtain the indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst.
[0048] Example 5
[0049] This embodiment provides a method for preparing an indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, the steps of which are as follows:
[0050] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol. Indium nitrate hydrate (In(NO3)3·xH2O) and zirconium oxychloride hydrate (ZrOCl2·8H2O) are added as indium and zirconium sources, respectively, at a molar ratio of indium to titanium of 1:100 and a molar ratio of zirconium to titanium of 3:100. Stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while continuously stirring, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL polytetrafluoroethylene-lined high-pressure reactor, seal it, and place it in an oven for hydrothermal reaction at 180 °C for 48 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The white precipitate was collected by centrifugation and washed three times each with deionized water and anhydrous ethanol. The precipitate was then dried under vacuum at 80°C for 12 hours to obtain indium zirconium co-doped two-dimensional TiO2 nanosheets.
[0051] Step 2: Take 1.0 g of the indium-zirconium co-doped two-dimensional TiO2 nanosheets obtained in Step 1 and 0.015 g of carbon black, add them to 100 mL of anhydrous ethanol, and ultrasonically disperse for 2 h to form a uniform suspension. Stir the obtained suspension in an 80 °C water bath to evaporate the solvent, transfer the resulting solid powder to a tube furnace, and calcine it at a heating rate of 5 °C / min to 300 °C under nitrogen atmosphere protection for 3 h. After naturally cooling to room temperature, grind to obtain the indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst.
[0052] Example 6
[0053] This embodiment provides a method for preparing an indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, the steps of which are as follows:
[0054] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol. Indium nitrate hydrate (In(NO3)3·xH2O) and zirconium oxychloride hydrate (ZrOCl2·8H2O) are added as indium and zirconium sources, respectively, at a molar ratio of indium to titanium of 3:100 and a molar ratio of zirconium to titanium of 6:100. Stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while continuously stirring, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL high-pressure reactor lined with polytetrafluoroethylene (PTFE), seal it, and place it in an oven for hydrothermal reaction at 220 °C for 12 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The white precipitate was collected by centrifugation and washed three times each with deionized water and anhydrous ethanol. The precipitate was then dried under vacuum at 80°C for 12 hours to obtain indium zirconium co-doped two-dimensional TiO2 nanosheets.
[0055] Step 2: Take 1.0 g of the indium-zirconium co-doped two-dimensional TiO2 nanosheets obtained in Step 1 and 0.015 g of carbon black, add them to 100 mL of anhydrous ethanol, and ultrasonically disperse for 2 h to form a uniform suspension. Stir the obtained suspension in an 80 °C water bath to evaporate the solvent, transfer the resulting solid powder to a tube furnace, and calcine it at a heating rate of 5 °C / min to 450 °C under nitrogen atmosphere protection for 2 h. After naturally cooling to room temperature, grind to obtain the indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst.
[0056] Example 7
[0057] This embodiment provides a method for preparing an indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, the steps of which are as follows:
[0058] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol. Indium nitrate hydrate (In(NO3)3·xH2O) and zirconium oxychloride hydrate (ZrOCl2·8H2O) are added as indium and zirconium sources, respectively, at a molar ratio of indium to titanium of 5:100 and a molar ratio of zirconium to titanium of 8:100. Stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while continuously stirring, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL high-pressure reactor lined with polytetrafluoroethylene (PTFE), seal it, and place it in an oven for hydrothermal reaction at 240 °C for 8 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The white precipitate was collected by centrifugation and washed three times each with deionized water and anhydrous ethanol. The precipitate was then dried under vacuum at 80°C for 12 hours to obtain indium zirconium co-doped two-dimensional TiO2 nanosheets.
[0059] Step 2: Take 1.0 g of the indium-zirconium co-doped two-dimensional TiO2 nanosheets obtained in Step 1 and 0.015 g of carbon black, add them to 100 mL of anhydrous ethanol, and ultrasonically disperse for 2 h to form a uniform suspension. Stir the obtained suspension in an 80 °C water bath to evaporate the solvent, transfer the resulting solid powder to a tube furnace, and calcine it at a heating rate of 5 °C / min to 500 °C under nitrogen atmosphere protection for 2 h. After naturally cooling to room temperature, grind to obtain the indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst.
[0060] Comparative Example 1
[0061] This comparative example provides a method for preparing unmodified two-dimensional TiO2 nanosheets without indium zirconium or carbon black, the steps of which are as follows:
[0062] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol and stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while stirring continuously, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL high-pressure reactor lined with polytetrafluoroethylene (PTFE), seal it, and place it in an oven for hydrothermal reaction at 200 °C for 24 h. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to collect the white precipitate, wash it three times each with deionized water and anhydrous ethanol, and vacuum dry it at 80 °C for 12 h to obtain unmodified two-dimensional TiO2 nanosheets, denoted as Pure-TNS.
[0063] Comparative Example 2
[0064] This comparative example provides a method for preparing two-dimensional TiO2 nanosheets without indium zirconium doping but loaded with carbon black, the steps of which are as follows:
[0065] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol and stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while stirring continuously, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL high-pressure reactor lined with polytetrafluoroethylene (PTFE), seal it, and place it in an oven for hydrothermal reaction at 200 °C for 24 h. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to collect the white precipitate, wash it three times each with deionized water and anhydrous ethanol, and vacuum dry it at 80 °C for 12 h to obtain unmodified two-dimensional TiO2 nanosheets.
[0066] Step 2: Take 1.0 g of the unmodified two-dimensional TiO2 nanosheets obtained in Step 1 and 0.005 g of carbon black, add them to 100 mL of anhydrous ethanol, and ultrasonically disperse for 2 h to form a uniform suspension. Stir the obtained suspension in an 80 °C water bath to evaporate the solvent. Transfer the resulting solid powder to a tube furnace, heat it to 500 °C at a rate of 5 °C / min under nitrogen atmosphere protection, calcine it at this temperature for 2 h, and then grind it after naturally cooling to room temperature to obtain unmodified two-dimensional TiO2 nanosheets with a carbon black loading of 0.5 wt%, denoted as Pure-TNS-0.5.
[0067] Comparative Example 3
[0068] The only difference between this comparative example and comparative example 2 is that in step two, 1.0 g of the unmodified two-dimensional TiO2 nanosheets obtained in step one and 0.015 g of carbon black are added to 100 mL of anhydrous ethanol to finally obtain unmodified two-dimensional TiO2 nanosheets with a carbon black loading of 1.5 wt%, denoted as Pure-TNS-1.5.
[0069] Comparative Example 4
[0070] The only difference between this comparative example and comparative example 2 is that in step two, 1.0 g of the unmodified two-dimensional TiO2 nanosheets obtained in step one and 0.03 g of carbon black are added to 100 mL of anhydrous ethanol to finally obtain unmodified two-dimensional TiO2 nanosheets with a carbon black loading of 3.0 wt%, denoted as Pure-TNS-3.0.
[0071] Comparative Example 5
[0072] This comparative example provides a method for preparing indium-zirconium co-doped two-dimensional TiO2 nanosheets, the steps of which are as follows:
[0073] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol. Indium nitrate hydrate (In(NO3)3·xH2O) and zirconium oxychloride hydrate (ZrOCl2·8H2O) are added as indium and zirconium sources, respectively, at a molar ratio of indium to titanium of 2:100 and a molar ratio of zirconium to titanium of 5:100. Stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while continuously stirring, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL polytetrafluoroethylene-lined high-pressure reactor, seal it, and place it in an oven for hydrothermal reaction at 200 °C for 24 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature. The white precipitate was collected by centrifugation and washed three times each with deionized water and anhydrous ethanol. The precipitate was then dried under vacuum at 80°C for 12 hours to obtain indium-zirconium co-doped two-dimensional TiO2 nanosheets, denoted as In / Zr-TNS.
[0074] Comparative Example 6
[0075] This comparative example provides a method for preparing indium-doped two-dimensional TiO2 nanosheets, the steps of which are as follows:
[0076] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol. Add indium nitrate hydrate (In(NO3)3·xH2O) as the indium source for doping, according to an indium to titanium molar ratio of 2:100. Stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while stirring continuously, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL high-pressure reactor lined with polytetrafluoroethylene (PTFE), seal it, and place it in an oven for hydrothermal reaction at 200 °C for 24 h. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to collect the white precipitate, wash it three times each with deionized water and anhydrous ethanol, and vacuum dry it at 80 °C for 12 h to obtain indium-doped two-dimensional TiO2 nanosheets, denoted as In-TNS-0.
[0077] Comparative Example 7
[0078] This comparative example provides a method for preparing indium-doped and carbon black-loaded two-dimensional TiO2 nanosheets, the steps of which are as follows:
[0079] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol. Add indium nitrate hydrate (In(NO3)3·xH2O) as the indium source for doping, according to an indium to titanium molar ratio of 2:100. Stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while stirring continuously, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL high-pressure reactor lined with polytetrafluoroethylene (PTFE), seal it, and place it in an oven for hydrothermal reaction at 200 °C for 24 h. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to collect the white precipitate, wash it three times each with deionized water and anhydrous ethanol, and vacuum dry it at 80 °C for 12 h to obtain indium-doped two-dimensional TiO2 nanosheets.
[0080] Step 2: Take 1.0 g of the indium-doped two-dimensional TiO2 nanosheets obtained in Step 1 and 0.005 g of carbon black, add them to 100 mL of anhydrous ethanol, and ultrasonically disperse for 2 h to form a uniform suspension. Stir the obtained suspension in an 80 °C water bath to evaporate the solvent. Transfer the resulting solid powder to a tube furnace, heat it to 350 °C at a rate of 5 °C / min under nitrogen atmosphere protection, calcine it at a constant temperature for 3 h, and then grind it after naturally cooling to room temperature to obtain indium-doped two-dimensional TiO2 nanosheets with a carbon black loading of 0.5 wt%, denoted as In-TNS-0.5.
[0081] Comparative Example 8
[0082] The only difference between this comparative example and comparative example 7 is that in step two, 1.0 g of the indium-doped two-dimensional TiO2 nanosheets obtained in step one and 0.015 g of carbon black are added to 100 mL of anhydrous ethanol to finally obtain indium-doped two-dimensional TiO2 nanosheets with a carbon black loading of 1.5 wt%, denoted as In-TNS-1.5.
[0083] Comparative Example 9
[0084] The only difference between this comparative example and comparative example 7 is that in step two, 1.0 g of the indium-doped two-dimensional TiO2 nanosheets obtained in step one and 0.03 g of carbon black were added to 100 mL of anhydrous ethanol, and finally indium-doped two-dimensional TiO2 nanosheets with a carbon black loading of 3.0 wt% were obtained, denoted as In-TNS-3.0.
[0085] Comparative Example 10
[0086] This comparative example provides a method for preparing zirconium-doped two-dimensional TiO2 nanosheets, the steps of which are as follows:
[0087] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol. Add zirconium oxychloride hydrate (ZrOCl2·8H2O) as the zirconium doping source at a zirconium to titanium molar ratio of 5:100. Stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while continuously stirring, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL high-pressure reactor lined with polytetrafluoroethylene (PTFE), seal it, and place it in an oven for hydrothermal reaction at 200 °C for 24 h. After the reaction, allow it to cool naturally to room temperature, centrifuge to collect the white precipitate, wash it three times each with deionized water and anhydrous ethanol, and vacuum dry it at 80 °C for 12 h to obtain zirconium-doped two-dimensional TiO2 nanosheets, denoted as Zr-TNS-0.
[0088] Comparative Example 11
[0089] This comparative example provides a method for preparing zirconium-doped and carbon black-loaded two-dimensional TiO2 nanosheets, the steps of which are as follows:
[0090] Step 1: Add 10 mL of tetrabutyl titanate (Ti(OBu)4) to 40 mL of anhydrous ethanol. Add zirconium oxychloride (ZrOCl2·8H2O) as the zirconium doping source at a zirconium to titanium molar ratio of 5:100. Stir at room temperature for 30 min until completely dissolved to form solution A. Dissolve 2 mL of 40% hydrofluoric acid in 10 mL of deionized water to form solution B. Add solution B dropwise to solution A while continuously stirring, and continue stirring for 1 h to obtain a homogeneous mixed solution. Transfer the resulting mixed solution to a 100 mL polytetrafluoroethylene-lined high-pressure reactor, seal it, and place it in an oven for hydrothermal reaction at 200 °C for 24 h. After the reaction, allow it to cool naturally to room temperature, centrifuge to collect the white precipitate, wash it three times each with deionized water and anhydrous ethanol, and vacuum dry it at 80 °C for 12 h to obtain zirconium-doped two-dimensional TiO2 nanosheets.
[0091] Step 2: Take 1.0 g of the zirconium-doped two-dimensional TiO2 nanosheets obtained in Step 1 and 0.005 g of carbon black, add them to 100 mL of anhydrous ethanol, and ultrasonically disperse for 2 h to form a uniform suspension. Stir the obtained suspension in an 80 °C water bath to evaporate the solvent. Transfer the resulting solid powder to a tube furnace, heat it to 350 °C at a rate of 5 °C / min under nitrogen atmosphere protection, calcine it at this temperature for 3 h, and then grind it after naturally cooling to room temperature to obtain zirconium-doped two-dimensional TiO2 nanosheets with a carbon black loading of 0.5 wt%, denoted as Zr-TNS-0.5.
[0092] Comparative Example 12
[0093] The only difference between this comparative example and comparative example 11 is that in step two, 1.0 g of zirconium-doped two-dimensional TiO2 nanosheets obtained in step one and 0.015 g of carbon black are added to 100 mL of anhydrous ethanol to finally obtain zirconium-doped two-dimensional TiO2 nanosheets with a carbon black loading of 1.5 wt%, denoted as Zr-TNS-1.5.
[0094] Comparative Example 13
[0095] The only difference between this comparative example and comparative example 11 is that in step two, 1.0 g of zirconium-doped two-dimensional TiO2 nanosheets obtained in step one and 0.03 g of carbon black are added to 100 mL of anhydrous ethanol to finally obtain zirconium-doped two-dimensional TiO2 nanosheets with a carbon black loading of 3.0 wt%, denoted as Zr-TNS-3.0.
[0096] Experimental Example 1
[0097] This experiment evaluates the photocatalytic CO2 reduction to methanol production performance of the composite catalysts prepared in Examples 1-3 and the two-dimensional TiO2 nanosheets prepared in Comparative Examples 1-13.
[0098] The detection method is as follows:
[0099] A closed quartz photocatalytic reactor with a volume of 200mL is used. The reactor has a quartz window at the top, is equipped with a 300W xenon lamp light source, and is fitted with an AM1.5G filter to simulate sunlight.
[0100] Accurately weigh 50 mg of the catalyst to be tested and ultrasonically disperse it in 100 mL of deionized water. Transfer the resulting suspension to a reactor. After sealing the reactor, replace the air inside the reactor three times with high-purity CO2 gas (99.999% purity), and finally purge CO2 to a pressure of 0.2 MPa. Turn on the light source and carry out the photocatalytic reaction under magnetic stirring. The reaction temperature is controlled at 25 ± 2 °C using circulating cooling water. During the reaction, samples are taken from the top of the reactor every 1 hour using a gas-tight syringe. The gaseous products are analyzed by gas chromatography (GC-FID / TCD), and the liquid products are qualitatively and quantitatively analyzed by proton nuclear magnetic resonance spectroscopy. The reaction continues for 6 hours, and the methanol yield of each catalyst is calculated.
[0101] Methanol yield results are as follows Figure 1 As shown in Table 1.
[0102] Table 1
[0103]
[0104] As shown in Table 1 and Figure 1 As shown, compared with the benchmark sample Pure-TNS-0, both In single-doping and Zr single-doping can significantly improve the photocatalytic CO2 to methanol production performance: In-TNS-1.5 methanol yield is 18.5 μmol·g.-1 ·h -1 The performance was improved by 12.3 times; the methanol yield of Zr-TNS-1.5 was 20.5 μmol·g. -1 ·h -1 The performance was improved by 13.7 times. This indicates that both metal doping has a significant catalytic promoting effect, with Zr single doping showing a slightly better improvement than In single doping. This is presumably due to the introduction of oxygen vacancies by zirconium doping, which enhances CO2 adsorption and activation capabilities.
[0105] Under the same doping conditions, the In / Zr co-doped catalyst outperforms the single-doped In or Zr catalyst, with the best co-doped sample, In / Zr-TNS-1.5, achieving a methanol yield of 28.5 μmol·g. -1 ·h -1 Compared to the best-performing single-doped sample Zr-TNS-1.5, the performance is improved by approximately 39%. This indicates that there is a synergistic enhancement effect between In and Zr, rather than a simple superposition of the effects of the two single doping elements. The co-doped system can further optimize the catalytic interface and regulate charge transfer and active sites.
[0106] The amount of carbon black (CB) added has an optimal range for catalytic activity, showing a pattern of initial increase followed by a decrease. Taking the In / Zr co-doped system as an example: without carbon (In / Zr-TNS-0): methanol yield 14.5 μmol·g -1 ·h -1 Low carbon (In / Zr-TNS-0.5): Methanol yield 22.0 μmol·g -1 ·h -1 Medium carbon (In / Zr-TNS-1.5): reached a peak of 28.5 μmol·g -1 ·h -1 High carbon (In / Zr-TNS-3.0): Yield decreased to 20.5 μmol·g -1 ·h -1 This indicates that an appropriate amount of carbon black can construct a conductive network, accelerate the migration of photogenerated electrons, inhibit electron-hole recombination, and improve reaction efficiency; however, when excessive carbon black is added, it will produce a light-shielding effect, blocking the incident light source, and at the same time, carbon particles will agglomerate, which will reduce photocatalytic activity.
[0107] The In / Zr-TNS-1.5 prepared in Example 1 is the best performing catalyst, with a 19.0-fold increase in methanol yield compared to the original unmodified Pure-TNS-0.
[0108] Experimental Example 2
[0109] In this experiment, UV-Vis diffuse reflectance spectroscopy was performed on the catalysts of Comparative Example 1 (Pure-TNS-0), Comparative Example 5 (In / Zr-TNS-0), Example 1 (In / Zr-TNS-1.5), and Example 3 (In / Zr-TNS-3.0) to analyze the light absorption characteristics and band structure changes of the samples. The results are shown in Table 2 and... Figure 2 As shown.
[0110] Table 2
[0111]
[0112] From Table 2 and Figure 2 It is known that the absorption edge of unmodified Pure-TNS-0 is located at 387 nm, with a band gap of 3.20 eV, and it can only respond to ultraviolet light. After In / Zr co-doping modification (In / Zr-TNS-0), the absorption edge redshifts to 405-410 nm, and the band gap shrinks to 3.05 eV, significantly widening the visible light response range of the material. The above-mentioned absorption edge redshift phenomenon can be attributed to two aspects: orbital hybridization occurs between the In 5s orbital and the O 2p orbital, and at the same time, Zr doping introduces a large number of oxygen vacancies, constructing intermediate energy levels within the semiconductor band gap and reducing the energy required for electron transitions.
[0113] Introducing 1.5 wt% carbon black into the composite yielded In / Zr-TNS-1.5, with the absorption edge maintained in the 405–410 nm range and the band gap further reduced to approximately 3.00 eV. It is speculated that carbon doping in the carbon black resulted in hybridization between the C 2p and O 2p orbitals, raising the valence band top and further narrowing the band gap, which is beneficial for capturing visible light photons. This finding corroborates the optimal photocatalytic methanol yield of this sample.
[0114] When the carbon black content was increased to 3.0 wt% (In / Zr-TNS-3.0), the characteristic absorption edge of the semiconductor in the spectrum disappeared, and the sample exhibited continuous high absorption characteristics across the entire spectrum. This phenomenon directly confirms that high carbon black content brings about a significant light-shielding effect: excessive carbon black absorbs and scatters a large amount of incident light, making it difficult for the two-dimensional TiO2 nanosheets on the substrate to receive effective photons and generate photogenerated carriers. This explains the significant decrease in the catalytic activity of In / Zr-TNS-3.0 from the perspective of light trapping.
[0115] In summary, In / Zr co-doping can effectively narrow the band gap and extend visible light absorption; appropriate carbon black composites can further optimize the band structure.
[0116] Experimental Example 3
[0117] This experiment tested the sulfur poisoning resistance of the composite catalysts prepared in Examples 1-3 and the two-dimensional TiO2 nanosheets prepared in Comparative Examples 1-13.
[0118] The testing method is as follows:
[0119] A 200 mL sealed quartz photocatalytic reactor was used, with a quartz window at the top. A 300 W xenon lamp light source was installed, fitted with an AM1.5G filter to simulate sunlight. 50 mg of the catalyst was accurately weighed and ultrasonically dispersed in 100 mL of deionized water. The suspension was then transferred to the reactor. After sealing the reactor, the air inside was replaced three times with a mixed gas (CO2 substrate + 50 ppm H2S), finally increasing the pressure to 0.2 MPa. The light source was turned on, and the photocatalytic reaction was carried out under magnetic stirring. The system temperature was controlled at 25 ± 2 °C using circulating cooling water. The reaction lasted for 5 hours, with samples taken every hour using a gas-tight syringe. The gaseous products were detected using gas chromatography (GC-FID / TCD), and the methanol yield was monitored in real time. The catalyst activity retention rate was calculated using the following formula:
[0120] Catalytic activity retention rate = (methanol yield with H2S / methanol yield without H2S) × 100%.
[0121] The test results of undoped, single-doped, and indium-zirconium co-doped samples with different carbon black loadings are as follows: Figure 3 As shown, the experimental data of representative samples of each system (Example 1: In / Zr-TNS-1.5, Comparative Example 12: Zr-TNS-1.5, Comparative Example 8: In-TNS-1.5 and Comparative Example 1: Pure-TNS-0) were selected for comparative analysis. The performance after continuous reaction for 5 hours in a 50ppmH2S atmosphere is shown in Table 3.
[0122] Table 3
[0123]
[0124] Pure-TNS-0 initial methanol yield: 1.5 μmol·g -1 ·h -1 The concentration decreased to 0.45 μmol·g after 5 hours of reaction. -1 ·h -1 The activity retention rate was only about 30%, and the activity loss rate was as high as 70%; the activity loss rate of In single-doped In-TNS-1.5 was 40%; the sulfur resistance of Zr single-doped Zr-TNS-1.5 was further improved, with an activity loss rate of 32%; the In / Zr co-doped sample In / Zr-TNS-1.5 had the lowest activity loss rate, only about 25%, and had the best resistance to hydrogen sulfide poisoning.
[0125] Combination Figure 3The variation curves show that, within the same doping system, increasing the amount of carbon black added can effectively slow down the rate of catalytic activity decay over time. This is because In and Zr co-doping have a synergistic effect, regulating the electron distribution on the catalyst surface and inhibiting S... 2- Strong adsorption at active sites alleviates sulfide deactivation of active sites; carbon black forms a continuous conductive network, accelerates interfacial charge migration, weakens the damage of sulfide byproducts to carrier transport pathways, and further improves sulfur resistance stability.
[0126] In summary, the modification scheme of In / Zr co-doped composite carbon black not only improves the photocatalytic activity of CO2 to methanol production, but also significantly enhances the catalyst's ability to tolerate trace amounts of hydrogen sulfide impurities, making it more suitable for industrial CO2 feed gas conditions containing sulfur impurities.
[0127] Test Example 4
[0128] In this experiment, the composite catalysts In / Zr-TNS-1.5 and In / Zr-TNS-3.0 prepared in Examples 1 and 3, and the two-dimensional TiO2 nanosheets Pure-TNS-0 and In / Zr-TNS-0 prepared in Comparative Examples 1 and 5 were characterized and analyzed in terms of microstructure, elemental composition and valence state, and crystalline phase.
[0129] (I) Morphological characterization by scanning electron microscopy (SEM)
[0130] Test method: The sample to be tested was ultrasonically dispersed in an ethanol solution, dropped onto the surface of a silicon wafer, dried, and sputter-coated with gold. The microstructure of the catalyst was then observed using a scanning electron microscope.
[0131] The results are as follows Figure 4 As shown, Pure-TNS-0 exhibits a regular two-dimensional layered framework structure with clean nanosheet surfaces and orderly stacked layers, with lateral dimensions of 50–500 nm. In / Zr co-doping yields In / Zr-TNS-0, which roughens the nanosheet surface, resulting in uniformly distributed nanocrystals and an increased specific surface area. In In / Zr-TNS-1.5 of Example 1, carbon black particles are highly dispersed and adhered to the surface of TiO2 nanosheets, preserving the complete two-dimensional layered framework. The catalyst forms a tight "sheet-point" interface contact, which is beneficial for interfacial charge transport. In In / Zr-TNS-3.0 of Example 3, carbon black undergoes severe agglomeration, with excessive carbon black covering a large area of the nanosheet surface, burying the original layered morphology of the support.
[0132] SEM results show that carbon black can achieve good dispersion at an addition of 1.5 wt%; however, when the addition of carbon black is increased to 3.0 wt%, obvious agglomeration occurs, providing direct morphological evidence for the light shielding effect caused by excessive carbon black.
[0133] (II) Elemental Valence State and Composition Analysis by X-ray Photoelectron Spectroscopy (XPS)
[0134] Test method: X-ray photoelectron spectroscopy was used to acquire the full spectrum of the sample and the fine spectra of Ti 2p, C 1s, and In 3d to analyze the types, relative contents, and changes in elemental binding energy of the surface elements.
[0135] The results are as follows Figure 5 As shown, Pure-TNS-0 is mainly composed of Ti and O elements, with only trace amounts of surface contaminant carbon. (Ti 2p) 3 / 2 The binding energy is 458.9 eV; In / Zr-TNS-0 samples showed detectable In 3d (444–455 eV) and Zr elemental signals, confirming the successful introduction of In and Zr into the TiO2 system; Ti 2p 3 / 2 The binding energy shifted to 459.1 eV, a positive shift of 0.2 eV compared to the pure sample, indicating that In / Zr doping reduces the electron cloud density of Ti atoms and that there is a significant electronic interaction between the dopant ions and the TiO2 lattice.
[0136] As the amount of carbon black added increased, the carbon content on the sample surface gradually increased: In / Zr-TNS-0 carbon content was 6.1%; In / Zr-TNS-1.5 carbon content was 22.5%; and In / Zr-TNS-3.0 carbon content reached 58.3%. The surface proportion of Ti element continued to decrease, which is consistent with the theoretical trend of material addition. The moderate carbon content of In / Zr-TNS-1.5 indicates that the carbon black adhered in a dispersed form and did not form a continuous, fully covered carbon layer.
[0137] (III) Phase and Crystallinity Analysis by X-ray Powder Diffraction (XRD)
[0138] Test method: X-ray diffraction patterns of the samples were collected using an X-ray diffractometer with a scanning range of 10° to 80°. The positions of the diffraction peaks were compared with the anatase TiO2 standard card PDF#21-1272 to analyze the changes in crystal phase and degree of crystallization.
[0139] The result is as follows Figure 6 As shown, Pure-TNS-0 exhibits complete and sharp anatase TiO2 characteristic diffraction peaks, indicating high crystallinity. The In / Zr co-doped sample In / Zr-TNS-0 shows no significant shift in diffraction peak position, maintaining a stable peak shape with a slight decrease in peak intensity, suggesting that In / Zr doping does not alter the anatase crystal structure of TiO2. The diffraction peak intensity of In / Zr-TNS-1.5 further decreases, attributed to the dilution absorption effect of carbon black on X-rays. No carbon black characteristic diffraction peaks were observed in the sample, confirming that carbon black is an amorphous phase and highly dispersed. The anatase diffraction peaks of In / Zr-TNS-3.0 show a significant attenuation, and a distinct amorphous carbon broad diffraction bulge appears in the 2θ=20°~30° range, corroborating the carbon black agglomeration observed by SEM.
Claims
1. Indium-zirconium co-doped two-dimensional TiO2 nanosheet / carbon black composite photocatalyst, characterized in that, The composite photocatalyst uses two-dimensional TiO2 nanosheets as a substrate. The lattice of the two-dimensional TiO2 nanosheets is doped with indium and zirconium, wherein the molar ratio of indium to titanium is 0.5~5:100 and the molar ratio of zirconium to titanium is 1~8:
100. The surface of the two-dimensional TiO2 nanosheets is loaded with carbon black, and the loading amount of carbon black is 0.5~3.0 wt% based on the total mass of the composite photocatalyst.
2. The composite photocatalyst according to claim 1, wherein The molar ratio of indium to titanium is 1~3:100, the molar ratio of zirconium to titanium is 3~6:100, and the loading of carbon black is 1.5wt%.
3. The composite photocatalyst according to claim 1 or 2, characterized by, The two-dimensional TiO2 nanosheets have a thickness of 2~10 nm, a lateral dimension of 50~500 nm, and exposed {001} active crystal planes.
4. A method for preparing the composite photocatalyst according to any one of claims 1 to 3, characterized by, Includes the following steps: Step 1: Titanium source, indium source and zirconium source are subjected to hydrothermal or solvothermal reaction at 160~240℃ in the presence of hydrofluoric acid for 8~72h to obtain indium-zirconium co-doped two-dimensional TiO2 nanosheets. Step 2: Mix the obtained indium-zirconium co-doped two-dimensional TiO2 nanosheets with carbon black in a solvent, disperse them ultrasonically, evaporate the solvent, and calcine them at 250~500℃ for 2~4h under an inert atmosphere to obtain the composite photocatalyst.
5. The preparation method according to claim 4, characterized in that, The titanium source is tetrabutyl titanate, the indium source is indium nitrate or indium chloride, and the zirconium source is zirconium oxychloride or zirconium nitrate.
6. The production method according to claim 4 or 5, characterized by, The hydrothermal or solvothermal reaction temperature in step one is , and the reaction time is 12-48 h.
7. The production method according to claim 4 or 5, characterized by, The solvent in step two is anhydrous ethanol, the mass-to-volume ratio of the indium-zirconium co-doped two-dimensional TiO2 nanosheets, carbon black and the anhydrous ethanol is 1.0g:0.005~0.03g:100mL, the ultrasonic dispersion time is 0.5~2h, and the calcination temperature is 300~450℃.
8. The application of a composite photocatalyst as described in any one of claims 1-3 or a composite photocatalyst prepared by any one of claims 4-7 in the photocatalytic reduction of CO2 to methanol.
9. Use according to claim 8, characterized in that, The composite photocatalyst is dispersed in a reaction system containing H2O as a proton source. The amount of the composite photocatalyst is 0.5~5 g / L. Under light conditions, biogas produced by anaerobic fermentation is introduced to carry out the photocatalytic reaction. The partial pressure of CO2 is 0.1~0.5 MPa. Methanol is collected after 2~12 h of reaction.
10. Use according to claim 9, characterized in that, The illumination is simulated sunlight or visible light with a wavelength of not less than 420nm, the concentration of H2S in the biogas is 0~5000ppm, and the reaction temperature is 15~60℃.