A catalyst for purifying circulating gas from propane oxidation to acrylic acid, its preparation method, and its application.
By coating SiO2 onto a CuO-CeO2-MnOx catalyst, the problems of acid gas removal and raw material stability in the propane oxidation to acrylic acid production cycle gas were solved, achieving highly efficient purification and a long-life catalyst.
Patent Information
- Application Number
- CN202611337817.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing catalysts cannot effectively remove acidic gases such as acrylic acid and acetic acid from the propane oxidation to acrylic acid cycle gas, while maintaining the stability of propane and by-product propylene, resulting in decreased catalyst activity and shortened service life.
CuO-CeO2-MnOx composite metal oxides are used as the active components of the catalyst and coated with a SiO2 modification layer. The support is Al2O3 or SiO2. By adjusting the molar ratio of the active components and the preparation process, a mesoporous SiO2 film is formed to inhibit carbonate and oligomeric carbon deposits and prevent carbon accumulation and corrosion on the catalyst surface.
It significantly reduces the complete oxidation ignition temperature of organic acids, improves the decomposition efficiency of acrylic acid and acetic acid, maintains the stability of propane and propylene, extends catalyst life, and improves purification effect.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalysts, specifically relating to a catalyst for the purification of circulating gas from propane oxidation to acrylic acid, its preparation method, and its application. Background Technology
[0002] Acrylic acid (CH2=CH-COOH) is an important unsaturated organic acid with highly reactive chemical properties. It can undergo various esterification and polymerization reactions. Its downstream products, such as methyl acrylate, ethyl acrylate, butyl acrylate, and superabsorbent resins, are widely used in various sectors of the national economy and people's livelihood, including coatings, adhesives, garden water retention, and hygiene products. Currently, China's acrylic acid production capacity is approximately 4.6 million tons, all produced from propylene through a two-step oxidation process.
[0003] Compared to propylene, propane is cheaper and more readily available. Furthermore, propane can be oxidized in one step on a MoVTeNbOx composite metal oxide catalyst to obtain acrylic acid, significantly reducing the production and investment costs of acrylic acid. Numerous research reports have already documented the one-step oxidation of propane to produce acrylic acid. Because propane is a saturated alkane with only three carbon atoms and is very stable, while acrylic acid is a highly reactive unsaturated organic acid that is easily oxidized to the more stable carbon dioxide, the conversion rate of propane is controlled at a relatively reasonable level to ensure high selectivity for acrylic acid. Complete conversion is not achieved; the single-pass conversion rate of propane is generally controlled between 40% and 70%. Unreacted propane needs to be returned to the reactor to participate in the oxidation reaction again, thus reducing unit consumption.
[0004] The main products of propane oxidation are acrylic acid, acetic acid, acetone, propionic acid, propylene, carbon monoxide, and carbon dioxide. In addition, the gas exiting the reactor contains unreacted propane, oxygen, and nitrogen as a balance gas. This mixed gas, after cooling, enters a spray absorption tower, typically using water as the absorbent. Most of the high-boiling-point organic compounds such as acrylic acid, acetic acid, acetone, and propionic acid in the mixed gas are absorbed by the water, forming an acidic solution at the bottom of the tower. The remaining non-condensable gases are discharged from the top of the tower, pressurized, and recycled back to the reactor inlet. Despite the spray absorption process, the non-condensable gas at the top of the tower still carries trace amounts of incompletely absorbed acidic gases, including approximately 200-500 ppm of acrylic acid, approximately 300-1000 ppm of acetic acid, and small amounts of propionic acid, acetone, and high-boiling-point organic compounds, all <50 ppm. These acidic gases can cause carbon deposition or even coking on the surface of the MoVTeNbOx catalyst, severely reducing the catalyst's activity and lifespan.
[0005] Therefore, the purification of the circulating gas for propane oxidation to acrylic acid production needs to meet two requirements at the same time: (1) remove acidic gases, mainly acrylic acid and acetic acid, from the circulating gas; (2) maintain the stability of propane and by-product propylene in the circulating gas.
[0006] Patent CN105478134A discloses a suitable supported catalyst for purifying air at room temperature, using copper, cerium and manganese as active ingredients. It can continuously and effectively remove harmful gases such as benzene, formaldehyde, CO, NO and SO2 from the air, but it does not address the issue of purifying the circulating gas from propane oxidation to acrylic acid.
[0007] Therefore, there is an urgent need in the industry to develop a catalyst that can simultaneously meet the above two requirements for the purification of circulating gas and to promote the industrialization of the propane oxidation to acrylic acid process. Summary of the Invention
[0008] To address the aforementioned problems, this invention provides a catalyst for purifying the circulating gas from propane oxidation to acrylic acid production. This invention utilizes CuO-CeO2-MnO... x Composite metal oxides serve as the active components of the catalyst, with CuO providing the basic low-temperature oxidation sites and MnO... x It possesses strong intrinsic oxidizing properties. After the introduction of Ce, a multivalent electron cyclic coupling system is constructed, which significantly reduces the complete oxidation ignition temperature of organic acids such as acrylic acid and acetic acid, and lowers the complete conversion temperature of organic acids by 30~60℃. It can efficiently decompose trace amounts of acrylic acid and acetic acid of 200~1000ppm at the normal operating temperature of the circulating gas, avoiding the enrichment and coking of acidic components. At the same time, it weakens the excessive oxidation of propane and saturated / unsaturated alkanes such as propylene, ensuring the stability of the raw material component concentration in the circulating gas.
[0009] To achieve the above technical objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides a catalyst for purifying circulating gas from propane oxidation to acrylic acid, wherein the active components are copper, cerium and manganese, the active components are coated with a SiO2 modification layer, the support is Al2O3 or SiO2, the content of copper, cerium and manganese accounts for 10%-30% of the total mass of the catalyst, and their molar ratio is 1:(1-1.5):(1-3).
[0010] A second aspect of the present invention provides a method for preparing a catalyst for purifying circulating gas from propane oxidation to acrylic acid, comprising: Cu salt solution, Ce salt solution, and Mn salt solution are mixed, the pH is adjusted to alkaline to form a precipitate, a single aging reaction is carried out, solid-liquid separation is performed, drying is carried out, and a single calcination is performed to obtain a composite metal oxide catalyst. The composite metal oxide catalyst was dispersed in a solvent, an organosilicon source was added under alkaline conditions, a secondary aging reaction was carried out, solid-liquid separation was performed, and the catalyst powder was obtained by drying. The catalyst powder is mixed evenly with the carrier, water and guar gum powder are added, kneaded, extruded into strips, granulated, dried, and then calcined a second time to obtain the final product.
[0011] A third aspect of the present invention provides the application of the above-described catalyst or the catalyst prepared by the above-described method in the purification of circulating gas from propane oxidation to acrylic acid.
[0012] The beneficial effects of this invention are as follows: (1) CuO-CeO2-MnO in this invention x The ternary system has controllable oxidation intensity and can directionally catalyze the deep decomposition of highly active organic acids such as acrylic acid and acetic acid into CO2 and H2O. At the same time, it weakens the excessive oxidation of propane and saturated / unsaturated alkanes, ensuring the stability of the raw material component concentration in the circulating gas and not reducing the overall yield of the acrylic acid process. It solves the defect of single strong oxidizing Mn-based catalysts that easily consume propylene and propane.
[0013] (2) This invention utilizes TEOS hydrolysis in CuO-CeO2-MnO x The formation of a mesoporous SiO2 film on the surface can effectively inhibit the formation and accumulation of carbonate and oligomeric carbonaceous deposits on the catalyst surface, while not affecting the CuO-CeO2-MnO2 production. X Surface activity significantly improves the purification effect of circulating gas.
[0014] (3) The method of the present invention is simple, easy to operate, highly practical, and easy to promote. Detailed Implementation
[0015] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0016] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Therefore, the detailed description of the embodiments of the present invention provided below is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0017] As described in the background section, to meet the requirements for purifying the circulating gas from propane oxidation to acrylic acid, a catalyst is needed that can effectively remove acidic gases from the circulating gas while maintaining the stability of propane and byproduct propylene. However, currently, there are many types of catalysts for gas purification, including photocatalytic (TiO2), non-photocatalytic (noble metal / transition metal), composite synergistic, and bioenzyme types, etc., and no catalyst that can meet the above requirements has yet been found in the industry. Therefore, after long-term research and experimental exploration, this invention provides a catalyst for purifying the circulating gas from propane oxidation to acrylic acid. The active components are copper, cerium, and manganese, and the active components are coated with a SiO2 modification layer. The support is Al2O3 or SiO2, and the content of copper, cerium, and manganese accounts for 10%-30% of the total mass of the catalyst, with a molar ratio of 1:(1-1.5):(1-3). The catalyst of this invention can directionally catalyze the deep decomposition of highly reactive organic acids such as acrylic acid and acetic acid into CO2 and H2O, while weakening the excessive oxidation of propane and saturated / unsaturated alkanes, thus ensuring the stability of the raw material component concentration in the circulating gas.
[0018] The present invention does not impose any special limitation on the specific shape of the catalyst. Preferably, the shape of the catalyst is selected from one of the following: columnar, Raschig ring, cloverleaf, and gear shape. Those skilled in the art can select the appropriate shape according to the specific loading conditions.
[0019] The composition, dosage, structure, preparation process, and type of gas to be treated of the catalyst all affect the gas purification effect. Therefore, this invention also provides a method for preparing a catalyst for purifying the circulating gas from propane oxidation to acrylic acid, comprising: Cu salt solution, Ce salt solution, and Mn salt solution are mixed, the pH is adjusted to alkaline to form a precipitate, a single aging reaction is carried out, solid-liquid separation is performed, drying is carried out, and a single calcination is performed to obtain a composite metal oxide catalyst. The composite metal oxide catalyst was dispersed in a solvent, an organosilicon source was added under alkaline conditions, a secondary aging reaction was carried out, solid-liquid separation was performed, and the catalyst powder was obtained by drying. The catalyst powder is mixed evenly with the carrier, water and guar gum powder are added, kneaded, extruded into strips, granulated, dried, and then calcined a second time to obtain the final product.
[0020] Ternary CuO-CeO2-MnO XThe intrinsic oxidizing properties are strong, and without coating, it is prone to over-oxidation of unreacted propane and intermediate product propylene in the circulating gas, reducing the overall yield of the acrylic acid unit. To address this, the present invention uses an ultra-thin SiO2 mesoporous shell layer to act as a molecular sieving and oxidation buffer: small molecules of acrylic acid and acetic acid can easily diffuse into the shell layer and be completely oxidized and decomposed by the highly active composite oxide in the core; the diffusion resistance of propane and propylene alkane / olefin molecules is increased, weakening their deep combustion at highly oxidizing active sites and avoiding raw material loss; at the same time, the thickness of the SiO2 mesoporous shell can be precisely controlled, significantly improving the oxidation selectivity for propane and propylene without significantly reducing the organic acid purification efficiency.
[0021] Since there are many types of air purification catalysts with varying performance, this invention studies the composition and dosage of the active components of the catalyst. Preferably, the chemical formula of the composite metal oxide catalyst is CuO-CeO2-MnO. x This invention has found that using this ternary active ingredient can effectively improve the adsorption efficiency of organic acids and inhibit the excessive oxidation of propane and by-product propylene.
[0022] The calcination temperature affects the Cu-Ce and Mn-Ce heterostructure and solid solution structure, which in turn affects the number of core active sites for decomposing organic acids. Therefore, this invention studies the calcination temperature. Preferably, the primary calcination is carried out at 350-450℃ for 4-8 hours in an air atmosphere to obtain a better catalyst structure and improve the purification effect of circulating gas.
[0023] The circulating gas from the main propane oxidation reaction carries trace amounts of organic acids such as acrylic acid and acetic acid. These polar acid molecules are readily and strongly adsorbed onto CuO-CeO2-MnO. X On the active surface, carbonate and oligomeric carbonaceous deposits form, blocking active sites; simultaneously, acidic components continuously corrode the metal oxide interface, causing activity decay. This invention has found that traditional methods of physically mixing SiO2 powder only serve as macroscopic carriers and cannot form a protective layer on the surface of nano-active grains. Therefore, through long-term research and experimental exploration, this invention has discovered that the mesoporous SiO2 film generated by TEOS hydrolysis uniformly coats the ternary oxide grains, forming a "sieve barrier" that does not affect the CuO-CeO2-MnO... X While enhancing surface activity, it effectively inhibits the formation and accumulation of carbonate and oligomeric carbonaceous deposits on the catalyst surface. Therefore, preferably, the mass ratio of the organosilicon source to the composite metal oxide catalyst is (0.05-0.30):1 to obtain better circulating gas purification effect.
[0024] The temperature and pH of aging can affect the uniformity, pore structure and catalytic activity of the SiO2 mesoporous shell. Therefore, this invention studies the temperature, pH and time of the secondary aging reaction. Preferably, the conditions for the secondary aging reaction are a temperature of 60-80℃, a pH of 8-9 and a time of 3-4h, in order to optimize the SiO2 mesoporous shell structure and improve the purification effect of circulating gas.
[0025] The amount of carrier affects the overall structure of the inorganic framework, particle strength, and loading effect of active powder. In order to meet the requirements of long-term operation of catalyst in industrial applications, this invention studies the mass ratio of catalyst powder to carrier. Preferably, the mass ratio of catalyst powder to carrier is (50-70):(30-50) to obtain better solid strength and catalytic performance.
[0026] The temperature, time, and atmosphere of secondary calcination can affect the pore structure, strength, and activity of the catalyst. Therefore, this invention has studied the conditions for secondary calcination. Preferably, the conditions for secondary calcination are calcination at 280-580℃ in an air atmosphere for 2-6 hours to obtain a better circulating gas purification effect.
[0027] The present invention will be further described in detail below with reference to specific embodiments. It should be noted that the specific embodiments are explanations of the present invention and not limitations thereof.
[0028] Example 1: A catalyst for purifying circulating gas from propane oxidation to acrylic acid, the composition and preparation method of which are as follows: (1) The catalyst is a CuO-CeO2-MnOx composite metal oxide. First, Cu(NO3)2, Ce(NO3)3, and Mn(NO3)2 are dissolved in water to prepare solutions. The three solutions are mixed in a molar ratio of 1:1.25:2, and the pH is adjusted to 10.5 with ammonia solution to form a precipitate. After aging for 12 hours, the precipitate is filtered. The filter cake is then dried in a forced-air drying oven at 120°C for 12 hours and calcined. After calcination at 400°C for 6 hours in air atmosphere, a highly active composite metal oxide catalyst powder is obtained.
[0029] (2) Disperse the catalyst powder in a 45% ethanol aqueous solution, heat it to 70°C while stirring, add ammonia or sodium hydroxide solution, adjust the pH to 8.5, then add tetraethyl orthosilicate (the mass ratio of tetraethyl orthosilicate to catalyst powder is 0.15:1), age for 3 hours, the total volume of the solution to the volume ratio of catalyst powder is 7.5:1, filter to separate the solid and liquid, and further dry the obtained solid powder in air at 120°C before molding.
[0030] (3) Mix the catalyst powder and SiO2 in a mass ratio of 60:40, add a certain amount of water and guar gum powder, knead for 3 hours to form a plastic wet material, place it in a screw extruder for extrusion molding, use a blade to cut into granules, dry the granules in air at 120°C for 3 hours, and then calcine them in air at 420°C for 4 hours to obtain the catalyst for final industrial application.
[0031] Example 2: A catalyst for purifying circulating gas from propane oxidation to acrylic acid, the composition and preparation method of which are as follows: (1) The catalyst is a CuO-CeO2-MnOx composite metal oxide. First, Cu(NO3)2, Ce(NO3)3, and Mn(NO3)2 are dissolved in water to prepare solutions. The three solutions are mixed in a molar ratio of 1:1.5:3, and the pH is adjusted to 10.5 with ammonia solution to form a precipitate. After aging for 12 hours, the precipitate is filtered. The filter cake is then dried in a forced-air drying oven at 120°C for 12 hours and calcined. After calcination at 450°C for 4 hours in air atmosphere, a highly active composite metal oxide catalyst powder is obtained.
[0032] (2) The catalyst powder is dispersed in a 30% ethanol aqueous solution, heated to 70°C under stirring, sodium hydroxide solution is added, the pH is adjusted to 8.5, and then tetraethyl orthosilicate (the mass ratio of tetraethyl orthosilicate to catalyst powder is 0.10:1) is added. After aging for 3 hours, the total volume of the solution and the volume ratio of the catalyst powder are 5:1. The solid and liquid are separated by filtration. The resulting solid powder is further dried in air at 120°C and then shaped.
[0033] (3) Mix the catalyst powder and SiO2 in a mass ratio of 70:30, add a certain amount of water and guar gum powder, knead for 3 hours to form a plastic wet material, place it in a screw extruder for extrusion molding, use a blade to cut into granules, dry the granules in air at 120°C for 3 hours, and then calcine them in air at 580°C for 2 hours to obtain the catalyst for final industrial application.
[0034] Example 3: A catalyst for purifying circulating gas from propane oxidation to acrylic acid, the composition and preparation method of which are as follows: (1) The catalyst is a CuO-CeO2-MnOx composite metal oxide. First, Cu(NO3)2, Ce(NO3)3, and Mn(NO3)2 are dissolved in water to prepare solutions. The three solutions are mixed in a molar ratio of 1:1.5:3, and the pH is adjusted to 10.5 with ammonia solution to form a precipitate. After aging for 12 hours, the precipitate is filtered. The filter cake is then dried in a forced-air drying oven at 120°C for 12 hours and calcined. After calcination at 350°C for 8 hours in air atmosphere, a highly active composite metal oxide catalyst powder is obtained.
[0035] (2) Disperse the catalyst powder in a 60% ethanol aqueous solution, heat it to 70°C while stirring, add ammonia or sodium hydroxide solution, adjust the pH to 8.5, then add tetraethyl orthosilicate (the mass ratio of tetraethyl orthosilicate to catalyst powder is 0.20:1), age for 3 hours, the total volume of the solution to the volume ratio of catalyst powder is 10:1, filter to separate the solid and liquid, and further dry the obtained solid powder in air at 120°C before molding.
[0036] (3) Mix the catalyst powder and SiO2 in a mass ratio of 50:50, add a certain amount of water and guar gum powder, knead for 3 hours to form a plastic wet material, place it in a screw extruder for extrusion molding, use a blade to cut into granules, dry the granules in air at 120°C for 3 hours, and then calcine them in air at 280°C for 6 hours to obtain the catalyst for final industrial application.
[0037] Comparative Example 1 The difference from Example 1 is that Ce(NO3)3 is omitted, and the molar ratio of Cu(NO3)2 to Mn(NO3)2 is 1:2. Specifically, it includes: (1) The catalyst is a CuO-MnOx composite metal oxide. First, Cu(NO3)2 and Mn(NO3)2 are dissolved in water to prepare solutions. The two solutions are mixed at a molar ratio of 1:2, and the pH is adjusted to 10.5 with ammonia solution to form a precipitate. After aging for 12 hours, the precipitate is filtered. The filter cake is then dried in a forced-air drying oven at 120°C for 12 hours and calcined. After calcination at 400°C for 6 hours in air atmosphere, a highly active composite metal oxide catalyst powder is obtained.
[0038] (2) Disperse the catalyst powder in a 45% ethanol aqueous solution, heat it to 70°C while stirring, add ammonia or sodium hydroxide solution, adjust the pH to 8.5, then add tetraethyl orthosilicate (the mass ratio of tetraethyl orthosilicate to catalyst powder is 0.15:1), age for 3 hours, the total volume of the solution to the volume ratio of catalyst powder is 7.5:1, filter to separate the solid and liquid, and further dry the obtained solid powder in air at 120°C before molding.
[0039] (3) Mix the catalyst powder and SiO2 in a mass ratio of 60:40, add a certain amount of water and guar gum powder, knead for 3 hours to form a plastic wet material, place it in a screw extruder for extrusion molding, use a blade to cut into granules, dry the granules in air at 120°C for 3 hours, and then calcine them in air at 420°C for 4 hours to obtain the catalyst for final industrial application.
[0040] Comparative Example 2 The difference from Example 1 is that Y(NO3)3·6H2O is used instead of Ce(NO3)3, while the molar amount remains the same. Specifically, it includes: (1) The catalyst is a CuO-Y2O3-MnOx composite metal oxide. First, Cu(NO3)2, Y(NO3)3·6H2O, and Mn(NO3)2 are dissolved in water to prepare solutions. The three solutions are mixed in a molar ratio of 1:1.25:2, and the pH is adjusted to 10.5 with ammonia solution to form a precipitate. After aging for 12 hours, the precipitate is filtered. The filter cake is then dried in a forced-air drying oven at 120℃ for 12 hours and calcined. After calcination at 400℃ for 6 hours in air atmosphere, a highly active composite metal oxide catalyst powder is obtained.
[0041] (2) Disperse the catalyst powder in a 45% ethanol aqueous solution, heat it to 70°C while stirring, add ammonia or sodium hydroxide solution, adjust the pH to 8.5, then add tetraethyl orthosilicate (the mass ratio of tetraethyl orthosilicate to catalyst powder is 0.15:1), age for 3 hours, the total volume of the solution to the volume ratio of catalyst powder is 7.5:1, filter to separate the solid and liquid, and further dry the obtained solid powder in air at 120°C before molding.
[0042] (3) Mix the catalyst powder and SiO2 in a mass ratio of 60:40, add a certain amount of water and guar gum powder, knead for 3 hours to form a plastic wet material, place it in a screw extruder for extrusion molding, use a blade to cut into granules, dry the granules in air at 120°C for 3 hours, and then calcine them in air at 420°C for 4 hours to obtain the catalyst for final industrial application.
[0043] Comparative Example 3 The difference from Example 1 is that Zr(NO3)4 is used instead of Ce(NO3)3, while the molar amount remains the same.
[0044] Specifically, it includes: (1) The catalyst is a CuO-Zr2O3-MnOx composite metal oxide. First, Cu(NO3)2, Zr(NO3)4, and Mn(NO3)2 are dissolved in water to prepare solutions. The three solutions are mixed in a molar ratio of 1:1.25:2, and the pH is adjusted to 10.5 with ammonia solution to form a precipitate. After aging for 12 hours, the precipitate is filtered. The filter cake is then dried in a forced-air drying oven at 120°C for 12 hours and calcined. After calcination at 400°C for 6 hours in air atmosphere, a highly active composite metal oxide catalyst powder is obtained.
[0045] (2) Disperse the catalyst powder in a 45% ethanol aqueous solution, heat it to 70°C while stirring, add ammonia or sodium hydroxide solution, adjust the pH to 8.5, then add tetraethyl orthosilicate (the mass ratio of tetraethyl orthosilicate to catalyst powder is 0.15:1), age for 3 hours, the total volume of the solution to the volume ratio of catalyst powder is 7.5:1, filter to separate the solid and liquid, and further dry the obtained solid powder in air at 120°C before molding.
[0046] (3) Mix the catalyst powder and SiO2 in a mass ratio of 60:40, add a certain amount of water and guar gum powder, knead for 3 hours to form a plastic wet material, place it in a screw extruder for extrusion molding, use a blade to cut into granules, dry the granules in air at 120°C for 3 hours, and then calcine them in air at 420°C for 4 hours to obtain the catalyst for final industrial application.
[0047] Comparative Example 4 The difference from Example 1 is that step (2) is omitted. Specifically, it includes: (1) The catalyst is a CuO-CeO2-MnOx composite metal oxide. First, Cu(NO3)2, Ce(NO3)3, and Mn(NO3)2 are dissolved in water to prepare solutions. The three solutions are mixed in a molar ratio of 1:1.25:2, and the pH is adjusted to 10.5 with ammonia solution to form a precipitate. After aging for 12 hours, the precipitate is filtered. The filter cake is then dried in a forced-air drying oven at 120°C for 12 hours and calcined. After calcination at 400°C for 6 hours in air atmosphere, a highly active composite metal oxide catalyst powder is obtained.
[0048] (2) The catalyst powder and SiO2 are mixed evenly at a mass ratio of 60:40. A certain amount of water and guar gum powder are added and kneaded for 3 hours to form a plastic wet material. The material is then placed in a screw extruder for extrusion molding, granulated with blades, and dried in air at 120°C for 3 hours. The granules are then further calcined in air at 420°C for 4 hours to obtain the catalyst for final industrial application.
[0049] Comparative Example 5 The difference from Example 1 is that in step (2), the mass ratio of tetraethyl orthosilicate to catalyst powder is 0.05:1. Specifically, it includes: (1) The catalyst is a CuO-CeO2-MnOx composite metal oxide. First, Cu(NO3)2, Ce(NO3)3, and Mn(NO3)2 are dissolved in water to prepare solutions. The three solutions are mixed in a molar ratio of 1:1.25:2, and the pH is adjusted to 10.5 with ammonia solution to form a precipitate. After aging for 12 hours, the precipitate is filtered. The filter cake is then dried in a forced-air drying oven at 120°C for 12 hours and calcined. After calcination at 400°C for 6 hours in air atmosphere, a highly active composite metal oxide catalyst powder is obtained.
[0050] (2) Disperse the catalyst powder in a 45% ethanol aqueous solution, heat it to 70°C while stirring, add ammonia or sodium hydroxide solution, adjust the pH to 8.5, then add tetraethyl orthosilicate (the mass ratio of tetraethyl orthosilicate to catalyst powder is 0.05:1), age for 3 hours, the total volume of the solution to the volume of the catalyst powder is 7.5:1, filter to separate the solid and liquid, and further dry the obtained solid powder in air at 120°C before molding.
[0051] (3) Mix the catalyst powder and SiO2 in a mass ratio of 60:40, add a certain amount of water and guar gum powder, knead for 3 hours to form a plastic wet material, place it in a screw extruder for extrusion molding, use a blade to cut into granules, dry the granules in air at 120°C for 3 hours, and then calcine them in air at 420°C for 4 hours to obtain the catalyst for final industrial application.
[0052] Comparative Example 6 The difference from Example 1 is that in step (2), the mass ratio of tetraethyl orthosilicate to catalyst powder is 0.40:1. Specifically, it includes: (1) The catalyst is a CuO-CeO2-MnOx composite metal oxide. First, Cu(NO3)2, Ce(NO3)3, and Mn(NO3)2 are dissolved in water to prepare solutions. The three solutions are mixed in a molar ratio of 1:1.25:2, and the pH is adjusted to 10.5 with ammonia solution to form a precipitate. After aging for 12 hours, the precipitate is filtered. The filter cake is then dried in a forced-air drying oven at 120°C for 12 hours and calcined. After calcination at 400°C for 6 hours in air atmosphere, a highly active composite metal oxide catalyst powder is obtained.
[0053] (2) Disperse the catalyst powder in a 45% ethanol aqueous solution, heat it to 70°C while stirring, add ammonia or sodium hydroxide solution, adjust the pH to 8.5, then add tetraethyl orthosilicate (the mass ratio of tetraethyl orthosilicate to catalyst powder is 0.40:1), age for 3 hours, the total volume of the solution to the volume ratio of catalyst powder is 7.5:1, filter to separate the solid and liquid, and further dry the obtained solid powder in air at 120°C before molding.
[0054] (3) Mix the catalyst powder and SiO2 in a mass ratio of 60:40, add a certain amount of water and guar gum powder, knead for 3 hours to form a plastic wet material, place it in a screw extruder for extrusion molding, use a blade to cut into granules, dry the granules in air at 120°C for 3 hours, and then calcine them in air at 420°C for 4 hours to obtain the catalyst for final industrial application.
[0055] Experimental example: Catalyst performance evaluation: 10 mL of 20-40 mesh catalyst particles were packed into a stainless steel fixed-bed reactor with an inner diameter of φ10 mm. 15 mL of 20-40 mesh quartz sand was filled at both ends of the catalyst as a preheating and support section. Before the reaction, the catalyst was pretreated in air at a rate of 2℃ / min to 350℃ for 1.5 h at a space velocity of 1000 h⁻¹.
[0056] The simulated circulating gas composition was: propane 10 vol%, propylene 1 vol%, acrylic acid 1000 ppm, acetic acid 500 ppm, oxygen 5 vol%, water vapor 10 vol%, CO + CO2 2 vol%, and nitrogen as the balance gas. The reaction temperature range was 200–350 °C, the reaction pressure was atmospheric pressure, and the gas hourly space velocity was 5000 h⁻¹.
[0057] Samples were taken 2 hours after the reaction stabilized. The concentrations of acrylic acid and acetic acid at the inlet and outlet were analyzed using a gas chromatograph equipped with an FID detector, while the concentrations of propane, propylene, CO, CO2, and O2 were analyzed using a gas chromatograph equipped with a TCD detector. The conversion rates of acrylic acid, acetic acid, propane + propylene, and CO were calculated. x Selectivity.
[0058] The long-term stability test was conducted continuously for 500 hours at 280℃ and a space velocity of 5000 h⁻¹, with samples taken and analyzed every 24 hours to examine the catalyst activity decay.
[0059] Wherein, the acrylic acid activity decay rate after 500 hours = (X0 − X 500 ) / X0.
[0060] Table 1. Steady-state catalytic performance data at 250℃
[0061] As described in Examples 1-3, the catalyst of the present invention possesses excellent low-temperature purification activity for organic acids, high retention selectivity for propane / propylene, mechanical strength, and long-term thermal stability. By adjusting the ratio of active powder to SiO2 carrier within the range of 50-70:30-50 and matching it with the corresponding primary calcination, silicon coating, and secondary calcination processes, it can balance purification efficiency, raw material protection effect, and industrial molding performance, and is suitable for long-term continuous purification of circulating gas from propane oxidation to acrylic acid.
[0062] A comparison of Example 1 and Comparative Examples 1-3 shows that the low-temperature oxidation activity of the Cu-Mn binary system catalyst prepared by replacing Ce with Y / Zr rare earth elements is significantly reduced, with acrylic acid conversion rates of only 72.5%~84.6%. 90 The ignition temperature rises to 261~305℃; at the same time, Ce-free system grains are prone to sintering and agglomeration at high temperatures, and the activity decay rate is as high as 10.7%~18.6% after 500h long-term operation. Propane and propylene are prone to excessive oxidation and loss, and the total raw material retention rate is less than 97.4%. This proves that the combination of Cu, Ce and Mn ternary metal components has significant electronic synergy and oxygen storage enhancement effect. Rare earth Ce is the core indispensable functional component and cannot be replaced by other rare earth / metal equivalents.
[0063] A comparison of Example 1 and Comparative Examples 4-6 shows that the mechanical strength of the catalyst without silicon coating is only 72 N / cm, which does not meet the industrial standard. Acidic media directly corrodes the core active components, and the activity decays by 14.5% after 500 hours. If the amount of silicon source added is too low, the coating film will have a large number of defects, insufficient resistance to carbon deposition and organic acid corrosion, and a significant decline in organic acid purification efficiency. If the amount of silicon source added is too high, the SiO2 shell will be too thick and block the channels, greatly increasing the diffusion resistance of organic acid molecules, reducing the acrylic acid conversion rate to 82.8%, and significantly increasing the ignition temperature. This proves that the pre-coating process with a specific ratio of organosilicon is the key step in balancing catalytic activity, selectivity, mechanical strength and thermal stability. The silicon source addition ratio must be strictly controlled within the range defined in this invention.
[0064] While the specific embodiments of the present invention have been described above, they are not intended to limit the scope of protection of the present invention. Those skilled in the art should understand that various modifications or variations that can be made by those skilled in the art without creative effort based on the technical solutions of the present invention are still within the scope of protection of the present invention.
Claims
1. A catalyst for purification of a recycle gas of a propane oxidation to propylene acid cycle, characterized in that, The active ingredients are copper, cerium and manganese, and the active ingredients are coated with a SiO2 modification layer. The support is Al2O3 or SiO2. The content of copper, cerium and manganese accounts for 10%-30% of the total mass of the catalyst, and their molar ratio is 1:(1-1.5):(1-3).
2. The catalyst for purification of the propane oxidation to propylene acid cycle gas according to claim 1, characterized by that, The shape of the catalyst is selected from one of the following: columnar, Raschig ring, cloverleaf, and gear.
3. A process for the preparation of a catalyst for the purification of the off-gas of a propane oxidation to propylene acid cycle, characterized by, include: Cu salt solution, Ce salt solution, and Mn salt solution were mixed, and the pH was adjusted to alkaline to form a precipitate. After a single aging reaction, solid-liquid separation, drying, and a single calcination, a composite metal oxide catalyst was obtained. The composite metal oxide catalyst was dispersed in a solvent, an organosilicon source was added under alkaline conditions, a secondary aging reaction was carried out, solid-liquid separation was performed, and the catalyst powder was obtained by drying. The catalyst powder is mixed evenly with the carrier, water and guar gum powder are added, kneaded, extruded into strips, granulated, dried, and then calcined a second time to obtain the final product.
4. The method of producing a catalyst for purifying a propane oxidation to propylene cycle gas according to claim 1, characterized by, The chemical formula of the composite metal oxide catalyst is CuO-CeO2-MnO x .
5. The method of producing a catalyst for purifying a propane oxidation to propylene cycle gas according to claim 1, characterized by, The conditions for the first calcination are: calcination at 350-450℃ for 4-8 hours in an air atmosphere.
6. The method of producing a catalyst for purification of a propane oxidation to propylene acid cycle gas according to claim 1, characterized in that, The mass ratio of the organosilicon source to the composite metal oxide catalyst is (0.05-0.30):
1.
7. The method of producing a catalyst for purification of a propane oxidation to propylene acid cycle gas according to claim 1, characterized in that, The conditions for the secondary aging reaction are a temperature of 60-80℃, a pH value of 8-9, and a time of 3-4 hours.
8. The method of producing a catalyst for purification of a propane oxidation to propylene cycle gas according to claim 1, characterized in that, The mass ratio of catalyst powder to support is (50-70):(30-50).
9. The method for preparing the catalyst for purifying the circulating gas from propane oxidation to acrylic acid as described in claim 1, characterized in that, The secondary roasting conditions are: roasting at 280-580℃ in air for 2-6 hours.
10. The use of the catalyst according to any one of claims 1-2 or the catalyst prepared by the method according to any one of claims 3-9 in the purification of circulating gas from propane oxidation to acrylic acid.
Citation Information
Patent Citations
Applicable load-type catalyst for purifying air at room temperature
CN105478134A