Method for synergistically enhancing the performance of silica optical thin films by ultraviolet and thermal curing

By synergistically enhancing silica optical films through UV curing and thermal curing, an organic-inorganic network is constructed, solving the problem of easy damage to existing films under high-power lasers and achieving a combination of high transmittance and high mechanical strength.

CN123102602APending Publication Date: 2026-11-17UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610371335.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-03-25
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silica optical films are prone to fatigue damage under high-power laser shock, and a single curing process cannot simultaneously guarantee optical performance and mechanical strength.

Method used

A method for synergistic enhancement of silica optical films using UV curing and thermosetting is employed. This involves modifying the film with a silane coupling agent and constructing an organic network, followed by UV curing to form a preliminary cross-linked network, and then thermosetting to construct a dense inorganic network.

Benefits of technology

It significantly improves the film's hardness and laser damage resistance threshold, while also enhancing light transmittance and film-substrate adhesion, ensuring the film's mechanical stability and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102602A_ABST
    Figure CN123102602A_ABST
Patent Text Reader

Abstract

This invention discloses a method for synergistically enhancing the performance of silica optical thin films through UV curing and thermal curing, relating to the field of optical thin film technology. The method includes: catalytic hydrolysis of tetraethyl orthosilicate with ammonia and aging to obtain a silica sol; modification with a silane coupling agent and aging to obtain a modified sol; refluxing the modified sol to remove ammonia, obtaining a deaminated sol; adding a photoinitiator and film-forming aid to the deaminated sol, spin-coating, and then sequentially performing UV curing and thermal curing treatments to obtain a silica optical thin film. This invention, through the synergistic effect of UV curing and thermal curing, constructs an organic-inorganic hybrid network structure, effectively improving the density, hardness, and adhesion of the film to the substrate, significantly enhancing the film's resistance to laser damage, while maintaining good light transmittance at specific wavelengths.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of optical thin film technology, specifically relating to a method for synergistic enhancement of the performance of silicon dioxide optical thin films through ultraviolet curing and thermal curing. Background Technology

[0002] With the widespread application of high-power lasers in laser fusion (such as the National Ignition Project) and civilian laser processing, the output power and energy density of lasers are constantly increasing, placing higher demands on the load capacity of optical components. In high-power pulsed laser drivers, optical thin films need to be deposited on the surfaces of various optical components to reduce transmission loss. Therefore, the thin films must not only have high transmittance, but also excellent resistance to laser damage and mechanical stability.

[0003] The sol-gel method has become a commonly used technique for preparing optical thin films due to its simple process and easy control of components. Among them, silica sol is widely used to prepare optical antireflective films because of its high porosity and good environmental stability after film formation. However, current silica optical thin films prepared by the sol-gel method still have the following shortcomings: First, the nanoparticles inside the film are mainly bound by weak van der Waals forces, which can easily lead to fatigue damage under high-frequency or high-energy laser shock; second, the curing process is singular. Ultraviolet light curing alone is prone to incomplete deep curing due to oxygen inhibition or limited light penetration depth, while simple thermal curing may generate large thermal stress due to solvent evaporation and skeleton shrinkage, causing the film to crack. It is difficult to simultaneously achieve both optical performance and mechanical strength of the film. Therefore, how to achieve efficient and crack-free curing of thin films while ensuring their excellent optical performance has become an urgent technical problem to be solved in this field. Summary of the Invention

[0004] In view of the above-mentioned defects in the prior art, the purpose of the present invention is to provide a method for synergistic enhancement of the performance of silica optical films by ultraviolet curing and thermal curing, so as to overcome the problems of insufficient mechanical strength and poor resistance to laser damage of existing silica films.

[0005] The technical solution adopted in this invention is as follows: A method for synergistically enhancing the properties of silica optical thin films through UV curing and thermal curing includes the following steps: Step 1: Using anhydrous ethanol as a solvent, tetraethyl orthosilicate is hydrolyzed under the catalysis of ammonia water, and after aging, silica sol is obtained; Step 2: Add a silane coupling agent to the silica sol to carry out a modification reaction, and after aging, obtain a modified sol; Step 3: The modified sol is refluxed to remove ammonia, resulting in a deammoniated sol; Step 4: Add photoinitiator and film-forming aid to the deaminated sol, mix well, and obtain coating sol; Step 5: Using the aforementioned coating sol, a film layer is formed on the substrate by spin coating, followed by UV curing and thermal curing treatments. After cooling, a silicon dioxide optical thin film is obtained.

[0006] Further, in step 1, the mass concentration of the ammonia water is 28%; the molar ratio of tetraethyl orthosilicate, ammonia water and anhydrous ethanol is 1:(2~4):40; the hydrolysis temperature is 20~30 ℃, the hydrolysis time is 2~3 h; the aging temperature is 20~30 ℃, and the aging time is 3~5 days.

[0007] Further, in step 2, the silane coupling agent is γ-methacryloxypropyltrimethoxysilane, and its molar ratio with tetraethyl orthosilicate in step 1 is (0.01~0.12):1; the modification reaction temperature is 20~30 ℃, the reaction time is 2~3 h; the aging temperature is 20~30 ℃, and the aging time is 3~5 days.

[0008] Furthermore, in step 3, the reflux temperature is 40~60 ℃ and the reflux time is 3~6 h.

[0009] Further, in step 4, the photoinitiator is one of 1-hydroxycyclohexylphenyl ketone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzoyl isopropyl ether, or 4,4'-diisopropyldiphenyliodonium hexafluorophosphate; the mass ratio of the deaminated sol to the photoinitiator is 1:(0.01~0.03).

[0010] Further, in step 4, the film-forming aid is one of isopropanol, n-butanol, ethanol, sec-butanol, cyclohexane, n-heptane, or ethylene glycol monoethyl ether; the mass ratio of deaminated sol to film-forming aid is 1:(0.3~0.6).

[0011] Furthermore, in step 5, the rotational speed of the spin coating is 1000~1200 r / min, the coating time is 20~40 s; the UV curing power is 180~220 mW / cm², the curing time is 10~30 s; the temperature of the heat curing treatment is 120~160 ℃, and the time is 3~6 h.

[0012] Furthermore, in step 5, the substrate is quartz glass, which needs to be cleaned before use: the quartz glass is immersed in an alkaline cleaning solution for washing, rinsed with clean water, and then wiped with a mixed solution of ethanol and ether in a volume ratio of 1:2 until there are no stains on the surface, and then dried for use.

[0013] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) This invention achieves the synergistic construction of organic and inorganic networks through the combined effect of UV curing and thermal curing. UV curing stimulates the free radical polymerization of carbon-carbon double bonds in the silane coupling agent, forming an organic cross-linked network between silica nanoparticles, effectively anchoring the particles and imparting good formability and toughness to the film. Thermal curing promotes further condensation of incompletely condensed silanol groups within the film, forming a denser Si-O-Si inorganic network. Experiments show that under two different precursor ratios (the molar ratio of tetraethyl orthosilicate, ammonia, and anhydrous ethanol in Example 1 was 1:2:40, and in Example 2 it was 1:3:40), the films simultaneously cured by UV and thermal curing achieved hardnesses of 471 MPa and 512 MPa, respectively; while the films of Comparative Examples 1 and 2, which only underwent UV curing and omitted the thermal curing step, had hardnesses of only 230 MPa and 290 MPa, respectively, significantly lower than the corresponding examples. This indicates that, regardless of how the basic formulation is adjusted, the thermosetting step plays an indispensable role in constructing a dense inorganic network and significantly improving the mechanical strength of the film.

[0014] (2) The synergistic effect of UV curing and thermal curing improves the transmittance of silica films at 527 nm. The films prepared by the method of this invention in Examples 1 and 2 achieved transmittances of 96.77% and 96.70% at the target wavelength, respectively. In contrast, the films of Comparative Examples 1 and 2, which were only UV-cured, had transmittances of 96.63% and 96.55% at the target wavelength, respectively. UV light can quickly induce preliminary curing of the film, forming a stable silica network structure. Subsequent thermal curing can promote the further reaction of residual hydroxyl groups inside the film and remove moisture, thereby reducing the absorption caused by hydroxyl groups in the visible light region. At the same time, heat treatment makes the film structure more compact, reduces the number of internal voids, and reduces light scattering caused by voids. In addition, heating can remove unreacted organic matter and a small amount of impurities in the film, release the internal stress caused by rapid UV curing, reduce the loss caused by internal defects and surface reflection, and ultimately enable the silica film to achieve higher transmittance at 527 nm.

[0015] (3) Thermosetting treatment can promote stronger chemical bonding between the film and the quartz glass substrate, significantly enhancing the adhesion between the film and the substrate. At the same time, the organic network formed by UV curing can buffer thermal stress and reduce the risk of interface cracking caused by mismatch in thermal expansion coefficients. The resulting film has good mechanical stability and durability. Most importantly, this structural stability significantly improves the laser damage threshold of the film. Test results show that under laser irradiation at a wavelength of 351 nm and a pulse width of 4 ns, the laser damage thresholds of the films of Examples 1 and 2 prepared by the method of this invention reached 14.52 J / cm² and 15.65 J / cm², respectively. In contrast, the films of Comparative Examples 1 and 2, which only underwent UV curing, lacked thermosetting treatment, resulting in a loose film structure and insufficient hardness. Irreversible damage occurred at lower laser energies, and neither could obtain a stable and reliable damage threshold. This fully demonstrates that regardless of the basic formulation, thermosetting treatment is a necessary step in constructing films with high laser damage resistance, and its synergistic effect with UV curing is the key to achieving the purpose of this invention. Attached Figure Description

[0016] Figure 1 This is a flowchart of the silicon dioxide optical thin film preparation process of the present invention.

[0017] Figure 2 This is a comparison chart of the hardness test results of the films prepared in Example 1 and Comparative Example 1 of the present invention.

[0018] Figure 3 These are the ultraviolet-visible-near-infrared transmission spectra of the thin films prepared in Example 1 and Comparative Example 1 of this invention.

[0019] Figure 4 This is a graph showing the laser damage threshold test results of the thin film prepared in Example 1 of the present invention.

[0020] Figure 5 This is a comparison chart of the hardness test results of the films prepared in Example 2 and Comparative Example 2 of the present invention.

[0021] Figure 6 These are the ultraviolet-visible-near-infrared transmission spectra of the films prepared in Example 2 and Comparative Example 2 of the present invention.

[0022] Figure 7 This is a graph showing the laser damage threshold test results of the thin film prepared in Example 2 of the present invention. Detailed Implementation

[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention. The preparation process of this invention is as follows: Figure 1 As shown.

[0024] To verify the crucial role of the thermosetting step in the method of this invention and to examine its universality under different formulations, the following comparative examples were set up: Comparative Example 1 compared with Example 1 (molar ratio of tetraethyl orthosilicate, ammonia, and anhydrous ethanol was 1:2:40), and Comparative Example 2 compared with Example 2 (molar ratio of tetraethyl orthosilicate, ammonia, and anhydrous ethanol was 1:3:40). These examples were used to examine the effect of omitting the thermosetting step on the film properties under two different precursor ratios. The only difference between Comparative Example 1 and Example 1 was that thermosetting was not performed in step 5; all other steps and parameters were the same. The only difference between Comparative Example 2 and Example 2 was that thermosetting was not performed in step 5; all other steps and parameters were the same.

[0025] Example 1 This embodiment provides a method for synergistically enhancing the performance of silica optical thin films through UV curing and thermal curing, including the following steps: Step 1: Mix tetraethyl orthosilicate, 28% ammonia solution, and anhydrous ethanol in a molar ratio of 1:2:40 and stir at 25 °C for 2 h. Transfer the reaction solution to a sealed container and age at 25 °C for 4 days to obtain silica sol.

[0026] Step 2: To the silica sol obtained in Step 1, γ-methacryloxypropyltrimethoxysilane was added dropwise at a molar ratio of 0.02:1 to tetraethyl orthosilicate from Step 1. The mixture was stirred at 25 °C for 2 h. After the reaction was complete, the mixture was transferred to a sealed container and aged at 25 °C for 3 days to obtain the modified sol.

[0027] Step 3: Transfer the modified sol obtained in Step 2 to a flask equipped with a reflux device, set the oil bath temperature to 55 ℃, and reflux continuously for 4 hours to obtain a deaminated sol.

[0028] Step 4: Weigh 100 g of the deaminated sol obtained in Step 3, add 1 g of photoinitiator 2-hydroxy-2-methyl-1-phenyl-1-propanone and 40 g of film-forming aid sec-butanol, stir for 1 hour until the mixture is uniform, and obtain the coating sol.

[0029] Step 5: Soak and wash the quartz glass substrate with an alkaline cleaning solution, rinse thoroughly with clean water, and then repeatedly scrub under a strong light with a mixed solution of ethanol and ether (volume ratio 1:2) until the surface is free of any stains. Dry and set aside. Using a spin coating method, drop the coating sol from Step 4 onto the treated quartz glass substrate, set the spin speed to 1100 r / min, and spin coat for 30 s. Cure the coated film under a 200 mW / cm² UV lamp for 20 s, then transfer it to an oven and heat-cur at 140℃ for 4 hours. Allow it to cool naturally to room temperature to obtain the silica optical thin film.

[0030] The performance of the thin film prepared in this embodiment was tested, and the results are as follows: under laser irradiation with a wavelength of 351 nm and a pulse width of 4 ns, its laser damage threshold is 14.52 J / cm²; the light transmittance at the target wavelength of 527 nm is 96.77%; and the average hardness of the thin film is 471 MPa as measured by a nanoindenter.

[0031] Example 2 This embodiment is basically the same as Embodiment 1, except that the molar ratio of tetraethyl orthosilicate, ammonia and anhydrous ethanol in step 1 is 1:3:40.

[0032] The performance of the thin film prepared in this embodiment was tested, and the results are as follows: under laser irradiation with a wavelength of 351 nm and a pulse width of 4 ns, its laser damage threshold is 15.65 J / cm²; the light transmittance at the target wavelength of 527 nm is 96.70%; and the average hardness of the thin film is 512 MPa as measured by a nanoindenter.

[0033] Comparative Example 1: The only difference between this comparative example and Example 1 is that the thermosetting process was not performed in step 5.

[0034] The performance of the thin film prepared in this comparative example was tested, and the results are as follows: When tested under laser irradiation with a wavelength of 351 nm and a pulse width of 4 ns, the sample underwent irreversible damage at a low laser energy, making it impossible to obtain a stable and reliable damage threshold, and its resistance to laser damage was significantly lower; the light transmittance at the target wavelength of 527 nm was 96.63%, slightly lower than that of Example 1; the average hardness of the film was 230 MPa, significantly lower than that of Example 1, as measured by a nanoindenter.

[0035] Comparative Example 2: The only difference between this comparative example and Example 2 is that the thermosetting process was not performed in step 5.

[0036] The performance of the thin film prepared in this comparative example was tested, and the results are as follows: When tested under laser irradiation with a wavelength of 351 nm and a pulse width of 4 ns, the sample was damaged at a low laser energy, and a stable and reliable damage threshold could not be obtained; the light transmittance at the target wavelength of 527 nm was 96.55%, which was slightly lower than that of Example 2; the average hardness of the film was 290 MPa, which was significantly lower than that of Example 2, as measured by a nanoindenter.

[0037] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of protection of this invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the scope of protection of this application. Therefore, the scope of protection of this patent application should be determined by the appended claims.

Claims

1. A method for synergistically enhancing the properties of silica optical thin films through UV curing and thermal curing, characterized in that, Includes the following steps: Step 1: Using anhydrous ethanol as a solvent, tetraethyl orthosilicate is hydrolyzed under the catalysis of ammonia water, and after aging, silica sol is obtained; Step 2: Add a silane coupling agent to the silica sol to carry out a modification reaction, and after aging, obtain a modified sol; Step 3: The modified sol is refluxed to remove ammonia, resulting in a deammoniated sol; Step 4: Add photoinitiator and film-forming aid to the deaminated sol, mix well, and obtain coating sol; Step 5: Using the aforementioned coating sol, a film layer is formed on the substrate by spin coating, followed by UV curing and thermal curing treatments. After cooling, a silicon dioxide optical thin film is obtained.

2. The method according to claim 1, characterized in that, In step 1, the mass concentration of the ammonia water is 28%; the molar ratio of tetraethyl orthosilicate, ammonia water and anhydrous ethanol is 1:(2~4):40; the hydrolysis temperature is 20~30 ℃ and the hydrolysis time is 2~3 h; the aging temperature is 20~30 ℃ and the aging time is 3~5 days.

3. The method according to claim 1, characterized in that, In step 2, the silane coupling agent is γ-methacryloxypropyltrimethoxysilane, and its molar ratio with tetraethyl orthosilicate in step 1 is (0.01~0.12):1; the modification reaction temperature is 20~30 ℃, the reaction time is 2~3 h; the aging temperature is 20~30 ℃, and the aging time is 3~5 days.

4. The method according to claim 1, characterized in that, In step 3, the reflux temperature is 40~60 ℃ and the reflux time is 3~6 h.

5. The method according to claim 1, characterized in that, In step 4, the photoinitiator is one of 1-hydroxycyclohexylphenyl ketone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzoyl isopropyl ether, or 4,4'-diisopropyldiphenyliodonium hexafluorophosphate; the mass ratio of the deaminated sol to the photoinitiator is 1:(0.01~0.03).

6. The method according to claim 1, characterized in that, In step 4, the film-forming aid is one of isopropanol, n-butanol, ethanol, sec-butanol, cyclohexane, n-heptane, or ethylene glycol monoethyl ether; the mass ratio of deaminated sol to film-forming aid is 1:(0.3~0.6).

7. The method according to claim 1, characterized in that, In step 5, the rotation speed of the spin coating is 1000~1200 r / min, the coating time is 20~40 s; the UV curing power is 180~220 mW / cm², the curing time is 10~30 s; the temperature of the heat curing treatment is 120~160 ℃, and the time is 3~6 h.

8. The method according to claim 1, characterized in that, In step 5, the substrate is quartz glass, which needs to be cleaned before use: immerse the quartz glass in an alkaline cleaning solution, rinse with clean water, and then wipe it with a mixed solution of ethanol and ether in a volume ratio of 1:2 until there are no stains on the surface. After drying, it is ready for use.