A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system
By using a eutectic solvent formed by choline chloride and hydrogen bond donors to process photovoltaic laminates under the synergistic effect of ultrasound and thermal field, the problem of high-temperature and long-term processing in existing technologies has been solved. This enables rapid and efficient separation of EVA film from glass substrate, reduces energy consumption and equipment complexity, and promotes the recycling of photovoltaic glass.
Patent Information
- Application Number
- CN202611512465.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for processing waste photovoltaic module EVA film suffer from problems such as high operating temperature, long processing time, the need for pre-cutting or mechanical peeling, and difficulty in processing complete photovoltaic laminates, resulting in high energy consumption, complex equipment, and uneconomical practices.
A eutectic solvent formed by choline chloride and hydrogen bond donors is used as the reaction medium to process photovoltaic laminates under the simultaneous action of ultrasonic and thermal fields, achieving rapid separation of EVA film from glass substrate, combined with the recycling of the eutectic solvent.
This technology enables rapid depolymerization of EVA film at moderate temperatures, reducing energy consumption, simplifying the processing flow, improving separation efficiency, reducing the risk of glass substrate breakage, and promoting the recycling of photovoltaic glass.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of resource recycling technology for waste photovoltaic modules, specifically to a method for catalytic depolymerization of waste photovoltaic module EVA film using a eutectic solvent system. Background Technology
[0002] With the continuous growth of photovoltaic power generation capacity, the recycling and disposal of retired photovoltaic modules is becoming increasingly urgent. In crystalline silicon photovoltaic modules, EVA film serves as a key encapsulation and bonding layer between the solar cells and photovoltaic glass. Its cross-linked three-dimensional network structure gives the module excellent weather resistance and bonding strength, but it also makes it difficult to separate the various functional layers after the module reaches the end of its service life, becoming a bottleneck restricting recycling efficiency.
[0003] Currently, EVA film removal methods mainly fall into two categories: high-temperature pyrolysis and chemical solvent treatment. Pyrolysis is typically carried out at temperatures above 400 °C in an oxygen-free or inert atmosphere, where EVA molecular chains undergo random chain scission and depolymerization / crosslinking reactions, generating a mixture of small-molecule hydrocarbons. However, this process is extremely energy-intensive (consuming over 800 kWh per ton of module). Furthermore, the thermal decomposition of vinyl acetate segments in EVA releases acetic acid and halogenated byproducts, corroding equipment. The resulting coke adheres to the glass surface, significantly reducing the light transmittance of the recycled glass. Chemical solvent treatment utilizes aromatic or halogenated hydrocarbon organic solvents such as toluene, chlorobenzene, and trichloroethylene to swell the EVA film under heating conditions, weakening its interfacial adhesion to the glass substrate and thus achieving peeling. However, these organic solvents generally suffer from high volatility, high toxicity, and difficulty in recovery, with single-use loss rates often exceeding 50%. Moreover, the solvent recovery distillation process is energy-intensive, resulting in poor overall economic efficiency. Although chemical degradation methods using strong acid or strong alkali solutions can hydrolyze EVA ester groups at higher temperatures, the waste liquid is difficult to treat, and the corrosive media erodes the surface of photovoltaic glass, reducing its secondary utilization value.
[0004] Deep eutectic solvents (DES) are low-melting-point eutectic mixtures formed by the hydrogen bonding interactions of two or more components. They are typically composed of quaternary ammonium salts (such as choline chloride) as hydrogen bond acceptors combined with hydrogen bond donors such as organic acids, amides, or polyols in a specific stoichiometric ratio. DES combines the advantages of ionic liquids—high designability and extremely low vapor pressure—with ease of preparation, wide availability of raw materials, and good biocompatibility, and has been applied in fields such as metal leaching, polymer degradation, and biomass pretreatment. In recent years, some studies have attempted to apply DES to the separation of EVA films in photovoltaic modules. For example, the team at Kunming University of Science and Technology used choline chloride-oxalic acid DES, hydrothermally treating it in a high-pressure reactor at 175°C for 12.5 hours, achieving a 100% EVA separation rate. There are also related patent reports using a betaine-oxalic acid system. However, the reported DES treatment methods still have the following obvious shortcomings: (1) The reaction temperature is too high (175℃), which is close to or even exceeds the decomposition temperature of some DES components. Long-term heating can easily lead to solvent denaturation and deterioration. At the same time, the high operating temperature also increases energy consumption and equipment sealing requirements; (2) The treatment cycle is long (12.5 h), which is difficult to meet the efficiency requirements of large-scale recycling; (3) It needs to be carried out in a high-pressure reactor, which requires large equipment investment and complex processes. Existing literature generally adopts the experimental scheme of physically peeling the EVA film from the module before treatment, which does not solve the technical problem of overall treatment of laminates containing complete glass substrates. In practical applications, additional pretreatment steps are still required, which increases the process steps and the risk of breakage. Therefore, developing a DES system that can quickly treat complete photovoltaic laminates containing glass substrates at a moderate temperature and whose solvent can be recycled multiple times is of practical significance for promoting the development of green recycling technology for photovoltaic modules. Summary of the Invention
[0005] To overcome the problems of high operating temperature, long processing time, need for pre-cutting or mechanical peeling of photovoltaic modules, and difficulty in directly processing photovoltaic laminates containing intact glass substrates when using eutectic solvents to treat waste EVA films of photovoltaic modules, this invention provides a method for catalytic depolymerization of waste EVA films of photovoltaic modules using a eutectic solvent system. This method uses a eutectic solvent formed by choline chloride and a hydrogen bond donor as the reaction medium. The photovoltaic laminated glass module containing the EVA film is immersed in the eutectic solvent and treated under the simultaneous action of an ultrasonic field and a thermal field, thereby achieving rapid depolymerization of the EVA film and separation of the EVA film from the glass substrate, while simultaneously realizing the recycling of photovoltaic glass and the reuse of the eutectic solvent.
[0006] This invention is achieved through the following technical solutions:
[0007] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0008] (1) The hydrogen bond acceptor and the hydrogen bond donor are mixed in a molar ratio of 1:1 to 1:3 and stirred at 70°C to 80°C for 1 to 4 hours until a homogeneous and transparent liquid is formed to obtain a eutectic solvent (DES); the hydrogen bond acceptor is choline chloride and the hydrogen bond donor is selected from any one or more of oxalic acid, citric acid, malonic acid, ethylene glycol and glycerol.
[0009] (2) The photovoltaic laminated glass module containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely immersed in the liquid phase system. Under the condition that the photovoltaic laminate is not cut, crushed or mechanically peeled off beforehand, ultrasonic and heating treatments are performed simultaneously. The ultrasonic treatment frequency is 40 kHz and the power is 200~600 W. The heating temperature is 120℃~160℃ and the treatment time is 1~4 h. After the treatment, the complete glass substrate is separated from the reaction medium, and recycled glass is obtained after cleaning and drying. At the same time, the eutectic solvent is recovered.
[0010] Preferably, the hydrogen bond donor in step (1) is oxalic acid, and the molar ratio of choline chloride to oxalic acid is 1:1.
[0011] Preferably, the preparation conditions of the eutectic solvent in step (1) are as follows: stir the reaction at 70℃~80℃ for 2 h to fully mix choline chloride and hydrogen bond donor and form a homogeneous eutectic solvent system.
[0012] Preferably, the ultrasonic power in step (2) is 400~500 W, the frequency is 40 kHz, the heating temperature is 140℃~150℃, and the processing time is 2 h.
[0013] Preferably, the photovoltaic laminated glass module described in step (2) is immersed as a whole in a eutectic solvent for depolymerization treatment. The photovoltaic laminated glass module does not require pre-cutting, crushing, or mechanical peeling of the EVA film.
[0014] More preferably, the size of the photovoltaic laminated glass module is 50 mm × 50 mm.
[0015] Preferably, the ultrasonic treatment and heating treatment described in step (2) are carried out simultaneously. The synergistic effect of the ultrasonic field and the thermal field promotes the penetration of the eutectic solvent into the EVA adhesive layer and promotes the depolymerization of the EVA crosslinking network.
[0016] The synergistic effect of the ultrasonic field and the thermal field promotes full contact between the eutectic solvent and the EVA adhesive layer, and promotes the mass transfer of the eutectic solvent into the interior of the EVA adhesive layer, thereby promoting the depolymerization of the EVA crosslinking network and the separation between the EVA adhesive film and the glass substrate.
[0017] Further, the method for recovering the eutectic solvent in step (2) is as follows: the eutectic solvent system after the reaction is filtered to separate the solid residue, and the resulting filtrate is treated by rotary evaporation to recover the eutectic solvent for recycling.
[0018] This invention also protects the application of the above method in the depolymerization of EVA film in waste photovoltaic modules and the recycling of photovoltaic glass.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] 1. This invention uses a eutectic solvent formed by choline chloride and organic acid or polyol as a reaction medium. The eutectic solvent promotes the depolymerization of the EVA crosslinking network through full contact with the EVA adhesive layer. Combined with the synchronous action of ultrasonic field and thermal field, the processing efficiency of EVA adhesive film is improved.
[0021] 2. This invention utilizes the strongly polar hydrogen bond network microenvironment formed between hydrogen bond donors and acceptors in DES to produce a highly efficient swelling-penetration effect on EVA crosslinked macromolecules. Combined with the physical weakening of the interfacial adhesive layer by ultrasonic cavitation and the promoting effect of the thermal field on molecular chain motion, the three factors work synergistically to achieve rapid depolymerization at 150°C within 2 hours. This is significantly milder and more efficient than the operating conditions of above 170°C and ten hours reported for existing DES.
[0022] 3. This invention enables photovoltaic laminated glass modules containing EVA adhesive layers to be directly immersed in a eutectic solvent for processing as complete laminates, without the need for pre-cutting, crushing, or mechanically peeling off the EVA adhesive film from the photovoltaic modules. This reduces the pre-processing steps for photovoltaic modules and lowers the possibility of glass substrate breakage during mechanical processing, which is beneficial for the recycling of complete photovoltaic glass.
[0023] 4. This invention enables the control of the EVA film depolymerization process by adjusting the composition and molar ratio of choline chloride and hydrogen bond donors, as well as process parameters such as ultrasonic power, processing temperature, and processing time. Specifically, a higher EVA decomposition rate can be obtained under the preferred choline chloride-oxalic acid eutectic solvent system and simultaneous ultrasonic-thermal treatment conditions.
[0024] 5. The method for preparing the eutectic solvent used in this invention is simple. A homogeneous eutectic solvent system can be obtained by mixing choline chloride and hydrogen bond donor in a certain proportion and heating and stirring. After the reaction is completed, the reaction medium can be recovered by solid-liquid separation and rotary evaporation, which provides conditions for the recycling of the eutectic solvent. Detailed Implementation
[0025] The following embodiments are further illustrations of the present invention, but not limitations thereof.
[0026] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention. Unless otherwise specified, the experimental materials and reagents used herein are commercially available products conventionally available in this technical field.
[0027] Example 1
[0028] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0029] (1) Preparation of eutectic solvent: Choline chloride (ChCl) and oxalic acid (Oxa) were added to a round-bottom flask at a molar ratio of 1:1 and stirred in an oil bath at 70°C for 2 h until a clear and transparent homogeneous liquid was formed, thus obtaining choline chloride-oxalic acid (ChCl-Oxa) eutectic solvent with a viscosity of 80~90 mPa·s at 25°C.
[0030] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely wetted in the liquid phase system; the ultrasonic treatment device and the heating temperature control system are turned on simultaneously, wherein: the ultrasonic power is set to 400 W, the fixed frequency is 40 kHz, the heating temperature is controlled at 150℃, and the treatment time is set to 2 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass and the eutectic solvent is recovered at the same time.
[0031] The test results showed that the EVA decomposition rate reached 99.3%, achieving efficient and green separation between the glass substrate and the EVA film, as detailed in Table 1.
[0032] Comparative Example 1:
[0033] Referring to Example 1, the difference is that only choline chloride is used in step (1) (without adding hydrogen bond donor oxalic acid), and no eutectic solvent is formed. Choline chloride (ChCl) is stirred at 70 °C for 2 h to form a transparent liquid.
[0034] A method for catalytically depolymerizing waste EVA encapsulant film from photovoltaic modules includes the following steps:
[0035] (1) Preparation of solvent: Chlorochloride (ChCl) was stirred at 70 °C for 2 h to form a transparent liquid.
[0036] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the solvent obtained in step (1) to ensure that the module is completely wetted in the liquid phase system; the ultrasonic treatment device and the heating temperature control system are turned on simultaneously, wherein: the ultrasonic power is set to 400 W, the fixed frequency is 40 kHz, the heating temperature is controlled at 150℃, and the treatment time is set to 2 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass.
[0037] The test showed that the EVA decomposition rate was 18.7%, indicating that choline chloride alone does not have the effective ability to depolymerize the EVA crosslinked network. The introduction of hydrogen bond donors is a necessary condition for the formation of DES with depolymerization activity.
[0038] Comparative Example 2:
[0039] Referring to Example 1, the difference is that only oxalic acid is used in step (1) (choline chloride is not added), and the oxalic acid is stirred at 70 °C for 2 h.
[0040] A method for catalytically depolymerizing waste EVA encapsulant film from photovoltaic modules includes the following steps:
[0041] (1) Preparation of solvent: Oxalic acid was stirred at 70 °C for 2 h to form a transparent liquid.
[0042] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the solvent obtained in step (1) to ensure that the module is completely wetted in the liquid phase system; the ultrasonic treatment device and the heating temperature control system are turned on simultaneously, wherein: the ultrasonic power is set to 400 W, the fixed frequency is 40 kHz, the heating temperature is controlled at 150℃, and the treatment time is set to 2 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass.
[0043] The EVA decomposition rate was found to be 52.6%.
[0044] Comparative Example 3:
[0045] Referring to Example 1, the difference is that the ultrasonic processing device is not turned on in step (2).
[0046] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0047] (1) Preparation of eutectic solvent: Choline chloride (ChCl) and oxalic acid (Oxa) were added to a round-bottom flask at a molar ratio of 1:1 and stirred in an oil bath at 70°C for 2 h until a clear and transparent homogeneous liquid was formed, thus obtaining choline chloride-oxalic acid (ChCl-Oxa) eutectic solvent with a viscosity of 80~90 mPa·s at 25°C.
[0048] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely wetted in the liquid phase system; only the heating temperature control system is turned on, the heating temperature is controlled at 150°C, and the treatment time is set to 2 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass and the eutectic solvent is recovered at the same time.
[0049] The test showed that the EVA decomposition rate was 72.3%, which was significantly lower than that of Example 1, indicating that the synergistic effect of the ultrasonic field and the thermal field is one of the key factors for achieving efficient and rapid depolymerization of EVA.
[0050] Comparative Example 4:
[0051] Referring to Example 1, the difference is that the heating temperature control system is not turned on in step (2).
[0052] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0053] (1) Preparation of eutectic solvent: Choline chloride (ChCl) and oxalic acid (Oxa) were added to a round-bottom flask at a molar ratio of 1:1 and stirred in an oil bath at 70°C for 2 h until a clear and transparent homogeneous liquid was formed, thus obtaining choline chloride-oxalic acid (ChCl-Oxa) eutectic solvent with a viscosity of 80~90 mPa·s at 25°C.
[0054] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely wetted in the liquid phase system; only the ultrasonic treatment device is turned on, the ultrasonic power is set to 400 W, the ultrasonic power is set to a fixed frequency of 40 kHz, and the treatment time is set to 2 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass and the eutectic solvent is recovered at the same time.
[0055] The EVA decomposition rate was found to be 66.3%.
[0056] Example 2:
[0057] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0058] (1) Preparation of eutectic solvent: Choline chloride and citric acid were added to a round-bottom flask at a molar ratio of 1:1 and stirred in an oil bath at 70°C for 2 h until a clear and transparent homogeneous liquid was formed, thus obtaining choline chloride-citric acid eutectic solvent.
[0059] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely wetted in the liquid phase system; the ultrasonic treatment device and the heating temperature control system are turned on simultaneously, wherein: the ultrasonic power is set to 400 W, the fixed frequency is 40 kHz, the heating temperature is controlled at 150℃, and the treatment time is set to 2 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass and the eutectic solvent is recovered at the same time.
[0060] The test results showed that the EVA decomposition rate reached 97.8%, achieving efficient and green separation between the glass substrate and the EVA film, as detailed in Table 1.
[0061] Example 3:
[0062] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0063] (1) Preparation of eutectic solvent: Choline chloride and malonic acid were added to a round-bottom flask at a molar ratio of 1:1 and stirred in an oil bath at 70°C for 2 h until a clear and transparent homogeneous liquid was formed, thus obtaining the choline chloride-malonic acid eutectic solvent.
[0064] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely wetted in the liquid phase system; the ultrasonic treatment device and the heating temperature control system are turned on simultaneously, wherein: the ultrasonic power is set to 400 W, the fixed frequency is 40 kHz, the heating temperature is controlled at 150℃, and the treatment time is set to 2 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass and the eutectic solvent is recovered at the same time.
[0065] The EVA decomposition rate was found to be 88.1%, as detailed in Table 1.
[0066] Example 4:
[0067] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0068] (1) Preparation of eutectic solvent: Choline chloride (ChCl) and oxalic acid (Oxa) were added to a round-bottom flask at a molar ratio of 1:2 and stirred in an oil bath at 70 °C for 2 h until a clear and transparent homogeneous liquid was formed. The eutectic solvent of choline chloride-oxalic acid (ChCl-Oxa) was prepared, with a viscosity of 80~90 mPa·s at 25 °C.
[0069] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely wetted in the liquid phase system; the ultrasonic treatment device and the heating temperature control system are turned on simultaneously, wherein: the ultrasonic power is set to 400 W, the fixed frequency is 40 kHz, the heating temperature is controlled at 150℃, and the treatment time is set to 2 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass and the eutectic solvent is recovered at the same time.
[0070] The test results showed that the EVA decomposition rate reached 97.7%, achieving efficient and green separation between the glass substrate and the EVA film, as detailed in Table 1.
[0071] Example 5:
[0072] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0073] (1) Add choline chloride (ChCl) and oxalic acid (Oxa) in a molar ratio of 1:3 into a round-bottom flask and stir in an oil bath at 70°C for 2 h until a clear and transparent homogeneous liquid is formed. The choline chloride-oxalic acid (ChCl-Oxa) eutectic solvent is prepared with a viscosity of 80~90 mPa·s at 25°C.
[0074] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely wetted in the liquid phase system; the ultrasonic treatment device and the heating temperature control system are turned on simultaneously, wherein: the ultrasonic power is set to 400 W, the fixed frequency is 40 kHz, the heating temperature is controlled at 150℃, and the treatment time is set to 2 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass and the eutectic solvent is recovered at the same time.
[0075] The test results showed that the EVA decomposition rate reached 94.8%, achieving efficient and green separation between the glass substrate and the EVA film, as detailed in Table 1.
[0076] Example 6:
[0077] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0078] (1) Preparation of eutectic solvent: Choline chloride (ChCl) and oxalic acid (Oxa) were added to a round-bottom flask at a molar ratio of 1:1 and stirred in an oil bath at 70°C for 2 h until a clear and transparent homogeneous liquid was formed, thus obtaining choline chloride-oxalic acid (ChCl-Oxa) eutectic solvent with a viscosity of 80~90 mPa·s at 25°C.
[0079] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely immersed in the liquid phase system; the ultrasonic treatment device and the heating temperature control system are turned on simultaneously, wherein: the ultrasonic power is set to 400 W, the fixed frequency is 40 kHz, the heating temperature is controlled at 120℃, and the treatment time is set to 2 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass and the eutectic solvent is recovered at the same time.
[0080] The test results showed that the EVA decomposition rate reached 92.5%, achieving efficient and green separation between the glass substrate and the EVA film, as detailed in Table 1.
[0081] Example 7:
[0082] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0083] (1) Preparation of eutectic solvent: Choline chloride (ChCl) and oxalic acid (Oxa) were added to a round-bottom flask at a molar ratio of 1:1 and stirred in an oil bath at 70°C for 2 h until a clear and transparent homogeneous liquid was formed, thus obtaining choline chloride-oxalic acid (ChCl-Oxa) eutectic solvent with a viscosity of 80~90 mPa·s at 25°C.
[0084] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely immersed in the liquid phase system; the ultrasonic treatment device and the heating temperature control system are turned on at the same time, wherein: the ultrasonic power is set to 400 W, the fixed frequency is 40 kHz, the heating temperature is controlled at 160℃, and the treatment time is set to 2 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass and the eutectic solvent is recovered at the same time.
[0085] The test results showed that the EVA decomposition rate reached 99.1%, achieving efficient and green separation between the glass substrate and the EVA film, as detailed in Table 1.
[0086] Example 8:
[0087] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0088] (1) Preparation of eutectic solvent: Choline chloride (ChCl) and oxalic acid (Oxa) were added to a round-bottom flask at a molar ratio of 1:1 and stirred in an oil bath at 70°C for 2 h until a clear and transparent homogeneous liquid was formed, thus obtaining choline chloride-oxalic acid (ChCl-Oxa) eutectic solvent with a viscosity of 80~90 mPa·s at 25°C.
[0089] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely immersed in the liquid phase system; the ultrasonic treatment device and the heating temperature control system are turned on simultaneously, wherein: the ultrasonic power is set to 200 W, the fixed frequency is 40 kHz, the heating temperature is controlled at 150℃, and the treatment time is set to 2 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass and the eutectic solvent is recovered at the same time.
[0090] The test results showed that the EVA decomposition rate reached 91.6%, achieving efficient and green separation between the glass substrate and the EVA film, as detailed in Table 1.
[0091] Example 9:
[0092] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0093] (1) Preparation of eutectic solvent: Choline chloride (ChCl) and oxalic acid (Oxa) were added to a round-bottom flask at a molar ratio of 1:1 and stirred in an oil bath at 70°C for 2 h until a clear and transparent homogeneous liquid was formed. The eutectic solvent of choline chloride-oxalic acid (ChCl-Oxa) was prepared, with a viscosity of 80~90 mPa·s at 25°C.
[0094] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely wetted in the liquid phase system; the ultrasonic treatment device and the heating temperature control system are turned on at the same time, wherein: the ultrasonic power is set to 600 W, the fixed frequency is 40 kHz, the heating temperature is controlled at 150℃, and the treatment time is set to 2 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass and the eutectic solvent is recovered at the same time.
[0095] The test results showed that the EVA decomposition rate reached 99.3%, achieving efficient and green separation between the glass substrate and the EVA film, as detailed in Table 1.
[0096] Example 10:
[0097] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0098] (1) Preparation of eutectic solvent: Choline chloride (ChCl) and oxalic acid (Oxa) were added to a round-bottom flask at a molar ratio of 1:1 and stirred in an oil bath at 70°C for 2 h until a clear and transparent homogeneous liquid was formed. The eutectic solvent of choline chloride-oxalic acid (ChCl-Oxa) was prepared, with a viscosity of 80~90 mPa·s at 25°C.
[0099] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely wetted in the liquid phase system; the ultrasonic treatment device and the heating temperature control system are turned on simultaneously, wherein: the ultrasonic power is set to 400 W, the fixed frequency is 40 kHz, the heating temperature is controlled at 150℃, and the treatment time is set to 1 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass and the eutectic solvent is recovered at the same time.
[0100] The test results showed that the EVA decomposition rate reached 90.4%, achieving efficient and green separation between the glass substrate and the EVA film, as detailed in Table 1.
[0101] Example 11:
[0102] A method for catalytic depolymerization of waste EVA encapsulant film from photovoltaic modules using a eutectic solvent system includes the following steps:
[0103] (1) Preparation of eutectic solvent: Choline chloride (ChCl) and oxalic acid (Oxa) were added to a round-bottom flask at a molar ratio of 1:1 and stirred in an oil bath at 70 °C for 2 h until a clear and transparent homogeneous liquid was formed, thus obtaining the eutectic solvent of choline chloride-oxalic acid (ChCl-Oxa), which has a viscosity of 80~90 mPa·s at 25 °C.
[0104] (2) Overall depolymerization treatment of photovoltaic laminate: The photovoltaic laminated glass module (50 mm × 50 mm) containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely wetted in the liquid phase system; the ultrasonic treatment device and the heating temperature control system are turned on at the same time, wherein: the ultrasonic power is set to 400 W, the fixed frequency is 40 kHz, the heating temperature is controlled at 150 ℃, and the treatment time is set to 4 h; after the reaction is completed, the complete glass substrate is separated from the reaction medium, and subsequent cleaning treatment is carried out. The purity of the glass is tested to realize the regeneration of photovoltaic glass and the eutectic solvent is recovered at the same time.
[0105] The test results showed that the EVA decomposition rate reached 99.3%, achieving efficient and green separation between the glass substrate and the EVA film, as detailed in Table 1.
[0106] Table 1 compares the reaction conditions and results of Examples 1-11 and Comparative Examples 1-4, as shown in Table 1:
[0107] Table 1
[0108] The above description of the embodiments is only for the purpose of helping to understand the technical solution and core idea of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principle of the present invention, and these improvements and modifications also fall within the protection scope of the claims of the present invention.
Claims
1. A method for catalytic depolymerization of waste photovoltaic module EVA adhesive film by deep eutectic solvent system, characterized in that, Includes the following steps: (1) The hydrogen bond acceptor and the hydrogen bond donor are mixed in a molar ratio of 1:1 to 1:3 and stirred at 70℃ to 80℃ for 1 to 4 h until a homogeneous and transparent liquid is formed to obtain a eutectic solvent; the hydrogen bond acceptor is choline chloride and the hydrogen bond donor is selected from any one or more of oxalic acid, citric acid, malonic acid, ethylene glycol and glycerol. (2) The photovoltaic laminated glass module containing EVA adhesive layer is immersed in the eutectic solvent obtained in step (1) to ensure that the module is completely wetted in the liquid phase system; without cutting, crushing or pre-mechanically peeling off the EVA adhesive film from the photovoltaic laminate, ultrasonic and heating treatments are performed simultaneously; the ultrasonic treatment frequency is 40 kHz, the power is 200~600 W, the heating temperature is 120℃~160℃, and the treatment time is 1~4 h; after the treatment, the complete glass substrate is separated from the reaction medium, and after cleaning and drying, recycled glass is obtained, and the eutectic solvent is recovered at the same time.
2. The method of claim 1, wherein, The hydrogen bond donor in step (1) is oxalic acid, and the molar ratio of choline chloride to oxalic acid is 1:
1.
3. The method of claim 1, wherein, The ultrasonic power in step (2) is 400~500 W, the frequency is 40 kHz, the heating temperature is 140℃~150℃, and the processing time is 2 h.
4. The method of claim 1, wherein, In step (2), the photovoltaic laminated glass assembly is immersed as a whole in a eutectic solvent for depolymerization treatment.
5. The method of claim 1, wherein, The ultrasonic treatment and heating treatment described in step (2) are carried out simultaneously. The synergistic effect of the ultrasonic field and the thermal field promotes the penetration of the eutectic solvent into the EVA adhesive layer and promotes the depolymerization of the EVA crosslinking network.
6. The method of claim 1, wherein, The method for recovering the eutectic solvent in step (2) is as follows: the eutectic solvent system after the reaction is filtered to separate the solid residue, and the resulting filtrate is treated by rotary evaporation to recover the eutectic solvent for recycling.