A method for controlling the uncoiling collapse of thin-gauge cold-rolled high-strength steel base materials with strengths of 780 MPa and above.

By precisely controlling the microstructure and stress state of the strip head during the hot rolling stage, and by adopting thickness-graded dry head length and high-temperature slow cooling methods, the problem of cold rolling uncoiling and bending of thin-gauge high-strength steel was solved, thereby improving the yield and production efficiency.

CN123102750APending Publication Date: 2026-11-17МААНЬШАНЬ АЙРОН ЭНД СТИЛ КО ЛТД
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611333915.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot effectively solve the problem of flattened ends caused by high hardness and high residual stress in the cold rolling and uncoiling process of thin-gauge, high-tensile-strength cold-rolled high-strength steel base materials, resulting in low yield, waste of raw materials and low production efficiency.

Method used

By finely and collaboratively controlling the microstructure and residual stress state of the strip head during the hot rolling stage, and by using methods such as thickness-graded setting of dry head length, automated segmented shutdown of cooling water, and slow cooling of residual heat in high-temperature storage areas, the hardness and stress concentration of the strip head can be controlled.

Benefits of technology

It completely eliminates the defect of cold-rolled uncoiling with a flat head, improves the yield by 0.5%~1.5% and production efficiency, and realizes forward uncoiling without cutting off the head section.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102750A_ABST
    Figure CN123102750A_ABST
Patent Text Reader

Abstract

This invention discloses a control method for eliminating the head-down defect in cold-rolled high-strength steel base materials with a thickness of 780MPa and above. The method includes: setting the dry head length L according to the target thickness h of the strip; when the strip head passes through the coiling area, a signal is collected by a hot metal detector and tracked by a secondary system, controlling the closure of laminar flow water, pinch roll water, auxiliary coiling roll water, and mandrel internal cooling water, and reopening them after the strip head has traveled L meters; after uncoiling, the strip is transferred to a high-temperature storage area where the temperature is maintained at ≥150℃ using residual heat for slow cooling for 36-48 hours. This invention, through the coordinated control of "thickness-graded dry head + segmented sequential water shut-off + high-temperature slow cooling," reduces the Vickers hardness of the strip head to 212-230HV, completely eliminating the head-down defect after leveling and turning, allowing for smooth uncoiling without head cutting, significantly improving product yield and cold-rolling production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of hot-rolled strip steel production and cold-rolled base material processing technology. Specifically, it relates to a hot-rolling production control method for cold-rolled high-strength steel base materials with a tensile strength ≥780MPa, which is particularly suitable for eliminating the buckling defect that occurs in the cold rolling uncoiling process of thin-gauge 780MPa and above duplex high-strength steel base materials. Background Technology

[0002] This invention belongs to the technical field of hot-rolled strip steel production processes, specifically relating to a method for improving tensile strength. Hot rolling production control methods for high-strength cold-rolled steel base materials, especially suitable for eliminating thin gauges. The flattening defect that occurs in the cold rolling and uncoiling process of duplex high-strength steel base materials of grade A and above.

[0003] In cold-rolled high-strength steel (especially tensile strength) In the hot rolling production process of the base material of dual-phase high-strength steel (DP steel), the slab is heated in a heating furnace and then rolled into strip steel of specified specifications through a roughing mill and a seven-stand finishing mill. After the strip steel is cooled by a laminar flow cooling system, it is coiled into a steel coil by a coiler and then transported to the finished product warehouse by an uncoiling trolley to be cooled to room temperature.

[0004] Due to tensile strength High-strength cold-rolled steel requires extremely stringent final sheet shape quality. After hot-rolled coils come off the production line, they must undergo a leveling process to optimize their shape. In this leveling process, the coil is uncoiled and then re-coiled, causing the inner coil of the original hot-rolled coil to flip and become the outer coil of the leveled coil. This is because the inner coil of the original hot-rolled coil had a small diameter, high curvature, and was thin (thickness...) The elastic rebound and residual stress generated during the bending deformation of strip steel are extremely large; in addition, the hardness and strength of high-strength steel matrix are much higher than those of ordinary steel. When the flattened steel coil is transported to the cold rolling process for uncoiling and threading, the strip head (i.e., the original inner ring defect section) is prone to severe downward sagging, warping, or even bending under the combined action of huge internal residual stress and local high-hardness structure after it is released from the constraint of the coiler drum, forming a defect commonly known in the industry as "uncoiling head collapse" (the shape is as follows). Figure 1 (As shown). The "head-down" defect prevents the strip head from passing smoothly through the gaps between the oil scraper roll, pinch roll, and work roll of the cold rolling mill, causing the cold rolling mill to jam and pile up steel, making it impossible to establish a normal rolling state.

[0005] Currently, the most direct solution to the aforementioned "uncoiled head" defect in industrial production is manual head cutting, which involves directly removing approximately 2-10 meters of the defective section from the outer edge of the strip head. However, tensile strength... High-strength steel of this grade has high added value. Directly cutting off 2 to 10 meters of strip not only leads to a significant reduction in yield (an average reduction of about 0.5% to 1.5%), resulting in a huge waste of raw materials, but also seriously disrupts the production rhythm, causing a significant decrease in the production efficiency of the cold rolling continuous production line.

[0006] Existing technologies have explored some solutions to the problem of strip head abnormalities during the uncoiling or threading stages of cold rolling. For example, a Chinese patent discloses a threading method for cold-rolled strip steel, which assists threading by overlapping the tail of the previous coil with the head of the next coil while maintaining the uncoiling speed equal to the mill speed. This method is merely a mechanical threading aid, which can prevent the strip head from inserting into the roll gap, but it does not change the microstructure and mechanical state of the strip head itself, and cannot eliminate the tendency for the strip head to "collapse" due to the release of internal stress after it is released from its restraints.

[0007] A Chinese patent discloses a method for controlling the uncoiling of cold-rolled steel coils. This method uses a magnetic belt to detect signals and control the forward and reverse rotation of the uncoiler, the lifting and lowering of the guide plate, and the start and stop of the straightener to solve the problem of coil creasing caused by bundling. This solution mainly addresses localized creasing and accidental uncoiling caused by the external force of the bundling machinery. However, it is ineffective for the "drooping head" problem caused by the high strength of high-strength steel, its large winding curvature, and the concentration of internal stress after flattening and turning.

[0008] A Chinese patent discloses a method for controlling the warping of steel sheet heads, which resists warping after coiling by applying a reverse force to the strip steel before the rolling process. This method mainly addresses the macroscopic warping problem of conventional steel grades such as stainless steel, and does not consider tensile strength. The ultra-high hardness of the head caused by local phase transformation (precipitation of hard martensite / bainite phases) and strong undercooling in the laminar cooling and coiling regions of dual-phase high-strength steel cannot solve the "bent head" defect under specific microstructure gradients of high-strength steel.

[0009] Existing technologies have failed to precisely control the physical and mechanical state of the head of thin-gauge high-strength steel from the metallurgical root causes such as hot-rolled phase transformation microstructure regulation, cooling gradient elimination, and residual stress evolution.

[0010] In summary, the technical problem to be solved by the present invention is: addressing the limitations of existing thin-gauge (thickness) specifications. ),tensile strength After the high-grade cold-rolled high-strength steel base material is subjected to temper rolling and coil turning, in the cold rolling uncoiling process, the strip head is extremely prone to "sagging, bending" and other head drooping defects due to the synergistic effect of high hardness, high residual stress and large curvature, leading to the specific technical problems that 2~10m of the defective strip head section must be cut off, which further causes low yield, serious raw material waste and poor continuity of cold rolling production; the present invention provides a collaborative control method that requires no equipment modification and no cutting off of the defective strip head section, and implements "thickness-grading setting of dry head length + automatic tracking and time-sequential shutting off of cooling water + slow cooling with residual heat in high-temperature warehouse area" on the hot rolling line, which reduces the hardness of the strip head and eliminates stress concentration from the root of metallographic structure and residual stress, thereby completely eliminating thin-gauge grade high-strength steel cold rolling uncoiling head drooping defect. Contents of the Invention

[0011] The purpose of the present invention is to overcome the defects and deficiencies of the prior art, and to provide a control method for eliminating uncoiling head drooping of thin-gauge 780MPa and above grade cold-rolled high-strength steel base material. The present invention realizes fine coordinated regulation of the microstructure and residual stress state of the strip head in the hot rolling stage, fundamentally solves the sagging and head drooping defects of the strip head during cold rolling uncoiling after temper rolling and coil turning, enables smooth cold rolling uncoiling without cutting off the defective strip head section, and significantly improves the product yield and production efficiency.

[0012] The technical solution adopted by the present invention to solve its technical problems is: a control method for eliminating uncoiling head drooping of thin-gauge 780MPa and above grade cold-rolled high-strength steel base material, comprising the following steps: S1. Grading and setting the dry head length L of the strip coiling head according to the target thickness h of the strip; wherein the thickness h of the strip is ≤3.0mm, and the tensile strength is ≥780MPa; S2. After finishing rolling, the strip enters the coiling area, the strip head arrival signal is collected by the hot metal detector, and the secondary system accumulates the mileage according to the real-time running speed of the strip. When the strip head passes through the laminar cooling zone and the coiling equipment, the corresponding cooling water circuits are controlled to close, and after the strip head travels the set dry head length L meters, the cooling water circuits are restored to open, forming a dry head section with the set length L; S3. After coiling is completed, the steel coil is unloaded and transferred to a high-temperature warehouse area that uses the residual heat of the steel coil to maintain the ambient temperature for slow cooling treatment, and after the set slow cooling time, it is transferred to the conventional finished product warehouse area, and is subjected to temper rolling for subsequent cold rolling uncoiling.

[0013] Further, in step S1, the control rule for grading and setting the dry head length L of the strip coiling head according to the thickness h is: when the strip thickness satisfies 2.55mm<h≤3.0mm, the dry head length L of the strip coiling head is controlled to be 2~5m; when the strip thickness satisfies 2.25mm<h≤2.55mm, the dry head length L of the strip coiling head is controlled to be 5~8m; when the strip thickness satisfies 2.0mm≤h≤2.25mm, the dry head length L of the strip coiling head is controlled to be 8~10m.

[0014] Further, in step S2, the cooling water circuit includes laminar flow normally open water. The control process of laminar flow normally open water is as follows: the hot metal detector at the end of the finishing mill collects the strip head arrival signal, the secondary system tracks the strip travel distance in real time, and the laminar flow normally open water is turned off when the strip head passes the laminar flow normally open water nozzle; when the secondary system accumulates the strip travel distance to the set dry head length L meters, it sends a signal to the primary automation system to control the laminar flow normally open water to be turned on.

[0015] Furthermore, in step S2, the cooling water path also includes pinch roll cooling water. The control process of pinch roll cooling water is as follows: a hot metal detector in the coiling area is used to identify when the strip head reaches the pinch roll, and the pinch roll cooling water is turned off; the secondary system accumulates the mileage according to the strip running speed, and when the accumulated distance of the strip head passing the pinch roll reaches the set dry head length L meters, the primary automation system issues a command to restart the pinch roll cooling water.

[0016] Furthermore, in step S2, the cooling water path also includes cooling water for the coiling roller and cooling water inside the mandrel. The control process is as follows: a hot metal detector in the coiling area is used to identify when the strip head reaches the coiling roller and the coiling mandrel, and the cooling water for the coiling roller and the cooling water inside the mandrel are turned off respectively; the secondary system accumulates the mileage according to the strip running speed. When the cumulative distance that the strip head has passed over the coiling roller and the coiling mandrel reaches the set dry head length L meters, the primary automation system issues a command to restore the cooling water for the coiling roller and the cooling water inside the mandrel respectively.

[0017] Furthermore, in step S3, the ambient temperature of the high-temperature storage area is maintained at ≥150℃; when the steel coil is unloaded and put into storage, the internal temperature of the steel coil core is 350-450℃, and the outer surface temperature of the steel coil is 220-300℃; the slow cooling time is 36-48h.

[0018] Furthermore, in high-temperature storage areas, steel coils are placed in direct stacks for slow cooling, or insulated covers are placed over the stacked steel coils for slow cooling.

[0019] Furthermore, after the coordinated control of steps S1 to S3, the Vickers hardness of the head of the hot-rolled strip is 212-230 HV.

[0020] Furthermore, the high-strength steel base material is duplex high-strength steel (DP steel) with a tensile strength of 780-1180 MPa.

[0021] Compared with existing technologies, this invention has the following significant advantages: It breaks away from the traditional, extensive method of relying solely on "manually removing 2-10m defective strip ends" in the industry. Through a three-pronged synergistic control of "thickness-graded dry strip end + time-sequential segmented cooling water shutdown + high-temperature residual heat slow cooling," it precisely avoids the formation of hardened structures at the strip head under rapid cooling conditions, significantly reducing the yield strength and internal concentrated residual stress of the strip head. After leveling and rewinding, the strip head no longer experiences severe sagging and warping during cold rolling uncoiling, achieving a 100% uncoiling smoothness rate, significantly improving product yield (by approximately 0.5%-1.5%) and cold rolling continuous production efficiency. Furthermore, this invention sets the head length L according to the strip thickness (longer head section for thinner strips) and shuts off the constant-flow cooling water, pinch roll water, coiling roller water, and mandrel cooling water in the finishing and coiling areas, thus blocking the strong supercooling at the head. Combined with slow cooling for 36-48 hours using the residual heat of the coil (≥150℃ warehouse temperature) after warehousing, this promotes sufficient tempering and softening of the strip head. The Vickers hardness of the hot-rolled strip head is significantly reduced from approximately HV285 in conventional processes to HV212-230, establishing an excellent head strength and hardness gradient. Furthermore, this invention fully utilizes the existing hot metal detector (HMD), secondary system (L2) speed-mileage cumulative tracking, and primary automation system (L1) to achieve precise control of the head length L meters and accurate issuance of water circuit switching actions. This results in high control accuracy and strong repeatability, completely eliminating the randomness and lag of manual operation. This invention is based entirely on the optimization and control of process parameters and logic of existing hot rolling and coiling equipment, without requiring any new hardware modifications. At the same time, it cleverly utilizes the residual heat of the steel coil itself to maintain the temperature of the high-temperature storage area, making it green and low-carbon, and of great value for large-scale industrial application and promotion. Attached Figure Description

[0022] The present invention will be further described below with reference to the accompanying drawings and embodiments. In the accompanying drawings: Figure 1 This is a schematic diagram of the "bent head" defect that occurs in the cold rolling uncoiling process of thin-gauge cold-rolled high-strength steel base material after leveling and turning under conventional process (the diagram shows the bent head shape where the strip head falls down severely and bends after being released from the coiler constraint under conventional process, and cannot enter the cold rolling mill to establish rolling). Detailed Implementation

[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0024] To make the objectives, technical solutions and beneficial effects of the present invention clearer, the present invention is further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not intended to limit the present invention.

[0025] The present invention provides a control method for eliminating the head drooping during uncoiling of thin-gauge cold-rolled high-strength steel base materials of 780MPa and above, and its overall hot-rolling process flow includes: hot metal pretreatment deep desulfurization → converter top-bottom combined blowing → continuous casting → heating in a heating furnace → primary descaling → edge press machine → rough rolling → secondary descaling → seven-stand finish rolling → laminar cooling → coiling → coil unloading → slow cooling in high-temperature storage area → temper rolling → cold rolling uncoiling.

[0026] For cold-rolled high-strength steel base materials with target thickness h ≤ 3.0mm and tensile strength ≥ 780MPa (such as 780MPa, 980MPa, 1180MPa grade dual-phase high-strength DP steels, etc.), the core control measures of the present invention include the following three coordinated steps: Step S1: Set the dry head length L at the coiling head by thickness grading: Based on the target thickness h of the hot-rolled strip, set the dry head length L at the coiling head of the strip to realize the strength gradient control of the strip head. The specific setting rules are: (1) When the strip thickness satisfies 2.55mm < h ≤ 3.0mm, control the dry head length L at the coiling head of the strip to be 2~5m; (2) When the strip thickness satisfies 2.25mm < h ≤ 2.55mm, control the dry head length L at the coiling head of the strip to be 5~8m; (3) When the strip thickness satisfies 2.0mm ≤ h ≤ 2.25mm, control the dry head length L at the coiling head of the strip to be 8~10m Step S2: Automatically and sequentially shut off the cooling water circuits in the coiling zone: When the strip head passes through the coiling zone, through the closed-loop cooperation of on-site hardware and the automation system, the multiple paths of cooling water in the coiling zone are shut off for a distance of L meters: (1) Laminar constant-flow water control: A hot metal detector (HMD) at the finishing mill exit is used to collect the strip head arrival signal; the Level 2 system (L2) tracks the strip length, and performs mileage cumulative integration in combination with the real-time running speed of the strip; when the strip head passes through the laminar constant-flow water nozzles, the laminar constant-flow water is shut off; after the cumulative traveling distance reaches the set L meters, the L2 issues a signal to the Level 1 automation system (L1) to control the laminar constant-flow water to resume opening. (2) Pinch roll cooling water control: The HMD in the coiling zone identifies that the strip head arrives at the pinch roll, and controls the pinch roll cooling water to shut off; the L2 accumulates the mileage according to the strip running speed, and when the cumulative distance that the strip head has traveled past the pinch roll reaches L meters, it issues an instruction to the L1 to resume opening the pinch roll cooling water. (3) Wrapper roll cooling water and mandrel internal cooling water control: The HMD in the coiling zone respectively identifies that the strip head arrives at the wrapper roll and the coiling mandrel, and controls the wrapper roll cooling water and the mandrel internal cooling water to shut off; the L2 accumulates the mileage according to the strip running speed, and when the cumulative distances that the strip head has traveled past the wrapper roll and the coiling mandrel respectively reach L meters, the L1 issues an instruction to resume opening the wrapper roll cooling water and the mandrel internal cooling water.

[0027] Step S3: Stacking and slow cooling treatment in the high-temperature storage area: The coiled steel coil after coiling is transported by the coil unloading trolley to the high-temperature storage area. The ambient temperature of the storage area is maintained at ≥150℃ (no additional heating required) by utilizing the residual heat of the steel coil itself; when the steel coil enters the storage area, the internal temperature of the coil core is controlled at 350-450℃, and the outer surface temperature is controlled at 220-300℃; the steel coils are placed in direct stacking (or optionally covered with a heat preservation cover), the slow cooling time is controlled to be 36-48 hours according to the specification, and after the time expires, the steel coils are transferred to the conventional finished product storage area.

[0028] Specific examples and comparative examples are listed below to further illustrate the technical effect of the present invention: Example 1 This example is directed to a 780 MPa grade dual-phase high-strength steel base material with a target thickness of 3.0 mm.

[0029] (1) The target finishing temperature is set to 880℃, and the target coiling temperature is set to 550℃. According to the thickness specification (2.55 mm < h ≤ 3.0 mm), the dry head length L of the strip head is set to 2 m.

[0030] (2) The laminar constant-flow water is shut off when the strip head passes through, and is controlled by L1 to resume opening after the strip head has traveled a distance of 2 m.

[0031] (3) When the HMD in the coiling zone detects that the strip head reaches the pinch roll, the wrapper roll and the coiling mandrel, the pinch roll cooling water, the wrapper roll cooling water and the internal mandrel cooling water are respectively turned off; after the L2 mileage accumulation reaches 2m, the L1 controls all the above cooling water to return to normal.

[0032] (4) The steel coil is unloaded and transferred to the warehouse, the coil core temperature is 380~430℃, the ambient temperature in the high-temperature storage area is ≥150℃, and the coil is stacked for slow cooling for 48h.

[0033] (5) Inspection and uncoiling effect: After temper mill flipping, the coil is supplied to the cold rolling line, and the measured Vickers hardness of the strip head is HV212; the cold rolling uncoiling process is smooth without head drooping defect.

[0034] Embodiment 2 This embodiment is directed at a 780MPa grade dual-phase high-strength steel base material with a target thickness of 2.8mm.

[0035] (1) The target finish rolling temperature is set to 880℃, and the target coiling temperature is set to 520℃. According to the thickness specification, the dry head length L is set to 4m.

[0036] (2) 2. Pinch roll cooling water: The HMD detects that the strip head reaches the pinch roll, and the pinch roll cooling water is turned off; after the L2 mileage accumulation reaches 4m, the cooling water returns to normal; 3. Wrapper roll cooling water: The HMD detects that the strip head reaches the wrapper roll, and the wrapper roll cooling water is turned off; after the L2 mileage accumulation reaches 4m, the cooling water returns to normal; 4. Mandrel cooling water: The HMD detects that the strip head reaches the mandrel, and the internal mandrel cooling water is turned off; after the L2 mileage accumulation reaches 4m, the internal mandrel cooling water returns to normal.

[0037] (3) The coil core temperature during unloading and warehousing is 370~420℃, the warehouse temperature is ≥150℃, and the coil is stacked for slow cooling for 48h.

[0038] (4) Inspection and uncoiling effect: The measured Vickers hardness of the strip head is HV218; no head drooping defect occurs during cold rolling uncoiling.

[0039] Embodiment 3 This embodiment is directed at a 980MPa grade dual-phase high-strength steel base material with a target thickness of 2.5mm.

[0040] (1) The target finish rolling temperature is set to 900℃, and the target coiling temperature is set to 520℃. According to the thickness specification (2.25mm<h≤2.55mm), the dry head length L is set to 6m.

[0041] (2) Pinch roll cooling water: When HMD detects that the strip head reaches the pinch roll, the pinch roll cooling water is turned off; after the L2 accumulated mileage reaches 6m, the cooling water returns to normal; 3. Wrapper roll cooling water: When HMD detects that the strip head reaches the wrapper roll, the wrapper roll cooling water is turned off; after the L2 accumulated mileage reaches 6m, the cooling water returns to normal; 4. Mandrel cooling water: When HMD detects that the strip head reaches the mandrel, the internal cooling water of the mandrel is turned off; after the L2 accumulated mileage reaches 6m, the internal cooling water of the mandrel returns to normal.

[0042] (3) The temperature of the coil core when the coil is unloaded and put into storage is 360~410℃, the warehouse temperature is ≥150℃, and the coil is stack-cooled slowly for 40h.

[0043] (4) Inspection and uncoiling effect: The measured Vickers hardness of the strip head is HV221; no head drooping defect occurs during cold rolling uncoiling.

[0044] Fourth Embodiment This embodiment targets a 980MPa grade dual-phase high-strength steel base material with a target thickness of 2.3mm.

[0045] (1) The target finishing rolling temperature is set to 910℃, and the target coiling temperature is set to 550℃. According to the thickness specification (2.25mm<h≤2.55mm), the dry head length L is set to 7m.

[0046] (2) Pinch roll cooling water: When HMD detects that the strip head reaches the pinch roll, the pinch roll cooling water is turned off; after the L2 accumulated mileage reaches 7m, the cooling water returns to normal; Wrapper roll cooling water: When HMD detects that the strip head reaches the wrapper roll, the wrapper roll cooling water is turned off; after the L2 accumulated mileage reaches 7m, the cooling water returns to normal; Mandrel cooling water: When HMD detects that the strip head reaches the mandrel, the internal cooling water of the mandrel is turned off; after the L2 accumulated mileage reaches 7m, the internal cooling water of the mandrel returns to normal.

[0047] (3) The temperature of the coil core when the coil is unloaded and put into storage is 360~410℃, the warehouse temperature is ≥150℃, and the coil is stack-cooled slowly for 40h.

[0048] (4) Inspection and uncoiling effect: The measured Vickers hardness of the strip head is HV224; no head drooping defect occurs during cold rolling uncoiling.

[0049] Fifth Embodiment This embodiment targets a 1180MPa grade ultra-high-strength dual-phase steel base material with a target thickness of 2.4mm.

[0050] (1) The target finishing rolling temperature is set to 910℃, and the target coiling temperature is set to 520℃. According to the thickness specification, the dry head length L is set to 7m.

[0051] (2) Laminar flow normally open water: The laminar flow normally open water is turned off when the strip head passes by, and is turned on by L1 control after the strip head has traveled 7m; Pinch roll cooling water: HMD detects that the strip head has reached the pinch roll, and the pinch roll cooling water is turned off; after the L2 mileage reaches 7m, the cooling water returns to normal; Auxiliary roll cooling water: HMD detects that the strip head has reached the auxiliary roll, and the auxiliary roll cooling water is turned off; after the L2 mileage reaches 7m, the cooling water returns to normal; Mandrel cooling water: HMD detects that the strip head has reached the mandrel, and the cooling water inside the mandrel is turned off; after the L2 mileage reaches 7m, the cooling water inside the mandrel returns to normal.

[0052] (3) The temperature of the core when unloading and putting it into the warehouse is 350~400℃, the warehouse temperature is ≥150℃, and the core is stacked and cooled slowly for 36 hours.

[0053] (4) Inspection and uncoiling effect: The measured Vickers hardness of the strip head is HV226; there is no drooping head defect in the cold rolled uncoiling.

[0054] Example 6 This embodiment is for 1180MPa level ultra-high strength duplex steel base material with a target thickness of 2.2mm.

[0055] (1) Set the final rolling target temperature to 930℃ and the coiling target temperature to 550℃. Based on the thickness specification (2.0mm≤h≤2.25mm), set the dry end length L=8m.

[0056] (2) Pinch roll cooling water: When the HMD detection belt reaches the pinch roll, the pinch roll cooling water is turned off; after the L2 mileage reaches 8m, the cooling water returns to normal; Auxiliary roll cooling water: When the HMD detection belt reaches the auxiliary roll, the auxiliary roll cooling water is turned off; after the L2 mileage reaches 8m, the cooling water returns to normal; Mandrel cooling water: When the HMD detection belt reaches the mandrel, the mandrel internal cooling water is turned off; after the L2 mileage reaches 8m, the mandrel internal cooling water returns to normal.

[0057] (3) The temperature of the core when unloading and putting it into the warehouse is 350~400℃, the warehouse temperature is ≥150℃, and the core is stacked and cooled slowly for 36 hours.

[0058] (4) Inspection and uncoiling effect: The measured Vickers hardness of the strip head is HV228; there is no drooping head defect in the cold rolled uncoiling.

[0059] Example 7 This embodiment is for 1180MPa level ultra-high strength duplex steel base material with a target thickness of 2.0mm.

[0060] (1) Set the final rolling target temperature to 930℃ and the winding target temperature to 520℃. Based on the thickness specification, set the dry end length L=10m.

[0061] (2) Pinch roll cooling water: When the HMD detection belt reaches the pinch roll, the pinch roll cooling water is turned off; after the L2 mileage reaches 10m, the cooling water returns to normal; Auxiliary roll cooling water: When the HMD detection belt reaches the auxiliary roll, the auxiliary roll cooling water is turned off; after the L2 mileage reaches 10m, the cooling water returns to normal; Mandrel cooling water: When the HMD detection belt reaches the mandrel, the mandrel internal cooling water is turned off; after the L2 mileage reaches 10m, the mandrel internal cooling water returns to normal.

[0062] (3) The temperature of the core when unloading and putting it into the warehouse is 350~400℃, the warehouse temperature is ≥150℃, and the core is stacked and cooled slowly for 36 hours.

[0063] (4) Inspection and uncoiling effect: The measured Vickers hardness of the strip head is HV230; there is no drooping head defect in the cold rolled uncoiling.

[0064] Comparative example (conventional process) This comparative example focuses on 1180MPa-grade ultra-high strength duplex steel base material with a target thickness of 2.0mm, using conventional control processes.

[0065] (1) The final rolling target temperature is 930℃, and the coiling target temperature is 550℃. The dry end length is set to 0m (the dry end control process is not enabled).

[0066] (2) The laminar flow normally open water is kept on and not closed throughout the entire process; the pinch roll cooling water, the auxiliary roll cooling water and the mandrel internal cooling water are kept on and not closed throughout the entire process.

[0067] (3) After the steel coils are unloaded, they are placed directly in the conventional finished product warehouse for natural cooling, without the requirement for high-temperature slow cooling.

[0068] (4) Inspection and Uncoiling Effect: After leveling and flipping, the strip is supplied to the cold rolling line. The measured Vickers hardness of the strip head is as high as HV285. During cold rolling uncoiling, the strip head sags and bends severely after being released from the constraint, exhibiting a significant "uncoiling head collapse" defect (the shape is as follows). Figure 1 As shown in the figure, rolling cannot be established normally, and the outer ring 2-10m defect section must be removed before it can barely be put into operation.

[0069] Note: 0m indicates that the head dryer control process is not enabled.

[0070] Table 1 lists the technical parameters and test results of Examples 1-7 and the comparative examples: As can be seen from Table 1 and the comparison of experimental data: In the comparative example, when using conventional processes, due to the lack of control over the dry end and the use of water cooling throughout the process, the strip head underwent strong overcooling hardening, generating a high-hardness martensitic phase, resulting in a Vickers hardness of up to HV285 at the strip head; after leveling and rewinding, under the influence of huge internal concentrated residual stress and high hardness, severe head collapse occurred during uncoiling. Figure 1 In embodiments 1-7, which employ the control method of this invention, the Vickers hardness of the strip head is successfully controlled within the range of HV212-230 by controlling the dry head length L through thickness grading, segmented shut-off of cooling water, and high-temperature slow cooling. This effectively reduces the yield strength of the strip head and releases residual stress. All the flattened steel coils in these embodiments show no protruding head defects during cold rolling uncoiling, achieving 100% forward uncoiling without strip head removal, significantly improving production efficiency and product yield.

[0071] It should be understood that those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.

Claims

1. A method for eliminating thin specifications The method for controlling the uncoiling head collapse of cold-rolled high-strength steel base materials of grades A and B is characterized by, Includes the following steps: S1, Based on the target thickness of the strip steel Grade setting of the dry head length of the strip coiling head Wherein, the thickness of the strip steel ,tensile strength S2. After finishing rolling, the strip enters the coiling area. A hot metal detector collects the strip head arrival signal, and the secondary system accumulates the mileage based on the real-time running speed of the strip. When the strip head passes through the laminar flow cooling zone and the coiling equipment, the corresponding cooling water circuits are shut off. The system continues operation until the strip head has traveled the set dry length. After a certain distance, the cooling water circuit is reopened, forming the set length. The dry section; S3, after the steel coil is uncoiled after coiling, it is transferred to a high-temperature warehouse area that uses the residual heat of the steel coil to maintain the ambient temperature for slow cooling treatment. After the set slow cooling time, it is transferred to the regular finished product warehouse area, and after being leveled, it is ready for cold rolling and uncoiling.

2. The method for eliminating thin specifications according to claim 1 The method for controlling the uncoiling head collapse of cold-rolled high-strength steel base materials of grades A and B is characterized by, In step S1, according to thickness Grade setting of strip coiling head dry length The control rules are as follows: When the strip thickness is At the same time, control the length of the strip coiling head. for ; When the strip thickness is At the same time, control the length of the strip coiling head. for ; When the strip thickness is At the same time, control the length of the strip coiling head. for .

3. The method for eliminating thin specifications according to claim 1 or 2 The method for controlling the uncoiling head collapse of cold-rolled high-strength steel base materials of grades A and B is characterized by, In step S2, the cooling water circuit includes laminar flow normally open water. The control process of laminar flow normally open water is as follows: the hot metal detector at the end of the finishing mill is used to collect the strip head arrival signal, the secondary system tracks the strip travel distance in real time, and the laminar flow normally open water is turned off when the strip head passes the laminar flow normally open water nozzle. When the cumulative strip travel distance of the secondary system reaches the set dry end length After a while, a signal is sent to the primary automation system to control the laminar flow of constantly boiling water.

4. The method for eliminating thin specifications according to claim 3 The method for controlling the uncoiling head collapse of cold-rolled high-strength steel base materials of grades A and B is characterized by, In step S2, the cooling water path also includes pinch roll cooling water. The control process for the pinch roll cooling water is as follows: a hot metal detector in the coiling area identifies when the strip head reaches the pinch roll, and controls the pinch roll cooling water to be turned off; the secondary system accumulates mileage based on the strip running speed, and when the accumulated distance of the strip head past the pinch roll reaches the set dry head length... After a certain distance, the primary automation system issues a command to resume the cooling water supply to the pinch rollers.

5. The method for eliminating thin specifications according to claim 4 The method for controlling the uncoiling head collapse of cold-rolled high-strength steel base materials of grades A and B is characterized by, In step S2, the cooling water circuit also includes cooling water for the coiling roller and cooling water inside the mandrel. The control process is as follows: a hot metal detector in the coiling area identifies when the strip head reaches the coiling roller and the coiling mandrel, and controls the cooling water for the coiling roller and the cooling water inside the mandrel to be shut off respectively; the secondary system accumulates mileage according to the strip running speed, and when the cumulative distance that the strip head has traveled over the coiling roller and the coiling mandrel reaches the set dry head length... After a certain distance, the primary automation system issues instructions to restore the cooling water for the auxiliary winding roller and the internal cooling water for the mandrel.

6. The method for eliminating thin specifications according to claim 1 The method for controlling the uncoiling head collapse of cold-rolled high-strength steel base materials of grades A and B is characterized by, In step S3, the ambient temperature of the high-temperature storage area is maintained at... When the steel coil is unwound and stored, the internal temperature of the coil core is: The outer surface temperature of the steel coil is The slow cooling time is .

7. The method for eliminating thin specifications according to claim 6 The method for controlling the uncoiling head collapse of cold-rolled high-strength steel base materials of grades A and B is characterized by, In high-temperature storage areas, steel coils are cooled slowly by directly stacking them or by covering the stacked steel coils with an insulation cover.

8. The method for eliminating thin specifications according to any one of claims 1 to 7 The method for controlling the uncoiling head collapse of cold-rolled high-strength steel base materials of grades A and B is characterized by, After the coordinated control of steps S1 to S3, the Vickers hardness of the head of the hot-rolled strip is [value missing]. .

9. The method for eliminating thin specifications according to any one of claims 1 to 7 The method for controlling the uncoiling head collapse of cold-rolled high-strength steel base materials of grades A and B is characterized by, The high-strength steel base material has a tensile strength of... Dual-phase high-strength steel (DP steel) of a certain grade.