A method for rapid forming of 60NiTi alloy plates with heat-shielded cladding and rolling

By combining heat treatment and forging with a sandwich structure design, the precipitation of Ni4Ti3 phase was controlled, which solved the cracking problem of 60NiTi alloy during rolling, achieving efficient and uniform alloy forming and improving the alloy's formability and performance.

CN123102783APending Publication Date: 2026-11-17HEBEI DAHE MATERIAL TECH CO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611211042.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

During the rolling process, the Ni4Ti3 phase in 60NiTi alloy rapidly precipitates, leading to cracking and making it difficult to achieve rapid forming. Existing methods have failed to effectively control phase transformation and reduce the risk of cracking.

Method used

By employing a combination of heat treatment and forging, a sandwich structure and a reasonable rolling process were designed. By controlling the precipitation of the Ni4Ti3 phase, and combining the sandwich structure and rolling parameters, the metal flow behavior was regulated to achieve rapid forming of 60NiTi alloy.

Benefits of technology

It significantly reduces the crack sensitivity of the alloy, improves the formability and product yield, and obtains 60NiTi alloy plates with uniform structure and excellent performance, with significantly improved tensile strength and hardness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102783A_ABST
    Figure CN123102783A_ABST
Patent Text Reader

Abstract

This invention discloses a hot-shielded cladding rolling method for rapid forming of 60NiTi alloy sheets. Specifically, a 60NiTi alloy slab is placed between two stainless steel sheets, and the two sheets are welded together using a stainless steel support to obtain a sandwich-structured 60NiTi alloy slab. Based on the millisecond-level rapid precipitation characteristics of the Ni4Ti3 strengthening phase in the alloy and the metal flow behavior during high-temperature rolling, the rolling process, including rolling temperature, rolling rate, and rolling pressure, is rationally designed and rolled. After rolling, the stainless steel support is cut off to obtain the 60NiTi alloy sheet. This invention solves the problem of transverse and longitudinal cracking in rolled sheets caused by the rapid precipitation of the strengthening phase in the 60NiTi alloy, significantly improving the yield of 60NiTi alloy and achieving the preparation of 60NiTi alloy sheets with uniform microstructure and excellent comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal forming technology, specifically relating to a heat-shielded cladding rolling method for rapid forming of 60NiTi alloy plates. Background Technology

[0002] 60NiTi alloy possesses advantages such as non-magnetic properties, strong corrosion resistance, and low density, overcoming the shortcomings of traditional aerospace bearing alloys, such as poor corrosion resistance and heavy weight. It meets the performance requirements of high thrust-to-weight ratio engines and is considered an ideal material for manufacturing aerospace bearings. The 60NiTi alloy is mainly composed of a metastable, Ni3Ti-stabilized, and B2-NiTi matrix. However, the Ni4Ti3 phase, as the main strengthening phase, exhibits a precipitation mechanism that differs significantly from traditional materials such as nickel-based superalloys and titanium alloys. The Ni4Ti3 phase precipitates rapidly and readily becomes a hard phase during rolling, deteriorating the alloy's rapid formability. Therefore, controlling the precipitation of the Ni4Ti3 phase is extremely difficult. CN 114101554 A discloses a forging method for 60NiTi alloy, which adopts a five-step method of "surface coating with anti-oxidation coating - solution treatment - heating and holding - axial upsetting - radial deformation" to solve the problem of intrinsic brittleness of the 60NiTi(X) alloy matrix and realize forging. It solves the problems of high difficulty and easy cracking in multi-directional forging processing. However, the method has strict requirements on strain rate. At the same time, the method does not solve the problem of rapid precipitation of Ni4Ti3 phase, which leads to transverse cracks, longitudinal cracks and other cracks during rolling, making the preparation cost of 60NiTi alloy parts high.

[0003] Clad rolling, as a plastic processing technology combining interlayer deformation and heat treatment, has advantages such as suppressing surface defects, reducing single-stage deformation resistance, and rapid heat dissipation. CN 117299793 A discloses a cladding rolling method for TiAl alloy plates. This invention effectively suppresses hydrogen and oxygen absorption and rapid heat dissipation during plate rolling by rationally designing the billet thickness, number of layers, and other material and pass deformation amounts, rolling temperature, and rolling rate, thus avoiding problems such as plate deformation and cracking, ensuring the formability and mechanical properties of the plate, and ultimately obtaining high-quality TiAl alloy plates. However, there are few reports on cladding rolling forming methods for 60NiTi alloys. Clad rolling provides a new approach to suppress the rapid precipitation of the Ni4Ti3 phase in 60NiTi alloys during rolling, enabling rapid rolling forming of 60NiTi alloys. Summary of the Invention

[0004] To address the challenges of complex phase microstructure and temperature-sensitive precipitation in 60NiTi alloys, which hinders their plastic forming, this invention aims to provide a hot-shielded cladding rolling method for rapid forming of 60NiTi alloy sheets. This method reduces the content of the metastable Ni4Ti3 phase through heat treatment, transforming it into the stable Ni3Ti phase. Based on the precipitation phase transformation temperature and melting point of the 60NiTi alloy, the rolling process, including initial / final rolling temperatures, reduction, and rolling passes, is rationally designed. Furthermore, a sandwich structure is used to regulate metal flow behavior during alloy forming, solving problems such as millisecond-level rapid precipitation of the Ni4Ti3 phase and uneven grain deformation, thus achieving rapid hot rolling forming of 60NiTi alloys.

[0005] To achieve the above objectives, the technical solution of the present invention is as follows: A method for rapid forming of 60NiTi alloy plates using heat-shielded cladding and lamination rolling includes the following steps: (1) Ingot preparation: 60NiTi alloy ingots were prepared by vacuum induction melting.

[0006] (2) Forging billet preparation: The 60NiTi alloy ingot is forged by isothermal forging process to obtain 60NiTi alloy forging billet.

[0007] (3) Slab preparation: 60NiTi alloy forging billet is obtained by wire cutting of 60NiTi alloy billet with electric spark.

[0008] (4) Sandwich structure design: Place the 60NiTi alloy slab between two stainless steel plates and weld the two stainless steel plates into a whole using a stainless steel bracket to obtain a sandwich structure 60NiTi alloy slab.

[0009] (5) Rolling: The sandwich structure 60NiTi slab described in step (4) is placed in a box furnace, heated to 950~1100℃, held for 2~6 h and then hot rolled. After each rolling pass, it is returned to the furnace for a period of time to be held. After the rolling process is completed, it is placed in a box furnace for stress relief annealing.

[0010] (6) Post-rolling treatment: The stainless steel bracket is cut off by wire cutting to obtain 60NiTi alloy plate.

[0011] Furthermore, the composition of the 60NiTi alloy of the present invention is C≤300 ppm, O≤500 ppm, N≤100ppm, 39 at.%≤Ti≤41 at.%, Ni: balance.

[0012] Further, the pre-forging heating regime of the 60NiTi alloy ingot in step (2) of the present invention is as follows: the heating rate from room temperature to 500 ℃ is 6~10 ℃ / min, and the furnace temperature is held for 10~20 min after reaching 500 ℃; the heating rate from 500 ℃ to 900 ℃ is 3~4 ℃ / min, and the furnace temperature is held for 20~30 min after reaching 900 ℃; the heating rate from 900 ℃ to 950~1100 ℃ is 2~3 ℃ / min, and the furnace temperature is held for 2~6 h after reaching 950~1100 ℃.

[0013] Furthermore, in step (2) of the present invention, the isothermal forging temperature is 950~1100℃, the deformation amount is 20~60%, and the deformation rate is 0.01~1 s. -1 After forging, the material is immediately placed in a box furnace and held at 950~1150℃ for 2~6 hours, then cooled with the furnace.

[0014] Furthermore, in the sandwich structure described in step (4) of the present invention, 1 to 4 60NiTi alloy slabs can be placed, and an isolation layer composed of high-temperature insulation cotton and ceramic powder in a thickness ratio of 3 to 5:1 is placed between the 60NiTi alloy slabs and between the 60NiTi alloy slabs and stainless steel; the thickness of the isolation layer is 1 to 2 mm.

[0015] Furthermore, in step (4), the stainless steel plate is coated with yttrium oxide or other anti-oxidation coatings on both sides.

[0016] Further, the rolling forming process in step (2) of the present invention is as follows: when the deformation per pass is 10%~20%, the rolling speed is 100 mm / s~400 mm / s; when the deformation per pass is 20%~40%, the rolling speed is 50 mm / s~200 mm / s; after each pass of rolling, the material is immediately returned to the furnace for 20~150 min to maintain its temperature, and then the above rolling process is repeated until the total deformation reaches the predetermined value. After rolling, the material is placed in a box furnace and held at 1000 ℃~1150 ℃ for 1 h~6 h, then cooled with the furnace for stress relief treatment.

[0017] The inventive principle of this invention is as follows: Currently, the main forming methods for 60NiTi alloy are near-net-shape forming using powder metallurgy and vacuum induction melting combined with forging. However, forging produces plates with poor parallelism and surface quality, and uneven microstructure. Furthermore, the 60NiTi alloy's Ni:Ti ratio is 55:45 (at.%), meaning it cannot achieve complete solid solution at high temperatures, inevitably resulting in the presence of a second phase. The nano-Ni4Ti3 phase precipitates in milliseconds under rapid cooling conditions, severely deteriorating the alloy's plasticity and leading to surface cracking when in contact with forging anvils or rolls. However, there are few reports on plastic forming processes developed based on the precipitation characteristics of 60NiTi alloy, hindering the development and application of 60NiTi alloys, which possess comprehensive advantages such as non-magnetic properties, low density, high wear resistance, and high corrosion resistance.

[0018] This invention achieves control over the billet opening and precipitated phase state of 60NiTi alloy through a combination of forging and heat treatment, providing sufficient recrystallization nuclei for rolling and thus reducing the risk of rolling cracks. Based on the precipitation characteristics of the Ni4Ti3 phase, a sandwich structure 60NiTi plate is rationally designed to improve the transformation degree of Ni3Ti phase to Ni4Ti3 phase and delay the precipitation rate of Ni4Ti3 phase. Furthermore, the rolling process, including rolling rate, rolling passes, and reduction, is adjusted to avoid defects such as transverse cracks, longitudinal cracks, and alligator cracks during the rapid forming of difficult-to-deform 60NiTi alloy, resulting in 60NiTi alloy plates with uniform grain size and excellent overall performance.

[0019] The present invention has the following beneficial effects: (1) In the forging process, the present invention adopts a heat treatment-brushing process synergistic method, appropriately introduces dislocations to provide recrystallization nuclei for subsequent rolling forming, and at the same time uses heat treatment to optimize the existence state of dislocations and precipitates, which greatly reduces the crack sensitivity of 60NiTi alloy.

[0020] (2) The stepped heating system described in this invention is specifically designed based on the characteristics of 60NiTi alloy, which has poor thermal conductivity and is sensitive to microstructure transformation temperature. By using a heating rate of 6~10℃ / min from room temperature to 500℃, thermal stress cracks caused by excessive internal and external temperature differences due to rapid heating in the low-temperature stage can be avoided. Setting up heat preservation platforms at 500℃ and 900℃ can homogenize the internal temperature of the ingot and promote the full removal of harmful gases, providing billets with good microstructure uniformity for subsequent high-temperature forging. Using a slow heating rate of 2-3℃ / min in the high-temperature stage is conducive to the gradual and controllable re-dissolution of precipitates such as Ni4Ti3, avoiding the risk of phase transformation runaway and cracking caused by rapid heating. Through the synergistic effect of this system, the success rate of 60NiTi alloy ingot blanking can be significantly improved, laying the foundation for obtaining uniform microstructure and crack-free forging blanks in the future.

[0021] (3) The sandwich structure of 60NiTi plate can avoid direct contact between the roll and the alloy, avoid the rapid precipitation of nano Ni4Ti3 phase, and reduce the temperature change of the alloy during rolling, thereby improving the rolling forming ability of 60NiTi alloy and improving the product yield.

[0022] (4) The present invention can reasonably design the thickness and number of layers of 60NiTi alloy plates based on product requirements, and can prepare multiple alloy plates in one process, which can effectively improve the production efficiency of 60NiTi alloy and reduce costs.

[0023] In summary, the process of this invention can precisely control the microstructure and rolling temperature changes of 60NiTi alloy through forging and sandwich structure design to reduce the alloy's temperature sensitivity. Based on this, controlling the rolling forming process improves the alloy's flow behavior, resulting in 60NiTi alloy plates with uniform microstructure and excellent performance. The tensile strength can reach 900~1200 MPa, and the Rockwell hardness value is as high as 56~64 HRC. Attached Figure Description

[0024] Figure 1 : Schematic diagram of the 60NiTi alloy sandwich structure described in this invention.

[0025] Figure 2 Microstructure of the 60NiTi alloy after rolling as described in Example 1.

[0026] Figure 3 Microstructure of the 60NiTi alloy after rolling as described in Example 2.

[0027] Figure 4 Microstructure of the 60NiTi alloy after rolling as described in Example 3.

[0028] Figure 5 Microstructure of the 60NiTi alloy after rolling as described in Comparative Example 1.

[0029] Figure 6 Microstructure of the 60NiTi alloy after rolling as described in Comparative Example 2. Detailed Implementation

[0030] The present invention will now be described in detail with reference to specific embodiments. The following examples will help those skilled in the art to further understand the present invention, but do not limit the invention in any way.

[0031] The 60NiTi alloy involved in this invention has the following composition by mass percentage: Ti: 39~41%, with the balance being Ni. Example 1

[0032] A method for rapid forming of 60NiTi alloy plates using heat-shielded cladding and lamination rolling includes the following steps: (1) Ingot preparation: 60NiTi alloy ingots were prepared by vacuum induction melting.

[0033] (2) Forging billet preparation: The heating rate of the ingot from room temperature to 500℃ was 8℃ / min, and the furnace temperature was held for 10 min after reaching 500℃; the heating rate from 500℃ to 900℃ was 4℃ / min, and the furnace temperature was held for 20 min after reaching 900℃; the heating rate from 900℃ to 950℃ was controlled at 3℃ / min, and the furnace temperature was held for 6 h after reaching 950℃. The 60NiTi alloy was forged using isothermal forging process, with an isothermal forging temperature of 950℃, a deformation amount of 20%, and a deformation rate of 1s. -1 60NiTi alloy slabs were obtained. After forging, the slabs were immediately placed in a box furnace and held at 950℃ for 2 hours, then cooled in the furnace.

[0034] (3) Slab preparation: The 60NiTi alloy slab is cut into plates of 300 mm (length) × 200 mm (width) × 20 mm (thickness) using wire electrical discharge machining.

[0035] (4) Sandwich structure design: such as Figure 1 As shown, a 60NiTi alloy slab is placed between two stainless steel plates coated with yttrium oxide. A 1mm thick insulating layer composed of high-temperature insulation cotton and ceramic powder in a thickness ratio of 3:1 is placed between the stainless steel plates and the 60NiTi alloy. The two stainless steel plates are welded together as a whole using a stainless steel bracket to obtain a sandwich structure 60NiTi alloy slab.

[0036] (5) Rolling and forming: The sandwich structure 60NiTi alloy slab obtained in step (4) is placed in a box furnace, heated to 1000℃ and held for 2 h. After the holding period, it is immediately hot rolled. The rolling speed of the first pass is 400 mm / s and the rolling deformation is 10%. After the rolling is completed, it is immediately returned to the furnace for holding for 20 min. The rolling speed of the second pass is 200 mm / s and the rolling deformation is 30%. After the rolling is completed, it is placed in a box furnace and held at 1000℃ for 1 h. It is then cooled with the furnace and subjected to stress relief treatment.

[0037] (6) Post-rolling treatment: Cut the stainless steel support in step (4) with wire cutting to remove the stainless steel plate and the isolation layer, and obtain the 60NiTi alloy plate.

[0038] The 60NiTi alloy sheet obtained in this embodiment has a smooth surface, no cracks, and no obvious oxidation. The microstructure of the sheet after rolling is as follows: Figure 2 As shown; by Figure 2It can be seen that its microstructure is mainly composed of grains elongated along the rolling direction and Ni3Ti phase, and the microstructure is relatively uniformly distributed.

[0039] The 60NiTi alloy plate obtained in this embodiment has a hardness of up to 56 HRC and a tensile strength of up to 900 MPa. Example 2

[0040] A method for rapid forming of 60NiTi alloy plates using heat-shielded cladding and lamination rolling includes the following steps: (1) Ingot preparation: 60NiTi alloy ingots were prepared by vacuum induction melting.

[0041] (2) Slab preparation: The heating rate of the ingot from room temperature to 500 ℃ was 8 ℃ / min, and the furnace temperature was held for 20 min after reaching 500 ℃; the heating rate from 500 ℃ to 900 ℃ was 2 ℃ / min, and the furnace temperature was held for 30 min after reaching 900 ℃; the heating rate from 900 ℃ to 1100 ℃ was controlled at 2 ℃ / min, and the furnace temperature was held for 2 h after reaching 1100 ℃. The 60NiTi alloy was forged using isothermal forging process, with an isothermal forging temperature of 1100 ℃, a deformation amount of 60%, and a deformation rate of 0.01 s. -1 60NiTi alloy slabs were obtained. After forging, the slabs were immediately placed in a box furnace and held at 1150℃ for 6 hours, followed by furnace cooling.

[0042] (3) Slab preparation: The 60NiTi alloy slab is cut into plates of 300 mm (length) × 200 mm (width) × 20 mm (thickness) using wire electrical discharge machining.

[0043] (4) Sandwich structure design: such as Figure 1 As shown, four 60NiTi alloy slabs are placed between two stainless steel plates coated with yttrium oxide. A 2 mm thick insulating layer composed of high-temperature insulation cotton and ceramic powder in a thickness ratio of 5:1 is placed between the stainless steel plates and the 60NiTi alloy, and between the 60NiTi alloy slabs.

[0044] (5) Rolling and forming: The sandwich structure 60NiTi alloy slab obtained in step (4) is placed in a box furnace, heated to 1100℃ and held for 3 h. After the holding period, it is immediately hot rolled. The rolling speed of the first pass is 100 mm / s and the rolling deformation is 10%. After the rolling is completed, it is immediately returned to the furnace for holding for 150 min. The rolling speed of the second pass is 50 mm / s and the rolling deformation is 20%. After the rolling is completed, it is placed in a box furnace and held at 1150℃ for 6 h. It is then cooled with the furnace and subjected to stress relief treatment.

[0045] (6) Post-rolling treatment: Cut the stainless steel support in step (4) with wire cutting to remove the stainless steel plate and the isolation layer, and obtain the 60NiTi alloy plate.

[0046] The 60NiTi alloy sheet obtained in this embodiment has a smooth surface, no cracks, and no obvious oxidation. The microstructure of the sheet after rolling is as follows: Figure 3 As shown; by Figure 3 It can be seen that its microstructure exhibits uniform equiaxed crystals, with the Ni3Ti phase mainly distributed along the grain boundaries, and the microstructure has good uniformity.

[0047] The 60NiTi alloy plate obtained in this embodiment has a hardness of up to 61 HRC and a tensile strength of up to 1124 MPa. Example 3

[0048] A method for rapid forming of 60NiTi alloy plates using heat-shielded cladding and lamination rolling includes the following steps: (1) Ingot preparation: 60NiTi alloy ingots were prepared by vacuum induction melting.

[0049] (2) Forging billet preparation: The heating rate of the ingot from room temperature to 500 ℃ was 8 ℃ / min, and the furnace temperature was held for 20 min after reaching 500 ℃; the heating rate from 500 ℃ to 900 ℃ was 2 ℃ / min, and the furnace temperature was held for 30 min after reaching 900 ℃; the heating rate from 900 ℃ to 1050 ℃ was controlled at 2 ℃ / min, and the furnace temperature was held for 4 h after reaching 1050 ℃. The 60NiTi alloy was forged using isothermal forging process, with an isothermal forging temperature of 1050 ℃, a deformation amount of 40%, and a deformation rate of 0.01 s. -1 60NiTi alloy slabs were obtained. After forging, the slabs were immediately placed in a box furnace and held at 1150℃ for 6 hours, followed by furnace cooling.

[0050] (3) Slab preparation: The 60NiTi alloy slab is cut into plates of 300 mm (length) × 200 mm (width) × 20 mm (thickness) using wire electrical discharge machining.

[0051] (4) Sandwich structure design: such as Figure 1 As shown, two 60NiTi alloy slabs are placed between two stainless steel plates coated with yttrium oxide. A 1.4 mm thick insulating layer composed of high-temperature insulation cotton and ceramic powder in a thickness ratio of 4:1 is placed between the stainless steel plates and the 60NiTi alloy, and between the 60NiTi alloy slabs.

[0052] (5) Rolling and forming: The sandwich structure 60NiTi alloy slab obtained in step (4) is placed in a box furnace, heated to 1100℃ and held for 3 h. After the holding period, it is immediately hot rolled. The rolling speed of the first pass is 200 mm / s and the rolling deformation is 15%. After the rolling is completed, it is immediately returned to the furnace for holding for 100 min. The rolling speed of the second pass is 100 mm / s and the rolling deformation is 40%. After the rolling is completed, it is placed in a box furnace and held at 1100℃ for 4 h. It is then cooled with the furnace and subjected to stress relief treatment.

[0053] (6) Post-rolling treatment: Cut the stainless steel support in step (4) with wire cutting to remove the stainless steel plate and the isolation layer, and obtain the 60NiTi alloy plate.

[0054] The 60NiTi alloy sheet obtained in this embodiment has a smooth surface, no cracks, and no obvious oxidation. The microstructure of the sheet after rolling is as follows: Figure 4 As shown, by Figure 4 It can be seen that its microstructure exhibits elongated grains along the rolling direction, with the Ni3Ti phase distributed at the grain boundaries.

[0055] The 60NiTi alloy plate obtained in this embodiment has a hardness of up to 64 HRC and a tensile strength of up to 1200 MPa. Comparative Example 1

[0056] A method for rolling 60NiTi alloy sheet includes the following steps: (1) Ingot preparation: 60NiTi alloy ingots were prepared by vacuum induction melting.

[0057] (2) Forging billet preparation: The heating rate of the ingot from room temperature to 500℃ was 8℃ / min, and the furnace temperature was held for 10min after reaching 500℃; the heating rate from 500℃ to 900℃ was 4℃ / min, and the furnace temperature was held for 20min after reaching 900℃; the heating rate from 900℃ to 1080℃ was controlled at 3℃ / min, and the furnace temperature was held for 2h after reaching 1080℃. The 60NiTi alloy was forged using isothermal forging process, with an isothermal forging temperature of 1080℃, a deformation amount of 20%, and a deformation rate of 1s. -1 60NiTi alloy slabs were obtained. After forging, the slabs were immediately placed in a box furnace and held at 950℃ for 2 hours, then cooled in the furnace.

[0058] (3) Slab preparation: The 60NiTi alloy slab is cut into plates of 300 mm (length) × 200 mm (width) × 20 mm (thickness) using wire electrical discharge machining.

[0059] (4) Rolling and forming: Unlike Example 1, this comparative example does not use a stainless steel plate cladding and rolling structure. Instead, the 60NiTi alloy slab obtained in step (3) is coated with yttrium oxide anti-oxidation coating and then exposed hot rolling is performed. The specific operation is as follows: the 60NiTi alloy slab coated with yttrium oxide anti-oxidation coating is placed in a box furnace, heated to 1000℃ and held for 2 h. After the holding period, it is immediately hot rolled and formed. The rolling speed of the first pass is 400 mm / s and the rolling deformation is 10%. After the rolling is completed, it is immediately returned to the furnace for 20 min. The rolling speed of the second pass is 200 mm / s and the rolling deformation is 20%. After the rolling is completed, it is placed in a box furnace and held at 1000℃ for 1 h. It is then cooled with the furnace and subjected to stress relief treatment.

[0060] (5) Post-rolling treatment: Use an angle grinder to remove the anti-oxidation coating on the surface of the rolled plate to obtain 60NiTi alloy rolled plate.

[0061] The fracture microstructure of the 60NiTi alloy obtained in this comparative example is as follows: Figure 5 As shown; by Figure 5 It can be seen that the board has developed transverse cracks and obvious oxidation. Comparative Example 2

[0062] A method for cladding and rolling 60NiTi alloy includes the following steps: (1) Ingot preparation: 60NiTi alloy ingots were prepared by vacuum induction melting.

[0063] (2) Forging billet preparation: The heating rate of the ingot from room temperature to 500℃ was 8℃ / min, and the furnace temperature was held for 10min after reaching 500℃; the heating rate from 500℃ to 900℃ was 4℃ / min, and the furnace temperature was held for 20min after reaching 900℃; the heating rate from 900℃ to 1050℃ was controlled at 3℃ / min, and the furnace temperature was held for 2h after reaching 1050℃. The 60NiTi alloy was forged using isothermal forging process, with an isothermal forging temperature of 1050℃, a deformation amount of 20%, and a deformation rate of 1s. -1 60NiTi alloy slabs were obtained. After forging, the slabs were immediately placed in a box furnace and held at 950℃ for 2 hours, then cooled in the furnace.

[0064] (3) Slab preparation: The 60NiTi alloy slab is cut into plates of 300 mm (length) × 200 mm (width) × 20 mm (thickness) using wire electrical discharge machining.

[0065] (4) Sandwich structure design: such as Figure 1As shown, a 60NiTi alloy slab is placed between two stainless steel plates coated with yttrium oxide. A 1mm thick insulating layer composed of high-temperature insulation cotton and ceramic powder in a thickness ratio of 4:1 is placed between the stainless steel plates and the 60NiTi alloy. The two stainless steel plates are welded together as a whole using a stainless steel bracket to obtain a sandwich structure 60NiTi alloy slab.

[0066] (5) Rolling and forming: The sandwich structure 60NiTi alloy slab obtained in step (4) is placed in a box furnace, heated to 900℃ and held for 3 h. After the holding period, it is immediately hot rolled. The rolling speed of the first pass is 1000 mm / s and the rolling deformation is 40%. After the rolling is completed, it is immediately returned to the furnace for 100 min. The rolling speed of the second pass is 800 mm / s and the rolling deformation is 20%. After the rolling is completed, it is placed in a box furnace and held at 1100℃ for 4 h. It is then cooled with the furnace and subjected to stress relief treatment.

[0067] (6) Post-rolling treatment: Cut the stainless steel support in step (4) with wire cutting to remove the stainless steel plate and the isolation layer, and obtain the 60NiTi alloy plate.

[0068] The fracture microstructure of the 60NiTi alloy obtained in this comparative example is as follows: Figure 6 As shown; by Figure 6 It is evident that the plate exhibits severe longitudinal cracking and a fracture surface displaying the typical blue brittleness characteristic of blue oxide. This is because 900℃ is a sensitive temperature for the large-scale precipitation of the Ni4Ti3 phase, resulting in significant alloy brittleness. Simultaneously, the initial large deformation of 40% far exceeds the alloy's plasticity limit, leading to the concentrated release of internal stress and the formation of longitudinal cracks. Furthermore, the deformation heat generated by the ultra-high speed of 1000 mm / s causes the local surface temperature to instantly drop to the blue brittleness sensitive range of 200~400℃. The pinning of dislocations by interstitial atoms further reduces plasticity, thereby causing the alloy to lose its plastic deformation capacity. Ultimately, this manifests as severe longitudinal cracking accompanied by a fracture surface displaying the typical blue brittleness characteristic of blue oxide, which, from the opposite perspective, confirms the rationality of the process parameter range of this invention.

[0069] The equipment used for the smelting, forging and rolling of the 60NiTi alloy is known in this technical field, and the operating process used is mastered by those skilled in this technical field.

Claims

1. A method for rapid forming of 60NiTi alloy plates using heat-shielded cladding and lamination rolling, characterized in that, A 60NiTi alloy slab is placed between two stainless steel plates, and the two stainless steel plates are welded together as a whole using a stainless steel bracket to obtain a sandwich structure 60NiTi alloy slab; then it is rolled; after rolling, the stainless steel bracket is cut off to obtain the 60NiTi alloy plate.

2. The method for rapid forming of 60NiTi alloy plates using heat-shielded cladding and lamination rolling according to claim 1, characterized in that, The sandwich structure can hold 1 to 4 60NiTi alloy slabs, and an isolation layer composed of high-temperature insulation cotton and ceramic powder in a thickness ratio of 3 to 5:1 is placed between the 60NiTi alloy slabs and between the 60NiTi alloy slabs and the stainless steel plate.

3. The method for rapid forming of 60NiTi alloy plates using heat-shielded cladding and lamination rolling according to claim 1, characterized in that, The thickness of the isolation layer is 1~2 mm.

4. The method for rapid forming of 60NiTi alloy plates using heat-shielded cladding and lamination rolling according to claim 1, characterized in that, The stainless steel sheet is coated with an anti-oxidation coating on both sides.

5. A method for rapid forming of 60NiTi alloy plates using heat-shielded cladding and lamination rolling according to claim 1, characterized in that, The rolling process is as follows: when the deformation per pass is 10%~20%, the rolling speed is 100 mm / s~400 mm / s; when the deformation per pass is 20%~40%, the rolling speed is 50 mm / s~200 mm / s; after each pass of rolling, the material is immediately returned to the furnace for heat preservation for 20~150 min; the above rolling process is repeated until the total deformation reaches the predetermined value; after rolling, the material is placed in a box furnace and held at 1000 ℃~1150 ℃ for 1 h~6 h, then cooled with the furnace for stress relief treatment.

6. The method for rapid forming of 60NiTi alloy plates using heat-shielded cladding and lamination rolling according to claim 1, characterized in that, The 60NiTi alloy slab is obtained by forging a 60NiTi alloy ingot into a 60NiTi alloy forging blank and then cutting it by electrical discharge wire cutting.

7. A method for rapid forming of 60NiTi alloy plates using heat-shielded cladding and lamination rolling according to claim 5, characterized in that, The 60NiTi alloy forging billet is prepared by isothermal forging, with an isothermal forging temperature of 950~1100℃, a deformation amount of 20~60%, and a deformation rate of 0.01~1 s. -1 After forging, the metal is immediately placed in a box furnace and held at 950~1150℃ for 2~6 hours, then cooled with the furnace.

8. A method for rapid forming of 60NiTi alloy plates using heat-shielded cladding and lamination rolling according to claim 5, characterized in that, The pre-forging heating regime for the 60NiTi alloy ingot is as follows: the heating rate from room temperature to 500℃ is 6~10℃ / min, and the furnace temperature is held for 10~20 min after reaching 500℃; the heating rate from 500℃ to 900℃ is 3~4℃ / min, and the furnace temperature is held for 20~30 min after reaching 900℃; the heating rate from 900℃ to the target temperature of 950~1100℃ is controlled at 2~3℃ / min, and the furnace temperature is held for 2~6 h after reaching the target temperature of 950~1100℃.

9. A method for rapid forming of 60NiTi alloy plates using heat-shielded cladding and lamination rolling according to claim 5, characterized in that, The 60NiTi alloy ingot was prepared by vacuum induction melting.

10. A method for rapid forming of 60NiTi alloy sheet using heat-shielded cladding rolling according to claim 5, characterized in that, The composition and mass percentage of the 60NiTi alloy are as follows: C≤300 ppm, O≤500 ppm, N≤100 ppm, 39 at.%≤Ti≤41 at.%, Ni: balance.

Citation Information

Patent Citations

  • Multidirectional forging method for nickel-rich nickel-titanium intermetallic compound

    CN114101554A

  • TiAl alloy plate sheathing and ply rolling method

    CN117299793A