A precision punching and flanging forming process for ultra-thin double-layer metal sheets
By using a process route based on clamping positioning and coaxial positioning references, the problems of interlayer slippage and warping in the punching and flanging process of ultra-thin double-layer metal sheets were solved, achieving precision forming and improving yield and forming accuracy.
Patent Information
- Application Number
- CN202611443835.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies are unable to effectively solve problems such as interlayer slippage, misalignment, warping, edge tearing, and hole position deviation that occur during the punching and flanging process of 0.1mm-level ultra-thin double-layer metal sheets, resulting in low yield and failure to meet precision assembly requirements.
The process route of clamping and positioning, determining the processing position, punching the bottom hole, grinding and polishing the edge of the bottom hole, punching the forming hole, flanging, and flattening is adopted. The double-layer thin plate is fixed by a fixture, the flanging allowance is accurately reserved, micro-cracks are eliminated, and the entire process is completed on a general-purpose drilling machine using a punch with a coaxial positioning reference.
It has achieved precision punching and flanging forming of double-layer thin plates with a thickness of 0.05mm to 0.1mm, solved the problems of interlayer slippage and warping, ensured forming accuracy and finished product quality, and improved the yield.
Smart Images

Figure CN123102840A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal sheet processing technology, and more specifically, to a precision punching and flanging forming process for ultra-thin double-layer metal sheets. Background Technology
[0002] Metal sheet stamping, as one of the main manufacturing processes, is widely used in the production of various precision structural parts. Among these processes, "punching and flanging" is often used to form bosses, threaded holes, or connecting lugs with specific geometric shapes on sheet metal to achieve assembly connections or functional integration between parts. Traditional punching and flanging processes are typically used for standard sheet metal with a thickness between 0.3mm and 2.0mm. For this type of sheet metal, existing punching and flanging die technologies are relatively mature, effectively controlling material springback, wrinkling, and cracking through reasonable clearance fits, lubrication measures, and die structure design, ensuring the dimensional accuracy and surface quality of the product. However, when the sheet metal thickness is reduced to 0.1mm or even thinner (e.g., in the 0.05mm~0.1mm range), existing stamping technology faces severe challenges, specifically in the following aspects: The material has extremely poor rigidity and is prone to unexpected deformation: a single-layer sheet with a thickness of 0.1mm is considered an extremely thin sheet with very low bending stiffness. During the stamping process, the sheet is easily affected by the lateral force of the die, frictional resistance, and inertial force, resulting in severe warping, offset, or "drifting" phenomena, leading to excessive deviation in punching position and difficulty in controlling the flange height and angle.
[0003] Edge quality is difficult to guarantee, and the risk of burrs and tears is high: In the stamping of ultra-thin plates, large burrs, tearing of the flanged edges, or thinning and cracking caused by uneven material stretching are very likely to occur.
[0004] Processing challenges of double-layer composite structures: The "double-layer thin plate" structure involved in this invention further increases the difficulty of the process. Punching and flanging in a double-layer state not only requires the upper and lower plates to deform synchronously, but also requires solving the problems of relative slippage between layers, interlayer interference, and stress concentration caused by the superposition of the thickness of the two layers of materials during the flanging process.
[0005] Currently, there is a lack of mature stamping solutions specifically for 0.1mm ultra-thin double-layer sheets on the market. If a step-by-step process of punching first and then flanging is adopted, the 0.1mm sheet is extremely prone to deformation during transportation and secondary positioning, which makes it difficult to align the upper and lower layers, resulting in huge cumulative errors and extremely low yield. If we try to directly perform double-layer synchronous stamping, the existing molds lack an effective interlayer positioning and constraint mechanism, which can easily cause the double-layer sheet to misalign, fold, or wrinkle locally during the flanging process, failing to meet the requirements of precision assembly.
[0006] In view of the shortcomings of the existing technology, there is an urgent need to develop a precision punching and flanging forming process specifically applicable to an ultra-thin double-layer metal sheet.
[0007] CN102527759A discloses a method for forming high-flange holes on thin sheets. This method includes steps of extruding a conical hole, reverse flanging, and shaping. It involves extruding a non-piercing conical hole into the sheet metal, flanging the conical hole in reverse, and drawing to form a high-flange hole. However, this method is designed for single-layer sheets and does not consider the interlayer fit problem after stacking two layers of thin sheets. When directly applied to ultra-thin double-layer metal sheets, the two layers are prone to relative slippage during the punching process, resulting in problems such as interlayer delamination, hole coaxiality deviation, and poor consistency of flanging height after flanging. At the same time, the hole openings of ultra-thin sheets naturally have micro-cracks after punching. Existing technology does not have a special bottom hole pretreatment process, and the tensile stress of flanging will cause the cracks to propagate, eventually leading to flanging tearing and a low finished product qualification rate. Summary of the Invention
[0008] To solve the above-mentioned technical problems, the present invention provides a precision punching and flanging forming process for ultra-thin double-layer metal sheets.
[0009] To achieve the above objectives, the present invention adopts the following technical solution: A precision punching and flanging forming process for ultra-thin double-layer metal sheets, wherein the double-layer metal sheet comprises an upper thin sheet and a lower thin sheet, both of which have a thickness of 0.5mm to 1mm; the process includes the following steps: S1. Clamping and positioning: The upper and lower thin plates are stacked together and fixed and pressed together by a clamp to form a double-layer thin plate; S2. Determine the machining location: Determine and mark the center position of the hole to be punched; S3. Punching the bottom hole: Fix the base on the worktable of the drilling machine, and clamp the bottom hole punch through the drilling machine chuck. The base has a countersunk hole. After the bottom hole punch is fixed, make sure that the countersunk hole of the base and the bottom hole punch are coaxial. Then place the clamped and positioned double-layer thin plate on the base, adjust the position so that the bottom hole punch is aligned with the center mark of the double-layer thin plate, and press down the drilling machine handle to drive the bottom hole punch to break through the double-layer thin plate and punch a bottom hole in the double-layer thin plate. The diameter of the bottom hole is the final formed hole diameter minus 3~4mm, and the punch size of the bottom hole punch is equal to the bottom hole diameter. S4. Grinding and polishing the edge of the bottom hole: Use a grinding tool to grind and polish the bottom hole obtained by punching. The diameter of the hole after grinding is controlled to be 0.1~0.5mm larger than the diameter of the punched bottom hole. S5. Punching Forming Holes: A forming punch is used for punching operations. The forming punch includes a clamping end and a punch end. The clamping end is fixed to the drill press chuck. The punch end has a trapezoidal structure, including a tapered transition section at the front end of the punch and a forming section connected to the tapered transition section. The diameter of the forming section is equal to the final forming hole diameter. During operation, the clamping end of the forming punch is fixed to the drill press chuck. The position of the base is adjusted so that the countersunk hole II on the base is coaxial with the forming punch. Then, the polished double-layer thin plate is placed on the base, and the position is adjusted so that the forming punch is aligned with the center of the bottom hole. Then, the forming punch is controlled to press down through the bottom hole to complete the punching forming hole operation. S6. Flanging: Flanging is performed using a flanging punch; the flanging punch is provided with a flanging working edge and a flanging end of a predetermined width, the flanging end is located at the front end of the flanging punch, and its diameter is adapted to the diameter of the forming hole; the flanging working edge is located at the rear end of the flanging end and has a tapered structure; during operation, the double-layer thin plate is placed on the base, so that the flanging punch is coaxial with the forming hole, and the flanging punch is pressed down to act on the opening of the forming hole, so that the edge of the forming hole is deformed outward along the circumferential direction to form an acute-angle flanging structure; S7. Flattening and shaping: Apply axial pressing force to the hole wall after flanging to flatten and shape the flanged part, thus completing the punching and flanging forming of ultra-thin double-layer metal sheet.
[0010] Furthermore, the clamp includes an upper pressure plate and a lower pressure plate, which are connected by bolts.
[0011] Furthermore, an upper pressure plate and a lower pressure plate are provided on each side of the double-layer thin plate, and a through hole is opened on each side of the pressure plate for connecting bolts.
[0012] Furthermore, in step S2, the center position of the hole is determined by scribing a line on the double-layer thin plate with calipers.
[0013] Furthermore, the front end of the bottom hole punch is provided with a conical tip.
[0014] Further, in step S4, a grinding milling tool is used for grinding and polishing.
[0015] Furthermore, in step S5, the forming punch is controlled to press down at a uniform speed through the bottom hole.
[0016] Furthermore, in step S7, the axial compressive force is applied by manually hammering and flattening the surface.
[0017] Furthermore, in step S7, the axial pressing force is applied by using a flattening punch in conjunction with a drilling machine to flatten the surface; the front end of the flattening punch is frustum-shaped, and the diameter of the frustum is larger than the final forming hole diameter.
[0018] Furthermore, the bottom hole punch, forming punch, turning punch, and flattening punch are all equipped with clamping ends, and the outer diameter of the clamping ends is uniformly set, all of which are compatible with the standard chuck of a general-purpose drilling machine.
[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention employs a process route of "clamping and positioning—determining the processing position—punching the bottom hole—grinding and polishing the edge of the bottom hole—punching the forming hole—flanging—flattening and shaping" to punch and flanging double-layer thin plates of 0.05mm~0.1mm. First, the double-layer thin plates are clamped and fixed by a pressure plate, effectively avoiding misalignment and warping caused by interlayer slippage or uneven force at a single point in traditional processes. After determining the center of the processing hole, the bottom hole is punched according to the design that the bottom hole diameter is equal to the final forming hole diameter minus 3~4mm, accurately reserving the flanging allowance to avoid cracking due to excessive allowance or insufficient size due to insufficient allowance. Then, the bottom hole opening is polished to remove micro-cracks and eliminate micro-cracks around the opening to prevent cracking during flanging. Then, the forming punch is used to expand the hole and the flanging punch is used to evenly extend the acute-angle flanging, and finally, it is flattened and shaped. The entire process uses a shared coaxial positioning reference, and the entire process can be completed on a general-purpose drilling machine with a punch. This breaks through the technical bottleneck that existing conventional molds cannot stably process double-layer thin plates below 0.1mm, providing a reliable solution for the field of precision machining, and combining stable forming accuracy with good economy. Attached Figure Description
[0020] Figure 1 This is a schematic diagram of the structure of the base, the flip-hole punch, the bottom hole punch, the forming punch, and the flattening punch of the present invention; Figure 2 This is a schematic diagram of the clamping of the present invention with the double-layer thin plate; Figure 3 This is a schematic diagram of the positioning hole determination method of the present invention; Figure 4 This is a schematic diagram of the bottom hole punching operation of the present invention; Figure 5 This is a schematic diagram of the bottom hole punch structure of the present invention; Figure 6 This is a schematic diagram showing the state of the sheet metal after the bottom hole has been punched. Figure 7 This is a schematic diagram of the forming punch structure of the present invention; Figure 8 This is a schematic diagram showing the state of the sheet metal after punching the forming holes according to the present invention; Figure 9 This is a schematic diagram of the state of the sheet metal after flanging according to the present invention; Figure 10 This is a schematic diagram of the perforated punch structure of the present invention; Figure 11 This is a schematic diagram of the flattening punch structure of the present invention; Figure 12 This is a schematic diagram of the structure of the sheet metal after it has been flattened according to the present invention; The components are: 1. Base; 2. Flanging punch; 21. Tapered structure; 3. Bottom hole punch; 31. Conical tip; 4. Forming punch; 41. Clamping end; 42. Tapered transition section; 43. Forming section; 5. Flattening punch; 6. Countersunk hole one; 7. Countersunk hole two; 8. Upper pressure plate; 9. Lower pressure plate; 10. Upper thin plate; 11. Lower thin plate; 12. Worktable; 13. Flanging. Detailed Implementation
[0021] The technical features of the present invention can be clearly explained. The present invention will be described in detail below through specific embodiments and with reference to the accompanying drawings.
[0022] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and therefore the scope of protection of the invention is not limited to the specific embodiments disclosed below.
[0023] Furthermore, in the description of this invention, it should be understood that the terms "center," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "axial," "radial," and "circumferential," etc., indicating orientation or positional relationships, are based on the orientation or positional relationships shown in the accompanying drawings and are only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the invention. In addition, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined with "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified.
[0024] In this invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection, an electrical connection, or a communication connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.
[0025] In this invention, unless otherwise expressly specified and limited, the "on" or "below" of the second feature can mean that the first feature is in direct contact with the second feature, or that the first and second features are in indirect contact through an intermediate medium. In the description of this specification, references to terms such as "an embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described can be combined in any suitable manner in one or more embodiments or examples.
[0026] Example 1 Please see Figures 1 to 12 This embodiment provides a precision punching and flanging forming process for ultra-thin double-layer metal sheets. The double-layer metal sheet includes an upper thin plate 10 and a lower thin plate 11, both of which have a thickness of 0.1 mm. This embodiment takes the forming of a φ15 mm hole and flanging process as an example. The process includes the following steps: S1. Clamping and positioning: The upper thin plate 10 and the lower thin plate 11 are stacked together and fixed and pressed by a clamp to form a double-layer thin plate.
[0027] In step S1, the clamp includes an upper pressure plate 8 and a lower pressure plate 9, which are connected by bolts. The clamping method is as follows: Figure 2 As shown, an upper pressure plate 8 and a lower pressure plate 9 are provided on each side of the double-layer thin plate. The upper thin plate 10 and the lower thin plate 11 are stacked together and pressed together by the upper pressure plate 8 and the lower pressure plate 9. At the same time, a through hole is opened on each side of the pressure plate for connecting bolts. The double-layer thin plate can be fixed and pressed by tightening the bolts to prevent the thin plate from misaligning or warping in subsequent operations.
[0028] S2. Determine the machining position: Determine the center position of the hole to be punched and mark it.
[0029] In step S2, as Figure 3 As shown, the center position of the hole can be determined by scribing a line on the double-layer thin plate with calipers.
[0030] S3. Punching the Bottom Hole: Fix the base 1 on the worktable 12 of the drilling machine. The bottom hole punch 3 is clamped and fixed by the drilling machine chuck. The base 1 has a countersunk hole 6. After the bottom hole punch 3 is fixed, make sure that the countersunk hole 6 of the base 1 and the bottom hole punch 3 are coaxial. Then, place the clamped and positioned double-layer thin plate on the base 1, adjust the position so that the bottom hole punch 3 is aligned with the center mark of the double-layer thin plate, and press down the drilling machine handle to drive the bottom hole punch 3 to punch through the double-layer thin plate to obtain the bottom hole. Hole; the diameter of the bottom hole is the final forming hole diameter minus 3~4mm, and the punch size of the bottom hole punch 3 is equal to the bottom hole diameter; this step uses a precise design to control the subsequent flanging quality by making the bottom hole diameter equal to the final forming hole diameter minus 3~4mm. If the bottom hole diameter is too large, the flanging material allowance corresponding to the forming hole will be insufficient, and the target forming size and flanging height cannot be achieved; if the bottom hole diameter is too small, the flanging material allowance will be too large, and stress concentration during the flanging process will easily cause cracking.
[0031] In step S3, since the final formed hole is φ15mm, the bottom hole is set to 15-4=11mm, and the diameter of the countersunk hole on the base is... The bottom hole punch is The diameter of the punch's clamping end is φ10mm, and the clamping limit is 15mm. The bottom end of the punch is designed with a tapered tip to facilitate punching through thin plates and aligning with the scribing center. After the base and punch are fixed, ensure that the inner circle of the punch on the base is coaxial with the outer circle of the punch. The double-layer thin plate after punching the punch is as follows: Figure 6 As shown.
[0032] S4. Grinding and polishing the edge of the bottom hole: Use a grinding tool to grind and polish the bottom hole obtained by punching. The diameter of the hole after grinding is controlled to be 0.1~0.5mm larger than the diameter of the punched bottom hole.
[0033] In step S4, after the bottom hole is punched, micro-cracks are prone to appear at the edge of the hole. If not treated, more serious cracks will appear in the subsequent hole turning process. In actual operation, a general grinding milling tool should be used to grind the hole opening, and the diameter expansion should be controlled at 0.1~0.5mm to remove any possible micro-cracks.
[0034] S5. Punching a forming hole: A forming punch 4 is used for punching. The forming punch 4 includes a clamping end 41 and a punch end. The clamping end 41 is fixed to the drill press chuck. The punch end has a trapezoidal structure, including a tapered transition section 42 at the front end of the punch and a forming section 43 connected to the tapered transition section 42. The diameter of the forming section 43 is equal to the final forming hole diameter. During operation, the clamping end 41 of the forming punch 4 is fixed to the drill press chuck. The position of the base 1 is adjusted so that the countersunk hole 7 on the base 1 is coaxial with the forming punch 4. Then, the polished double-layer thin plate is placed on the base 1, and the position is adjusted so that the forming punch 4 is aligned with the center of the bottom hole. Then, the forming punch 4 is pressed down through the bottom hole to complete the punching of the forming hole.
[0035] In step S5, this process first positions the forming punch and the countersunk hole 7 on the base. The positioning method is the same as the method for punching the bottom hole, ensuring that the forming punch 4 is coaxial with the base. The forming punch is as follows... Figure 7 As shown, a trapezoidal structure is set at the bottom, with a minimum diameter of Slightly smaller than the diameter of the bottom hole; in actual operation, the operator uses the drill handle to press down slowly and evenly, and the forming punch 4 slowly passes through the bottom hole, and the final formed hole diameter is 15. The formed double-layer board is as follows: Figure 8 As shown.
[0036] S6. Flanging: Flanging is performed using a flanging punch 2. The flanging punch 2 is provided with a flanging working edge and a flanging end of a predetermined width. The flanging end is located at the front end of the flanging punch 2, and its diameter is adapted to the diameter of the forming hole. The flanging working edge is located at the rear end of the flanging end and has a tapered structure 21. During operation, the double-layer thin plate is placed on the base 1, so that the flanging punch 2 is coaxial with the forming hole. The flanging punch 2 is pressed down and acts on the opening of the forming hole, so that the edge of the forming hole is deformed outward along the circumferential direction to form an acute-angle flanging structure 13.
[0037] In step S6, the tool used for flanging is the flanging punch 2. The flanging punch 2 is used to expand the φ15 edge, forming an acute angle with the double-layer board, as shown in the schematic diagram. Figure 9 As shown. In actual operation, the selected punch 2 is as follows: Figure 10 As shown, in actual operation, place the double-layer thin plate that needs to be perforated on the plane of base 1. It is not necessary to align it with the hole on base 1; simply ensure that the perforating punch 2 is coaxial with the hole on the thin plate. Use the drill handle to press down slowly and evenly, causing the thin plate to deform gradually. Figure 9 The shape shown is acceptable; in addition, the width of the edge of the punch 2 used for punching is greater than the size of the flange 13 of the board, so as to ensure that the root will not contact the board. The end diameter of the punch 2 is φ14.9mm, so as to ensure that the end can be fitted inside the board.
[0038] S7. Flattening and shaping: Apply axial pressing force to the hole wall after flanging to flatten and shape the flanging part 13, thus completing the punching and flanging forming of ultra-thin double-layer metal sheet.
[0039] In step S7, the flattening punch 5 is used for the final flattening operation. The dimensions of the flattening punch 5 are shown in the schematic diagram below. Figure 11 As shown. The specific operation method is the same as the flanging operation. The double-layer board after flanging is as follows. Figure 12 As shown.
[0040] In this embodiment, the bottom hole punch 3, forming punch 4, turning punch 2 and flattening punch 5 are all provided with clamping ends, and the outer diameter of the clamping ends is uniformly set. They are all adapted to the standard chuck of a general drilling machine, so as to realize the rapid punch change operation between processes on a single drilling machine.
[0041] Example 2 Please see Figures 1 to 12 This embodiment provides a precision punching and flanging forming process for ultra-thin double-layer metal sheets. The double-layer metal sheet includes an upper thin plate 10 and a lower thin plate 11, both of which have a thickness of 0.1 mm. This embodiment takes the forming of a φ10 mm hole and flanging process as an example. The process includes the following steps: S1. Clamping and positioning: The upper thin plate 10 and the lower thin plate 11 are stacked together and fixed and pressed by a clamp to form a double-layer thin plate.
[0042] In step S1, the clamp includes an upper pressure plate 8 and a lower pressure plate 9, which are connected by bolts. The clamping method is as follows: Figure 2 As shown, an upper pressure plate 8 and a lower pressure plate 9 are provided on each side of the double-layer thin plate. The upper thin plate 10 and the lower thin plate 11 are stacked together and pressed together by the upper pressure plate 8 and the lower pressure plate 9. At the same time, a through hole is opened on each side of the pressure plate for connecting bolts. The double-layer thin plate can be fixed and pressed by tightening the bolts to prevent the thin plate from misaligning or warping in subsequent operations.
[0043] S2. Determine the machining position: Determine the center position of the hole to be punched and mark it.
[0044] In step S2, as Figure 3 As shown, the center position of the hole can be determined by scribing a line on the double-layer thin plate with calipers.
[0045] S3. Punching the Bottom Hole: Fix the base 1 on the worktable 12 of the drilling machine. The bottom hole punch 3 is clamped and fixed by the drilling machine chuck. The base 1 has a countersunk hole 6. After the bottom hole punch 3 is fixed, make sure that the countersunk hole 6 of the base 1 and the bottom hole punch 3 are coaxial. Then, place the clamped and positioned double-layer thin plate on the base 1, adjust the position so that the bottom hole punch 3 is aligned with the center mark of the double-layer thin plate, and press down the drilling machine handle to drive the bottom hole punch 3 to punch through the double-layer thin plate to obtain the bottom hole. Hole; the diameter of the bottom hole is the final forming hole diameter minus 3~4mm, and the punch size of the bottom hole punch 3 is equal to the bottom hole diameter; this step uses a precise design to control the subsequent flanging quality by making the bottom hole diameter equal to the final forming hole diameter minus 3~4mm. If the bottom hole diameter is too large, the flanging material allowance corresponding to the forming hole will be insufficient, and the target forming size and flanging height cannot be achieved; if the bottom hole diameter is too small, the flanging material allowance will be too large, and stress concentration during the flanging process will easily cause cracking.
[0046] In step S3, since the final formed hole is φ10mm, the bottom hole is set to 10-3=7mm, and the diameter of the countersunk hole on the base is... The bottom hole punch is The diameter of the clamping end of the punch is φ10mm, and the clamping limit is 15mm. The bottom end of the punch is set with a conical tip to facilitate punching through thin plates and aligning with the scribing center. After the base and the punch are fixed, ensure that the inner circle of the punch on the base is coaxial with the outer circle of the punch.
[0047] S4. Grinding and polishing the edge of the bottom hole: Use a grinding tool to grind and polish the bottom hole obtained by punching. The diameter of the hole after grinding is controlled to be 0.1~0.5mm larger than the diameter of the punched bottom hole.
[0048] In step S4, after the bottom hole is punched, micro-cracks are prone to appear at the edge of the hole. If not treated, more serious cracks will appear in the subsequent hole turning process. In actual operation, a general grinding milling tool should be used to grind the hole opening, and the diameter expansion should be controlled at 0.1~0.5mm to remove any possible micro-cracks.
[0049] S5. Punching a forming hole: A forming punch 4 is used for punching. The forming punch 4 includes a clamping end 41 and a punch end. The clamping end 41 is fixed to the drill press chuck. The punch end has a trapezoidal structure, including a tapered transition section 42 at the front end of the punch and a forming section 43 connected to the tapered transition section 42. The diameter of the forming section 43 is equal to the final forming hole diameter. During operation, the clamping end 41 of the forming punch 4 is fixed to the drill press chuck. The position of the base 1 is adjusted so that the countersunk hole 7 on the base 1 is coaxial with the forming punch 4. Then, the polished double-layer thin plate is placed on the base 1, and the position is adjusted so that the forming punch 4 is aligned with the center of the bottom hole. Then, the forming punch 4 is pressed down through the bottom hole to complete the punching of the forming hole.
[0050] In step S5, this process first positions the forming punch 4 and the countersunk hole 7 on the base 1. The positioning method is the same as the method for punching the bottom hole, ensuring that the forming punch 4 and the base 1 are coaxial. The forming punch 4 is as follows... Figure 7 As shown, a trapezoidal structure is set at the bottom, with a minimum diameter of Slightly smaller than the diameter of the bottom hole; in actual operation, the operator uses the drill handle to press down slowly and evenly, and the forming punch 4 slowly passes through the bottom hole, resulting in a final hole diameter of φ10. The formed double-layer plate is as follows. Figure 8 As shown.
[0051] S6. Flanging: Flanging is performed using a flanging punch 2. The flanging punch 2 is provided with a flanging working edge and a flanging end of a predetermined width. The flanging end is located at the front end of the flanging punch, and its diameter is adapted to the diameter of the forming hole. The flanging working edge is located at the rear end of the flanging end and has a tapered structure 21. During operation, the double-layer thin plate is placed on the base 1, so that the flanging punch 2 is coaxial with the forming hole. The flanging punch 2 is pressed down and acts on the opening of the forming hole, so that the edge of the forming hole is deformed outward along the circumferential direction to form an acute-angle flanging structure 13.
[0052] In step S6, the tool used for flanging is the flanging punch 2. The flanging punch 2 is used to expand the φ10 edge, forming an acute angle with the double-layer board, as shown in the schematic diagram. Figure 9 As shown. In actual operation, the selected punch 2 is as follows: Figure 10 As shown, in actual operation, place the double-layer thin plate that needs to be perforated on the plane of base 1. It is not necessary to align it with the hole on base 1; simply ensure that the perforating punch 2 is coaxial with the hole on the thin plate. Use the drill handle to press down slowly and evenly, causing the thin plate to deform gradually. Figure 9 The shape shown is acceptable; in addition, the width of the edge of the punch 2 used for punching is greater than the size of the flange 13 of the board, so as to ensure that the root will not contact the board. The end diameter of the punch 2 is φ9.9mm, so as to ensure that the end can be fitted inside the board.
[0053] S7. Flattening and shaping: Apply axial pressing force to the hole wall after flanging to flatten and shape the flanging part 13, thus completing the punching and flanging forming of ultra-thin double-layer metal sheet.
[0054] In step S7, the board that has already been flanged can be flattened by hammering; the double-layer board after flanging is as follows: Figure 12 As shown.
[0055] Example 3 Please see Figures 1 to 12This embodiment provides a precision punching and flanging forming process for ultra-thin double-layer metal sheets. The double-layer metal sheet includes an upper thin plate 10 and a lower thin plate 11, both with a thickness of 0.05 mm. This embodiment takes the forming of a φ15 mm hole and flanging process as an example. The process includes the following steps: S1. Clamping and positioning: The upper thin plate 10 and the lower thin plate 11 are stacked together and fixed and pressed by a clamp to form a double-layer thin plate.
[0056] In step S1, the clamp includes an upper pressure plate 8 and a lower pressure plate 9, which are connected by bolts. The clamping method is as follows: Figure 2 As shown, an upper pressure plate 8 and a lower pressure plate 9 are provided on each side of the double-layer thin plate. The upper thin plate 10 and the lower thin plate 11 are stacked together and pressed together by the upper pressure plate 8 and the lower pressure plate 9. At the same time, a through hole is opened on each side of the pressure plate for connecting bolts. The double-layer thin plate can be fixed and pressed by tightening the bolts to prevent the thin plate from misaligning or warping in subsequent operations.
[0057] S2. Determine the machining position: Determine the center position of the hole to be punched and mark it.
[0058] In step S2, as Figure 3 As shown, the center position of the hole can be determined by scribing a line on the double-layer thin plate with calipers.
[0059] S3. Punching the Bottom Hole: Fix the base 1 on the worktable 12 of the drilling machine. The bottom hole punch 3 is clamped and fixed by the drilling machine chuck. The base 1 has a countersunk hole 6. After the bottom hole punch 3 is fixed, make sure that the countersunk hole 6 of the base 1 and the bottom hole punch 3 are coaxial. Then, place the clamped and positioned double-layer thin plate on the base 1, adjust the position so that the bottom hole punch 3 is aligned with the center mark of the double-layer thin plate, and press down the drilling machine handle to drive the bottom hole punch 3 to punch through the double-layer thin plate to obtain the bottom hole. Hole; the diameter of the bottom hole is the final forming hole diameter minus 3~4mm, and the punch size of the bottom hole punch 3 is equal to the bottom hole diameter; this step uses a precise design to control the subsequent flanging quality by making the bottom hole diameter equal to the final forming hole diameter minus 3~4mm. If the bottom hole diameter is too large, the flanging material allowance corresponding to the forming hole will be insufficient, and the target forming size and flanging height cannot be achieved; if the bottom hole diameter is too small, the flanging material allowance will be too large, and stress concentration during the flanging process will easily cause cracking.
[0060] In step S3, since the final formed hole is φ15mm, the bottom hole is set to 15-4=11mm, and the diameter of the countersunk hole on the base is... The bottom hole punch is The diameter of the punch's clamping end is φ10mm, and the clamping limit is 15mm. The bottom end of the punch is designed with a tapered tip to facilitate punching through thin plates and aligning with the scribing center. After the base and punch are fixed, ensure that the inner circle of the punch on the base is coaxial with the outer circle of the punch. The double-layer thin plate after punching the punch is as follows: Figure 6 As shown.
[0061] S4. Grinding and polishing the edge of the bottom hole: Use a grinding tool to grind and polish the bottom hole obtained by punching. The diameter of the hole after grinding is controlled to be 0.1~0.5mm larger than the diameter of the punched bottom hole.
[0062] In step S4, after the bottom hole is punched, micro-cracks are prone to appear at the edge of the hole. If not treated, more serious cracks will appear in the subsequent hole turning process. In actual operation, a general grinding milling tool should be used to grind the hole opening, and the diameter expansion should be controlled at 0.1~0.5mm to remove any possible micro-cracks.
[0063] S5. Punching a forming hole: A forming punch 4 is used for punching. The forming punch 4 includes a clamping end 41 and a punch end. The clamping end 41 is fixed to the drill press chuck. The punch end has a trapezoidal structure, including a tapered transition section 42 at the front end of the punch and a forming section 43 connected to the tapered transition section 42. The diameter of the forming section 43 is equal to the final forming hole diameter. During operation, the clamping end 41 of the forming punch 4 is fixed to the drill press chuck. The position of the base 1 is adjusted so that the countersunk hole 7 on the base 1 is coaxial with the forming punch 4. Then, the polished double-layer thin plate is placed on the base 1, and the position is adjusted so that the forming punch 4 is aligned with the center of the bottom hole. Then, the forming punch 4 is pressed down through the bottom hole to complete the punching of the forming hole.
[0064] In step S5, this process first positions the forming punch and the countersunk hole 7 on the base. The positioning method is the same as the method for punching the bottom hole, ensuring that the forming punch 4 is coaxial with the base. The forming punch is as follows... Figure 7 As shown, a trapezoidal structure is set at the bottom, with a minimum diameter of Slightly smaller than the diameter of the bottom hole; in actual operation, the operator uses the drill handle to press down slowly and evenly, and the forming punch 4 slowly passes through the bottom hole, and the final formed hole diameter is 15. The formed double-layer board is as follows: Figure 8 As shown.
[0065] S6. Flanging: Flanging is performed using a flanging punch 2. The flanging punch 2 is provided with a flanging working edge and a flanging end of a predetermined width. The flanging end is located at the front end of the flanging punch 2, and its diameter is adapted to the diameter of the forming hole. The flanging working edge is located at the rear end of the flanging end and has a tapered structure 21. During operation, the double-layer thin plate is placed on the base 1, so that the flanging punch 2 is coaxial with the forming hole. The flanging punch 2 is pressed down and acts on the opening of the forming hole, so that the edge of the forming hole is deformed outward along the circumferential direction to form an acute-angle flanging structure 13.
[0066] In step S6, the tool used for flanging is the flanging punch 2. The flanging punch 2 is used to expand the φ15 edge, forming an acute angle with the double-layer board, as shown in the schematic diagram. Figure 9 As shown. In actual operation, the selected punch 2 is as follows: Figure 10 As shown, in actual operation, place the double-layer thin plate that needs to be perforated on the plane of base 1. It is not necessary to align it with the hole on base 1; simply ensure that the perforating punch 2 is coaxial with the hole on the thin plate. Use the drill handle to press down slowly and evenly, causing the thin plate to deform gradually. Figure 9 The shape shown is acceptable; in addition, the width of the edge of the punch 2 used for punching is greater than the size of the flange 13 of the board, so as to ensure that the root will not contact the board. The end diameter of the punch 2 is φ14.9mm, so as to ensure that the end can be fitted inside the board.
[0067] S7. Flattening and shaping: Apply axial pressing force to the hole wall after flanging to flatten and shape the flanging part 13, thus completing the punching and flanging forming of ultra-thin double-layer metal sheet.
[0068] In step S7, the flattening punch 5 is used for the final flattening operation. The dimensions of the flattening punch 5 are shown in the schematic diagram below. Figure 11 As shown. The specific operation method is the same as the flanging operation. The double-layer board after flanging is as follows. Figure 12 As shown.
[0069] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. Those skilled in the art can make other variations or modifications based on the above description. It is neither necessary nor possible to exhaustively describe all embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the claims of the present invention.
Claims
1. A precision punching and flanging forming process for ultra-thin double-layer metal sheets, wherein the double-layer metal sheet comprises an upper thin sheet and a lower thin sheet, both the upper and lower thin sheets having a thickness of 0.5mm to 1mm; characterized in that, The process includes the following steps: S1. Clamping and positioning: The upper and lower thin plates are stacked together and fixed and pressed by a clamp to form a double-layer thin plate; S2. Determine the machining location: Determine and mark the center position of the hole to be punched; S3. Punching the bottom hole: Fix the base on the worktable of the drilling machine, and clamp the bottom hole punch through the drilling machine chuck. The base has a countersunk hole. After the bottom hole punch is fixed, make sure that the countersunk hole of the base and the bottom hole punch are coaxial. Then place the clamped and positioned double-layer thin plate on the base, adjust the position so that the bottom hole punch is aligned with the center mark of the double-layer thin plate, and press down the drilling machine handle to drive the bottom hole punch to break through the double-layer thin plate and punch a bottom hole in the double-layer thin plate. The diameter of the bottom hole is the final formed hole diameter minus 3~4mm, and the punch size of the bottom hole punch is equal to the bottom hole diameter. S4. Grinding and polishing the edge of the bottom hole: Use a grinding tool to grind and polish the bottom hole obtained by punching. The diameter of the hole after grinding is controlled to be 0.1~0.5mm larger than the diameter of the punched bottom hole. S5. Punching Forming Holes: A forming punch is used for punching operations. The forming punch includes a clamping end and a punch end. The clamping end is fixed to the drill press chuck. The punch end has a trapezoidal structure, including a tapered transition section at the front end of the punch and a forming section connected to the tapered transition section. The diameter of the forming section is equal to the final forming hole diameter. During operation, the clamping end of the forming punch is fixed to the drill press chuck. The position of the base is adjusted so that the countersunk hole II on the base is coaxial with the forming punch. Then, the polished double-layer thin plate is placed on the base, and the position is adjusted so that the forming punch is aligned with the center of the bottom hole. Then, the forming punch is controlled to press down through the bottom hole to complete the punching forming hole operation. S6. Flanging: Flanging is performed using a flanging punch; the flanging punch is provided with a flanging working edge and a flanging end of a predetermined width, the flanging end is located at the front end of the flanging punch, and its diameter is adapted to the diameter of the forming hole; the flanging working edge is located at the rear end of the flanging end and has a tapered structure; during operation, the double-layer thin plate is placed on the base, so that the flanging punch is coaxial with the forming hole, and the flanging punch is pressed down to act on the opening of the forming hole, so that the edge of the forming hole is deformed outward along the circumferential direction to form an acute-angle flanging structure; S7. Flattening and shaping: Apply axial pressing force to the hole wall after flanging to flatten and shape the flanged part, thus completing the punching and flanging forming of ultra-thin double-layer metal sheet.
2. The precision punching and flanging forming process for ultra-thin double-layer metal sheets according to claim 1, characterized in that, The clamp includes an upper pressure plate and a lower pressure plate, which are connected by bolts.
3. The precision punching and flanging forming process for ultra-thin double-layer metal sheets according to claim 2, characterized in that, An upper pressure plate and a lower pressure plate are provided on each side of the double-layer thin plate, and a through hole is opened on each side of the pressure plate for connecting bolts.
4. The precision punching and flanging forming process for ultra-thin double-layer metal sheets according to claim 1, characterized in that, In step S2, the center position of the hole is determined by scribing a line on the double-layer thin plate with calipers.
5. The precision punching and flanging forming process for ultra-thin double-layer metal sheets according to claim 1, characterized in that, The front end of the bottom hole punch is provided with a conical tip.
6. The precision punching and flanging forming process for ultra-thin double-layer metal sheets according to claim 1, characterized in that, In step S4, a grinding milling tool is used for grinding and polishing.
7. The precision punching and flanging forming process for ultra-thin double-layer metal sheets according to claim 1, characterized in that, In step S5, the forming punch is controlled to press down at a uniform speed through the bottom hole.
8. The precision punching and flanging forming process for ultra-thin double-layer metal sheets according to claim 1, characterized in that, In step S7, the axial compressive force is applied by manually hammering and flattening the surface.
9. The precision punching and flanging forming process for ultra-thin double-layer metal sheets according to claim 1, characterized in that, In step S7, the axial pressing force is applied by using a flattening punch in conjunction with a drilling machine to flatten the material; the front end of the flattening punch is frustum-shaped, and the diameter of the frustum is larger than the final forming hole diameter.
10. The precision punching and flanging forming process for ultra-thin double-layer metal sheets according to claim 9, characterized in that, The bottom hole punch, forming punch, turning punch, and flattening punch are all equipped with clamping ends, and the outer diameter of the clamping ends is uniformly set, all of which are compatible with the standard chuck of a general drilling machine.
Citation Information
Patent Citations
Hole flanging method and die for forming high flange on thin plate
CN102527759A