A high-conductivity and heat-resistant aluminum alloy material

By using a composite structure of high-purity aluminum in the core and an alloy on the surface, along with specific processing techniques, the contradiction between strength and conductivity in high-conductivity aluminum alloy materials has been resolved, achieving a balance between high conductivity and heat resistance, and improving the overall performance of the material.

CN123102970APending Publication Date: 2026-11-17SUZHOU JINJIDAN ALLOY MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611269582.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

While existing high-conductivity aluminum alloy materials improve strength, their conductivity is often negatively affected, and there are discontinuities at the mechanical assembly interface.

Method used

It adopts a composite structure of high-purity aluminum core and surface alloy, and forms a metallurgical interface and axial fiber structure through semi-solid concentric coating casting and variable temperature gradient drawing, combined with dual-zone aging treatment, thereby reducing the influence of surface strengthening elements on conductivity.

Benefits of technology

A balance between high conductivity and heat resistance was achieved, avoiding the problem of discontinuity at the mechanical assembly interface and improving the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102970A_ABST
    Figure CN123102970A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of aluminum alloy materials and metal composite material preparation technology, specifically relating to a high-conductivity and heat-resistant aluminum alloy material. It aims to solve the technical problem of the contradiction between strength and conductivity. The aluminum alloy material is prepared by concentric casting of a high-purity core aluminum and a surface alloy to form a composite billet, followed by continuous rolling, variable-temperature gradient drawing, and dual-zone aging treatment. The surface alloy, by mass percentage, comprises Ge 0.12%–0.45%, Ca 0.04%–0.18%, Sn 0.03%–0.16%, B 0.006%–0.035%, Te 0.01%–0.08%, with the balance being Al and unavoidable impurities. This material can also be used for heat-resistant wires, conductive rods, and high-current-carrying aluminum alloy components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aluminum alloy materials and metal composite materials preparation technology, and specifically relates to a high-conductivity and heat-resistant aluminum alloy material. Background Technology

[0002] Aluminum and aluminum alloys are widely used in conductors, conductive rods, busbars, and lightweight conductive components due to their low density, good electrical conductivity, and easy processing. Pure aluminum has high electrical conductivity but insufficient strength and heat resistance. Ordinary high-strength aluminum alloys improve strength through solid solution elements, dislocations, and precipitates, but solid solution atoms, grain boundaries, and coarse second phases increase electron scattering and reduce conductivity. Existing research has also indicated that highly conductive aluminum usually has low strength, while solid solution strengthening and segregation strengthening to improve strength often reduce conductivity; therefore, there is a trade-off between strength and conductivity.

[0003] Existing heat-resistant aluminum alloy wires are mostly alloyed using elements such as Zr, Sc, rare earth elements, Fe, and Si. For example, publication number CN101423908B discloses a high-conductivity, high-strength heat-resistant aluminum alloy wire, whose composition includes Zr 0.10%–0.40%, Fe 0.10%–0.80%, Si 0.04%–0.30%, Mg 0.50%–0.80%, and RE 0.10%–0.30%, etc., with a conductivity exceeding 58.0% IACS, a tensile strength exceeding 265 MPa, and a heat resistance exceeding 150℃. This approach can improve strength, but the distribution of multiple alloying elements throughout the conductive cross-section can easily increase electron scattering. Publication number CN112718907B discloses a high-strength, heat-resistant, heterogeneous aluminum alloy conductor and its preparation method. It uses 1070 aluminum rods and AlN / 1070 aluminum-based composite materials. First, the outer layer material is hot-extruded into a cylindrical tube, then the 1070 aluminum rod is inserted into the cylindrical tube and bonded by rotary forging. This method utilizes the outer AlN / 1070 composite material and the inner 1070 aluminum to form a heterogeneous conductor. This method involves mechanical assembly followed by rotary forging, with the outer layer being an AlN / 1070 composite material. It does not involve a Ge-Ca-Sn-B-Te surface alloy, nor does it employ semi-solid concentric casting to form a metallurgical bonding interface.

[0004] To address the aforementioned problems, this invention provides a high-conductivity and heat-resistant aluminum alloy material that reduces the adverse effects of strength on conductivity improvement. Summary of the Invention

[0005] This invention provides a high-conductivity and heat-resistant aluminum alloy material, composed of a core of high-purity aluminum and a surface alloy. The core high-purity aluminum provides a continuous low-resistance channel, while the surface alloy provides heat resistance strengthening and surface load-bearing capacity. Both contribute to electrical conductivity and load-bearing capacity. The material is produced through melting and refining, semi-solid concentric coating casting, continuous rolling, variable-temperature gradient drawing, and dual-zone aging treatment.

[0006] A high-conductivity and heat-resistant aluminum alloy material, the technical solution of which is as follows: S1: By mass percentage, Ge 0.12%–0.45%, Ca 0.04%–0.18%, Sn 0.03%–0.16%, B 0.006%–0.035%, Te 0.01%–0.08%, with unavoidable impurities not exceeding 0.10%, and the balance being Al, are used for batching. Specifically, Al-10%Ge master alloy, Al-10%Ca master alloy, pure tin, Al-5%B master alloy, pure tellurium, and industrial pure aluminum are weighed out. The surface alloy batch is added to a resistance melting furnace and heated to 720℃ for melting. After the furnace charge is completely melted, a sodium-free refining agent is added for spray refining, slag removal, and the melt temperature is controlled to be stable between 710℃ and 730℃. The melt is then filtered through a 30ppi ceramic foam filter to obtain the surface alloy melt. Industrial pure aluminum is added to another resistance melting furnace and melted at 720℃. After being treated with the same refining and degassing process, the melt temperature is controlled to be between 710℃ and 730℃ to obtain the high-purity aluminum core melt. S2: The surface alloy melt is subjected to semi-solid shearing and slurry preparation; the core high-purity aluminum melt and the surface semi-solid slurry are fed into a twin-flow concentric coating casting machine and formed in a coaxial nozzle to obtain a composite billet with a diameter of 100 mm, the core volume fraction being 62% to 68%, and the surface alloy volume fraction being 32% to 38%; S3: The composite billet is homogenized and annealed, and then continuously rolled to obtain a composite rod with a diameter of 20mm; S4: The composite rod is sequentially drawn in a gradient manner to obtain a composite wire with a diameter of 7.5mm; S5: The composite wire is subjected to dual-zone aging treatment, and then naturally cooled to room temperature to obtain the alloy material of the present invention.

[0007] Furthermore, the sodium-free refining agent mentioned in step S1 accounts for 0.3% of the total melt mass, and the sodium-free refining agent is a mixture of KCl and MgCl2 in a mass ratio of 1:1.

[0008] Furthermore, the spray refining described in step S1 specifically involves introducing high-purity nitrogen gas for spray refining, with a refining time of 15 minutes, a rotor speed of 300 rpm, and a settling time of 20 minutes.

[0009] Further, the semi-solid shearing pulping described in step S2 specifically involves cooling the surface alloy melt to 640℃~655℃ and performing semi-solid shearing pulping with a shearing speed of 1200rpm and a shearing time of 5min, so that the solid fraction reaches 25%~35%.

[0010] Furthermore, the homogenization annealing described in step S3 specifically involves an annealing temperature of 320–380°C, a holding time of 6–10 hours, and furnace cooling to room temperature.

[0011] Further, the continuous rolling described in step S3 specifically involves rolling the composite billet from 100mm to 20mm, with a total section reduction rate of 96% during continuous hot rolling, a continuous rolling temperature of 420-460℃, and a final rolling temperature controlled at 320℃.

[0012] Furthermore, the gradient pulling described in step S4 specifically includes: First pass: Die temperature 380℃, drawing deformation 15%; Second pass: Die temperature 360℃, drawing deformation 15%; Third pass: Die temperature 340℃, drawing deformation 15%; 4th pass: Die temperature 320℃, drawing deformation 15%; 5th pass: Die temperature 300℃, drawing deformation 15%; 6th pass: Die temperature 270℃, drawing deformation 15%. 7th pass: Die temperature 240℃, drawing deformation 15%; 8th pass: Die temperature 210℃, drawing deformation 15%; 9th pass: Die temperature 180℃, drawing deformation 15%; 10th pass: Die temperature 120℃, drawing deformation 15%; 11th pass: Die temperature 60℃, drawing deformation 15%; 12th pass: Die temperature room temperature, drawing deformation 16%.

[0013] Furthermore, in the dual-zone aging treatment described in step S5, the temperature of the first aging zone is 220℃~250℃, and the holding time is 0.5~3h; the temperature of the second aging zone is 150℃~180℃, and the holding time is 2~8h. The aging treatment is carried out in a nitrogen protective atmosphere.

[0014] Compared with the prior art, the present invention has the following beneficial effects: (1) The core of the present invention is continuously permeated with high-purity aluminum, and the conductive current is mainly transmitted through the core, which reduces the influence of the surface strengthening elements on the overall conductivity; the surface alloy is heat-resistant and strengthened by composite micro-alloying of Ge, Ca, Sn, B and Te, without relying on Zr, Sc and rare earth elements.

[0015] (2) The semi-solid concentric coating casting of the present invention forms a metallurgical bonding interface, avoiding the problems of mechanical fitting interface gap and rotary forging interface discontinuity; the variable temperature gradient drawing forms an axial fiber structure and work hardening layer, and the dual-zone aging stabilizes Ge precipitation and Ca grain boundary pinning. Attached Figure Description

[0016] Figure 1 This is a flowchart illustrating the preparation process of a high-conductivity and heat-resistant aluminum alloy material according to the present invention.

[0017] Figure 2 This is a characterization diagram of the test in Experiment Example 1. Detailed Implementation

[0018] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0019] The preferred embodiments of the present invention are described in detail below; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

[0020] like Figure 1 The flowchart shown illustrates the preparation process of a high-conductivity, heat-resistant aluminum alloy material. The detailed preparation steps are as follows: 1. Preparation of surface alloy melt and core high-purity aluminum melt Weigh out Al-10%Ge master alloy, Al-10%Ca master alloy, pure tin, Al-5%B master alloy, pure tellurium, and industrial pure aluminum. Add the surface alloy ingredients to a resistance melting furnace and melt them. After the furnace charge is completely melted, add a sodium-free refining agent, which is a mixture of KCl and MgCl2. Purge with high-purity nitrogen for refining, remove slag, and filter the melt through a 30ppi ceramic foam filter to obtain the surface alloy melt. Add the core high-purity aluminum ingredients to another resistance melting furnace and melt them. After processing with the same refining and degassing process, obtain the core high-purity aluminum melt. When the Ge content is too low, precipitation strengthening is insufficient; when the content is too high, coarse Ge-enriched phases are easily formed, reducing plasticity. This invention employs a low Ge content combined with rapid semi-solid solidification and aging. During aging, Ge precipitates from the supersaturated solid solution state in the aluminum matrix, forming fine Ge-enriched precipitates or Ge-enriched regions. These precipitates interact with dislocations, subgrain boundaries, or grain boundaries, thereby improving the thermal stability and softening resistance of the surface alloy. By controlling the Al4Ca phase size through low Ca content and semi-solid solidification, it is mainly distributed at grain boundaries and subgrain boundaries, suppressing grain boundary migration and re-grain boundary formation at high temperatures. Crystallization enhances heat resistance and softening resistance; the grain boundary segregation of Te ensures that Te preferentially resides at grain boundaries or in impurity-rich regions, rather than being largely dissolved in the Al matrix, thus reducing electron scattering caused by solid-solid impurities; Bo is added as an Al-B master alloy, which can form stable borides with transition metal impurities such as Ti, V, and Zr, reducing the solid-solid content of impurities in the aluminum matrix after heat preservation, sedimentation, and ceramic filtration; a trace amount of Sn is added to reduce interfacial energy, promote Ge precipitation nucleation, and improve surface deformation compatibility during surface solidification and aging.

[0021] 2. Semi-solid concentric coating casting The surface alloy melt is cooled and semi-solid sheared into a slurry; the core high-purity aluminum melt and the surface semi-solid slurry are respectively fed into a twin-flow concentric coating casting machine and formed in a coaxial nozzle to obtain a composite billet. The surface alloy is made into a semi-solid slurry and then coated onto the outside of the high-purity aluminum core. The semi-solid slurry has high viscosity, which reduces the large-scale diffusion of surface alloying elements into the high-purity aluminum core, while simultaneously forming a thin diffusion layer at the interface to achieve metallurgical bonding. Compared with mechanical casting, concentric coating casting can reduce interface voids and oxide film inclusions.

[0022] 3. Continuous rolling The composite billet is homogenized and annealed, then cooled to room temperature in the furnace, and then continuously rolled to obtain a composite rod with a diameter of 20 mm. Continuous rolling causes the core and the surface to undergo plastic deformation simultaneously, thereby improving the interfacial bonding strength.

[0023] 4. Temperature gradient drawing The composite rods are sequentially subjected to gradient drawing: First pass: Die temperature 380℃, drawing deformation 15%; Second pass: Die temperature 360℃, drawing deformation 15%; Third pass: Die temperature 340℃, drawing deformation 15%; 4th pass: Die temperature 320℃, drawing deformation 15%; 5th pass: Die temperature 300℃, drawing deformation 15%; 6th pass: Die temperature 270℃, drawing deformation 15%. 7th pass: Die temperature 240℃, drawing deformation 15%; 8th pass: Die temperature 210℃, drawing deformation 15%; 9th pass: Die temperature 180℃, drawing deformation 15%; 10th pass: Die temperature 120℃, drawing deformation 15%; 11th pass: Die temperature 60℃, drawing deformation 15%; 12th pass: Die temperature room temperature, drawing deformation 16%, finally obtaining composite wire; variable temperature gradient drawing first improves deformation coordination at a higher temperature, and then increases dislocation density and axial fiber structure at a lower temperature.

[0024] 5. Dual-zone timeliness processing The composite wire was subjected to a two-zone aging treatment. The first aging zone temperature was 220℃~250℃, and the holding time was 0.5~3h. The second aging zone temperature was 150℃~180℃, and the holding time was 2~8h. The first aging zone promoted Ge precipitation and Al4Ca phase stabilization, while the second aging zone reduced residual stress and reduced over-aging. The aging treatment was carried out in a nitrogen protective atmosphere, and the material was naturally cooled to room temperature after the aging treatment to obtain the alloy material of the present invention.

[0025] Example 1 Table 1 Raw Material Information Table S1: The alloy is prepared by mass percentage as follows: Ge 0.25%, Ca 0.08%, Sn 0.08%, B 0.015%, Te 0.03%, unavoidable impurities not exceeding 0.10%, with the balance being Al. Specifically, weigh out Al-10%Ge master alloy, Al-10%Ca master alloy, pure tin, Al-5%B master alloy, pure tellurium, and industrial pure aluminum. Add the surface alloy to a resistance melting furnace and heat to 720℃ to melt. After the furnace charge is completely melted, add 0.3% of a sodium-free refining agent (KCl and MgCl2 in a mass ratio of 1:1) to the total melt. The mixture of 1 was refined by blowing high-purity nitrogen gas for 15 minutes at a rotor speed of 300 rpm, and then allowed to stand for 20 minutes. Slag was removed, and the melt temperature was controlled to be stable at 720℃. The melt was then filtered through a 30 ppi ceramic foam filter to obtain a surface alloy melt. Industrial pure aluminum was added to another resistance melting furnace and melted at 720℃. After being treated with the same refining and degassing process, the melt temperature was controlled at 720℃ to obtain a core high-purity aluminum melt. S2: The surface alloy melt is cooled to 645℃ and subjected to semi-solid shearing slurry preparation at a shearing speed of 1200 rpm for 5 minutes to achieve a solid fraction of 30%. The core high-purity aluminum melt and the surface semi-solid slurry are fed into a twin-flow concentric coating casting machine and formed in a coaxial nozzle to obtain a composite billet with a diameter of 100 mm. The core volume fraction is 65% and the surface alloy volume fraction is 35%. S3: The composite billet is homogenized and annealed at a temperature of 350℃ for 8 hours. It is then cooled to room temperature in the furnace and continuously rolled from 100mm to 20mm. The total section reduction rate of the continuous hot rolling is 96%, the continuous rolling temperature is 440℃, and the final rolling temperature is controlled at 320℃ to obtain a composite rod with a diameter of 20mm. S4: The composite rod is sequentially drawn in a gradient manner: First pass: Die temperature 380℃, drawing deformation 15%; Second pass: Die temperature 360℃, drawing deformation 15%; Third pass: Die temperature 340℃, drawing deformation 15%; 4th pass: Die temperature 320℃, drawing deformation 15%; 5th pass: Die temperature 300℃, drawing deformation 15%; 6th pass: Die temperature 270℃, drawing deformation 15%. 7th pass: Die temperature 240℃, drawing deformation 15%; 8th pass: Die temperature 210℃, drawing deformation 15%; 9th pass: Die temperature 180℃, drawing deformation 15%; 10th pass: Die temperature 120℃, drawing deformation 15%; 11th pass: Die temperature 60℃, drawing deformation 15%; 12th pass: Die temperature room temperature, drawing deformation 16%, finally obtaining a composite wire with a diameter of 7.5mm; S5: The composite wire is subjected to a two-zone aging treatment. The temperature of the first aging zone is 235℃ and the holding time is 2 hours. The temperature of the second aging zone is 165℃ and the holding time is 5 hours. The aging treatment is carried out in a nitrogen protective atmosphere. After the aging treatment, the wire is naturally cooled to room temperature to obtain the alloy material of the present invention.

[0026] Example 2 The preparation method is the same as in Example 1, but with the following differences: In step S1: the ingredients are prepared according to the following mass percentages: Ge 0.12%, Ca 0.04%, Sn 0.03%, B 0.006%, Te 0.01%, unavoidable impurities not exceeding 0.10%, and the balance being Al.

[0027] Example 3 The preparation method is the same as in Example 1, but with the following differences: In step S1: the ingredients are prepared according to the following mass percentages: Ge 0.45%, Ca 0.18%, Sn 0.16%, B 0.035%, Te 0.08%, unavoidable impurities not exceeding 0.10%, and the balance being Al.

[0028] Example 4 The preparation method is the same as in Example 1, but with the following differences: In step S1: the melt temperature is controlled to be stable at 710℃ to obtain the surface alloy melt; the melt temperature is controlled at 710℃ to obtain the core high-purity aluminum melt. In step S2: the surface alloy melt is cooled to 640°C and semi-solid shearing is performed to make the solid fraction reach 35%; the core volume fraction is 62% and the surface alloy volume fraction is 38%.

[0029] Example 5 The preparation method is the same as in Example 1, but with the following differences: In step S1: the melt temperature is controlled to be stable at 730℃ to obtain the surface alloy melt; the melt temperature is controlled at 730℃ to obtain the core high-purity aluminum melt. In step S2: the surface alloy melt is cooled to 655°C and semi-solid shearing is performed to make the solid fraction reach 25%; the core volume fraction is 68% and the surface alloy volume fraction is 32%.

[0030] Example 6 The preparation method is the same as in Example 1, but with the following differences: In step S3: the annealing temperature is 380℃, the holding time is 6h; the continuous rolling temperature is 460℃. In step S5: the temperature of the first aging zone is 250℃ and the holding time is 0.5h; the temperature of the second aging zone is 180℃ and the holding time is 2h.

[0031] Example 7 The preparation method is the same as in Example 1, but with the following differences: In step S3: the annealing temperature is 320℃, the holding time is 10h; the continuous rolling temperature is 420℃; In step S5: the temperature of the first aging zone is 220℃, and the holding time is 3 hours; the temperature of the second aging zone is 150℃, and the holding time is 8 hours.

[0032] Comparative Example 1 The preparation method of Example 1 is followed, but a single homogeneous aluminum alloy material is prepared according to the surface alloy composition of Example 1, without the inclusion of a core high-purity aluminum. All other steps are the same.

[0033] Comparative Example 2 The preparation method of Example 1 is followed, but Ge is not added to the surface alloy composition. All other steps are the same.

[0034] Comparative Example 3 The preparation method of Example 1 is followed, but Ca is not added to the surface alloy composition. All other steps are the same.

[0035] Comparative Example 4 The preparation method of Example 1 is followed, but Te is not added to the surface alloy composition. All other steps are the same.

[0036] Comparative Example 5 The preparation method of Example 1 is followed, but B is not added to the surface alloy composition. All other steps are the same.

[0037] Comparative Example 6 The preparation method of Example 1 was followed, but without dual-zone aging; the sample was simply placed at room temperature for 24 hours. All other steps were the same.

[0038] Experimental Example 1 The finished product prepared in Example 1 was subjected to cross-sectional low-magnification testing, core / surface interface SEM-BSE high-magnification testing, and EDS / EPMA elemental surface testing, respectively. Cross-sectional low-magnification testing used SEM low-magnification BSE mode, with an accelerating voltage of 10–15 kV, a working distance of 8–12 mm, a magnification of 15×–40×, and a beam current of 0.5–2 nA. Core / surface interface SEM-BSE high-magnification testing used a field emission scanning electron microscope, with an accelerating voltage of 10–15 kV, a beam current of 1–3 nA, a working distance of 8–10 mm, an aperture of 30–60 μm, and a magnification of 500×–2000×. EDS / EPMA elemental surface testing used an FE-SEM+SDDEDS detector, EDSmapping mode, an accelerating voltage of 15–20 kV, and a beam current of 5–10 nA. The test results are as follows: Figure 2 As shown; Figure 2 (a) is a low-magnification morphology image of the cross-section of the finished composite wire of Example 1. The wire exhibits a distinct core-surface concentric composite structure, with the core continuously penetrating and the surface alloy uniformly coating the outer periphery of the core. Figure 2(b) is a SEM-BSE image of the interface between the high-purity aluminum core and the surface alloy. The interface is continuous and dense, and no through cracks, pores, mechanical gaps, or continuous oxide film interlayers were observed. Fine and diffuse compositional contrast differences are visible on the surface alloy side, while the microstructure on the core side is relatively clean, indicating that a stable metallurgical bonding interface was formed during concentric casting and subsequent rolling / drawing processes. Figure 2 (c) is the elemental distribution map of the core / surface interface region. Al is continuously distributed in the core and surface; Ge, Ca, Sn, and Te signals are mainly concentrated in the surface, while the core region is close to the background level; there is a narrow compositional transition region near the interface, indicating that the surface strengthening elements are confined to the outer region, while there is limited diffusion at the interface, which is conducive to metallurgical bonding.

[0039] Experiment Example 2 The comprehensive properties of the aluminum alloy materials prepared in Examples 1-7 and Comparative Examples 1-6 were determined. Conductivity Testing: Referring to standard GB / T 3048.2-2007 "Test Methods for Electrical Properties of Wires and Cables Part 2: Resistivity Test of Metallic Materials", the aluminum alloy materials prepared in each embodiment and comparative example were cut into straight specimens with a length of 300 mm. Both ends were smoothed with fine sandpaper. A double-arm bridge (accuracy class 0.05) was used to measure the resistance of the specimen under constant temperature conditions of 20℃±0.5℃. The distance between the current terminal and the potential terminal was accurate to 1 mm during measurement. Simultaneously, the diameter was measured at three locations: the middle and both ends of the specimen, and the average value was used to calculate the cross-sectional area. The resistivity was calculated using the formula ρ=R·S / L (where R is the measured resistance, S is the cross-sectional area, and L is the effective length between the potential terminals). After converting the resistivity to the standard value at 20℃, the value was calculated according to the International Association of Acrylic and Anodized Copper Standards (IACS, ρ0=0.017241Ω·mm). 2 The relative conductivity was calculated based on ρ / m: conductivity (%IACS) = 0.017241 / ρ × 100%; Tensile strength and elongation tests: Referring to standard GB / T 228.1-2021 "Metallic materials, tensile testing—Part 1: Tests at room temperature," tensile specimens with a length of 300 mm were cut from the finished wires of each embodiment and comparative example, with a gauge length of 200 mm. A CMT-5305 electronic universal testing machine equipped with a pneumatic flat-push clamp was used. The tensile rate was set to 2 mm / min in the elastic stage and 5 mm / min after yielding. Five parallel samples were tested for each scheme, and the arithmetic mean was taken. The tensile strength and elongation after fracture were recorded. Heat resistance test: Referring to standard GB / T 33381-2016 "Heat-resistant aluminum alloy wire for overhead stranded wire", 300mm long wire samples were cut from the finished wires of each embodiment and comparative example; the samples were placed in a constant temperature drying oven, heated to 280±2℃, and kept at that temperature for 1 hour; after the heat treatment, the samples were removed and allowed to cool naturally to room temperature in the air; the tensile strength after heat treatment was determined according to the above tensile test method; the strength retention rate was calculated according to the following formula: Strength retention rate = Tensile strength after heat treatment / Original tensile strength × 100%.

[0040] The specific test comparison results are shown in Table 2: Table 2. Comparison of overall performance between Examples 1-7 and Comparative Examples 1-6 The comparison results above show that Comparative Example 1, a homogeneous alloy without a core of high-purity aluminum, exhibits lower tensile strength, lower conductivity, and lower heat retention compared to the examples. When using a single homogeneous alloy, the strengthening element is dissolved throughout the matrix, resulting in electron scattering across the entire cross-section and significant conductivity loss. Furthermore, elements such as Ge and Ca consume their strengthening potential throughout the cross-section, failing to achieve the optimized configuration of "strengthening elements concentrated on the surface." Comparative Example 2, without Ge addition, shows lower tensile strength and lower heat retention compared to the examples. Ge is the core strengthening element of this invention; without Ge addition, the strength mainly relies on solid solution strengthening and a small amount of Al4Ca phase, significantly weakening the strengthening effect. Simultaneously, dislocations are easily recovered at high temperatures, leading to a significant deterioration in heat resistance. Comparative Example 3, without Ca addition, shows lower tensile strength and lower heat retention compared to the examples. The main function of Ca is to form the Al4Ca phase at grain boundaries and pin them. Without Ca addition, the grain boundaries lack an effective thermally stable pinning phase, leading to grain coarsening during homogenization annealing and aging. Simultaneously, grain boundary migration intensifies during heat treatment, resulting in a rapid decrease in high-temperature strength. Comparative Example 4, without Te addition, shows a decrease in conductivity and a slight decrease in tensile strength compared to the examples. Te is a key functional element in this invention; trace amounts of Te help regulate the solidification structure and grain boundary state of the surface alloy. Together with B purification, Ca grain boundary stabilization, and Ge enrichment precipitation, it reduces the negative impact of coarse second phases and harmful impurities in the surface alloy on conductivity and thermal stability. This comparative result directly verifies the unique contribution of Te grain boundary segregation to improved conductivity. Comparative Example 5, without B addition, shows a decrease in conductivity and a decrease in heat retention compared to the examples. The main function of B is to preferentially form high-melting-point borides with transition metal impurities such as Ti, V, and Cr, which are then removed through sedimentation and filtration, thereby purifying the aluminum matrix. Without B addition, impurity elements exist in the aluminum matrix in solid solution form. Each impurity atom causes local lattice distortion, becoming a strong electron scattering center. Meanwhile, solid solution impurities also affect the nucleation and growth behavior of Ge and Ca precipitates, indirectly and adversely impacting heat resistance. Comparative Example 6, without double-zone aging, showed a decrease in tensile strength and heat retention compared to the examples; this comparative example most directly verifies the crucial role of double-zone aging treatment. 24 hours at room temperature failed to effectively precipitate elements such as Ge and Sn; Ge remained in solid solution form within the Al matrix. The atomic radius of Ge differs from that of Al by approximately 3%, and the lattice distortion caused by solid solution produced a certain solid solution strengthening effect. However, the scattering effect of electrons by solid solution Ge is equally strong; the most significant difference lies in heat resistance: the alloy in the solid solution state rapidly undergoes over-aging and recovery softening at high temperatures, resulting in low strength retention.

[0041] In this invention, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0042] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.

Claims

1. A high-conductivity and heat-resistant aluminum alloy material, characterized in that, The composite aluminum alloy material comprises a core of high-purity aluminum extending continuously along the axial direction and a surface alloy concentrically covering the outer periphery of the core of high-purity aluminum, wherein the core of high-purity aluminum and the surface alloy form a metallurgical bonding interface; the mass fraction of Al in the core of high-purity aluminum is not less than 99.90%; the mass percentage composition of the surface alloy is: Ge 0.12%~0.45%, Ca 0.04%~0.18%, Sn 0.03%~0.16%, B 0.006%~0.035%, Te 0.01%~0.08%, unavoidable impurities not greater than 0.10%, and the balance being Al.

2. The high thermal conductivity and heat-resistant aluminum alloy material according to claim 1, characterized in that, The core has a volume fraction of 62% to 68%, the surface alloy has a volume fraction of 32% to 38%, and there is a metallurgical bonding interface between the high-purity aluminum core and the surface alloy.

3. A method for preparing a high-conductivity, heat-resistant aluminum alloy material according to any one of claims 1-2, characterized in that, Includes the following steps: S1: By mass percentage, Ge 0.12%–0.45%, Ca 0.04%–0.18%, Sn 0.03%–0.16%, B 0.006%–0.035%, Te 0.01%–0.08%, with unavoidable impurities not exceeding 0.10%, and the balance being Al, are used for batching. Specifically, Al-10%Ge master alloy, Al-10%Ca master alloy, pure tin, Al-5%B master alloy, pure tellurium, and industrial pure aluminum are weighed out. The surface alloy batch is added to a resistance melting furnace and heated to 720℃ for melting. After the furnace charge is completely melted, a sodium-free refining agent is added for spray refining, slag removal, and the melt temperature is controlled to be stable between 710℃ and 730℃. The melt is then filtered through a 30ppi ceramic foam filter to obtain the surface alloy melt. Industrial pure aluminum is added to another resistance melting furnace and melted at 720℃. After being treated with the same refining and degassing process, the melt temperature is controlled to be between 710℃ and 730℃ to obtain the high-purity aluminum core melt. S2: The surface alloy melt is subjected to semi-solid shearing and slurry preparation; the core high-purity aluminum melt and the surface semi-solid slurry are fed into a twin-flow concentric coating casting machine and formed in a coaxial nozzle to obtain a composite billet with a diameter of 100 mm, the core volume fraction being 62% to 68%, and the surface alloy volume fraction being 32% to 38%. S3: The composite billet is homogenized and annealed, and then continuously rolled to obtain a composite rod with a diameter of 20mm; S4: The composite rod is sequentially drawn in a gradient manner to obtain a composite wire with a diameter of 7.5mm; S5: The composite wire is subjected to dual-zone aging treatment, and then naturally cooled to room temperature to obtain the alloy material of the present invention.

4. The method for preparing a high-conductivity and heat-resistant aluminum alloy material according to claim 3, characterized in that, The sodium-free refining agent mentioned in step S1 accounts for 0.3% of the total melt mass. The sodium-free refining agent is a mixture of KCl and MgCl2 in a mass ratio of 1:

1.

5. The method for preparing a high-conductivity and heat-resistant aluminum alloy material according to claim 3, characterized in that, The spray refining described in step S1 specifically involves introducing high-purity nitrogen gas for spray refining, with a refining time of 15 minutes, a rotor speed of 300 rpm, and a settling time of 20 minutes.

6. The method for preparing a high-conductivity and heat-resistant aluminum alloy material according to claim 3, characterized in that, The semi-solid shearing pulping process described in step S2 specifically involves cooling the surface alloy melt to 640℃~655℃ and performing semi-solid shearing pulping at a shearing speed of 1200rpm for 5min, so that the solid fraction reaches 25%~35%.

7. The method for preparing a high-conductivity and heat-resistant aluminum alloy material according to claim 3, characterized in that, The homogenization annealing described in step S3 specifically involves an annealing temperature of 320–380°C, a holding time of 6–10 hours, and furnace cooling to room temperature.

8. The method for preparing a high-conductivity and heat-resistant aluminum alloy material according to claim 3, characterized in that, The continuous rolling process described in step S3 specifically involves rolling the composite billet from 100mm to 20mm, with a total section reduction rate of 96% during continuous hot rolling, a continuous rolling temperature of 420-460℃, and a final rolling temperature controlled at 320℃.

9. The method for preparing a high-conductivity and heat-resistant aluminum alloy material according to claim 3, characterized in that, The gradient pulling described in step S4 specifically refers to: First pass: Die temperature 380℃, drawing deformation 15%; Second pass: Die temperature 360℃, drawing deformation 15%; Third pass: Die temperature 340℃, drawing deformation 15%; 4th pass: Die temperature 320℃, drawing deformation 15%; 5th pass: Die temperature 300℃, drawing deformation 15%; 6th pass: Die temperature 270℃, drawing deformation 15%. 7th pass: Die temperature 240℃, drawing deformation 15%; 8th pass: Die temperature 210℃, drawing deformation 15%; 9th pass: Die temperature 180℃, drawing deformation 15%; 10th pass: Die temperature 120℃, drawing deformation 15%; 11th pass: Die temperature 60℃, drawing deformation 15%; 12th pass: Die temperature room temperature, drawing deformation 16%.

10. The method for preparing a high-conductivity and heat-resistant aluminum alloy material according to claim 3, characterized in that, The dual-zone aging treatment described in step S5 involves a first aging zone temperature of 220℃~250℃ and a holding time of 0.5~3h; and a second aging zone temperature of 150℃~180℃ and a holding time of 2~8h. The aging treatment is carried out in a nitrogen protective atmosphere.

Citation Information

Patent Citations

  • High conductivity, high intensity and heat resisting aluminum alloy conducting wire and method for producing the same and conducting wire

    CN101423908B

  • A high-strength, heat-resistant, heterogeneous aluminum alloy conductor and its preparation method

    CN112718907B