A welding process for a liquid-cooled pipeline distributor
By setting an annular flange and capillary gap on the liquid-cooled pipeline manifold, coating it with brazing flow retardant, and adopting low-temperature drying, medium-temperature glue removal, and four-zone continuous brazing processes, the problems of uneven brazing filler and poor joint forming consistency in the liquid-cooled pipeline manifold were solved, achieving continuous and stable brazing and reliable sealing of the copper-steel joint.
Patent Information
- Application Number
- CN202611546225.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing welding process of liquid-cooled pipeline manifolds, when multiple copper branch pipes are brazed to the carbon steel main water distribution pipe in batches, there are problems such as uneven filling of brazing filler metal, flow into the interior of the carbon steel main water distribution pipe, and poor joint formation consistency, which affect the flow distribution and operational stability of the liquid cooling system.
By machining annular flanges and setting annular capillary gaps on the carbon steel water distribution main pipe, coating it with brazing flow retardant, and combining low-temperature drying, medium-temperature glue removal, and four-zone continuous brazing processes, the furnace atmosphere and mesh belt running speed are controlled to achieve continuous and stable brazing of copper-steel joints.
The problem of uneven filler metal and poor joint forming consistency was solved, and the sealing reliability and stability of the liquid cooling pipeline distributor were improved, ensuring the continuous brazing effect of multiple copper-steel joints.
Smart Images

Figure CN123103104A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of liquid cooling pipeline welding technology, and in particular to a welding process for a liquid cooling pipeline distributor. Background Technology
[0002] Liquid cooling manifolds are used to distribute the coolant supplied by the main supply pipe to multiple liquid cooling branches. The quality of their connection directly affects the flow distribution and operational stability of the liquid cooling system. These manifolds are typically formed by connecting a carbon steel main supply pipe to multiple copper branch pipes. Copper and carbon steel differ in thermal conductivity, thermal expansion characteristics, and surface condition, so the forming quality of each branch connection point must be considered during batch welding.
[0003] Existing welding processes are prone to problems such as uneven filler metal, flow into the carbon steel main water distribution pipe, and poor consistency in the forming of multiple joints. At the same time, oxidation of the joint surface, concentrated escape of volatile components from the welding material, and asynchronous heating of the copper branch pipe and the carbon steel main water distribution pipe may also cause porosity, residues, misalignment of the copper branch pipe, and decreased sealing performance, making it difficult to meet the requirements for mass production and long-term stable operation of liquid-cooled pipeline manifolds. Summary of the Invention
[0004] The purpose of this invention is to propose a welding process for liquid-cooled pipeline manifolds, which aims to solve the problems of uneven filler metal filling, flow into the carbon steel water distribution main pipe, and poor joint formation consistency when multiple copper branch pipes are batch brazed to carbon steel water distribution main pipes.
[0005] A welding process for a liquid-cooled pipeline distributor according to an embodiment of the present invention includes the following steps:
[0006] S1. Machining multiple branch joint holes on the carbon steel water distribution main pipe, turning the edges of the branch joint holes outward to form an annular flange, and degreasing and removing oxides from the inner circumferential surface of the annular flange and the outer circumferential surface of the copper branch pipe insertion section to obtain the pretreated carbon steel water distribution main pipe and the pretreated copper branch pipe.
[0007] S2. Apply a brazing choke agent to the non-brazing area of the pretreated copper branch pipe insertion section, insert multiple pretreated copper branch pipes into the corresponding annular flanges respectively, retain the annular capillary gap between the pretreated copper branch pipe insertion section and the annular flanges, and apply brazing filler metal to the outer end of the annular flanges to obtain the water distributor assembly to be brazed.
[0008] S3. The water distributor assembly to be brazed is dried at low temperature and degummed at medium temperature to obtain a dried and degummed water distributor assembly.
[0009] S4. First, replace the atmosphere in the mesh belt continuous brazing furnace with nitrogen, then introduce a hydrogen-nitrogen mixed protective gas, place the dry glue removal water distributor assembly on the mesh belt in the furnace, and transport it through the preheating zone, reduction and activation zone, brazing filling zone and uniform temperature forming zone in sequence to obtain the brazed water distributor assembly.
[0010] S5. The brazed water distributor assembly is sent into the protective cooling zone of the mesh belt continuous brazing furnace and cooled in a hydrogen-nitrogen mixed protective atmosphere. After exiting the furnace, a liquid-cooled pipeline water distributor is obtained.
[0011] Optionally, in step S1, the annular flange extends 2-5 mm outward from the outer side of the carbon steel water distribution main pipe along the axial direction of the branch joint hole, and the distance between the outer end of the annular flange and the inner wall of the carbon steel water distribution main pipe along the axial direction of the branch joint hole is 5-10 mm.
[0012] Optionally, in step S1, the inner circumferential surface of the annular flange is pickled with a hydrochloric acid solution with a mass concentration of 5% to 10% for 1 to 3 minutes, and then sequentially washed with water, neutralized, rinsed with deionized water, and dried; the outer circumferential surface of the copper branch pipe insertion section is pickled with a sulfuric acid solution with a mass concentration of 5% to 10% for 1 to 3 minutes, and then sequentially washed with water, rinsed with deionized water, and dried.
[0013] Optionally, in step S2, the brazing throttling agent is a boron-based brazing throttling agent, the non-brazing area is an annular region with a width of 1 to 3 mm, and the non-brazing area is 0.5 to 1.5 mm away from the inner end of the annular capillary gap; after applying the brazing throttling agent, it is dried at 60 to 90°C for 5 to 15 minutes.
[0014] Optionally, in step S2, the one-sided gap between the outer circumferential surface of the pretreated copper branch pipe insertion section and the inner circumferential surface of the annular flange is 0.05 to 0.15 mm, and the end of the pretreated copper branch pipe extends into the interior of the carbon steel water distribution main pipe by 1 to 3 mm.
[0015] Optionally, in step S2, the solder is a copper-manganese-nickel solder paste, and the solidus temperature of the solder is 900-1000℃; the solder paste is continuously applied around the circumference of the pretreated copper branch pipe at the outer end of the annular flange to form an annular solder strip.
[0016] Optionally, in step S3, the low-temperature drying temperature is 80-110℃ and the time is 10-30 min; the medium-temperature debinding temperature is 180-250℃ and the time is 5-15 min.
[0017] Optionally, in step S4, nitrogen is first introduced until the residual oxygen content in the mesh belt continuous brazing furnace is less than 100 ppm, and then a hydrogen-nitrogen mixed protective gas with a hydrogen gas fraction of 5% to 25% is introduced until the residual oxygen content in the furnace does not exceed 10 ppm and the dew point of the hydrogen-nitrogen mixed protective gas is not higher than -40°C.
[0018] Optionally, in step S4, the running speed of the mesh belt inside the furnace is 220-300 mm / min; the temperature of the preheating zone is 750-850℃; the temperature of the reduction and activation zone is 880-950℃; the temperature of the brazing and filling zone is 1000-1030℃; and the temperature of the uniform forming zone is 980-1010℃.
[0019] Optionally, in step S5, before the temperature of the brazing filler metal drops below its solidus temperature, a hydrogen-nitrogen mixed protective gas is continuously introduced into the protective cooling zone; after the brazed water distributor assembly is taken out of the furnace, it undergoes surface cleaning, internal rinsing, weld appearance inspection, internal channel inspection and sealing performance testing in sequence, and the sealing performance testing pressure is not less than 1.5 times the design working pressure of the liquid-cooled pipeline water distributor.
[0020] The beneficial effects of this invention are:
[0021] 1. This invention solves the problems of uneven filler metal filling, flow into the carbon steel water distribution main, and poor joint forming consistency when multiple copper branch pipes are batch brazed to carbon steel water distribution main pipe. By setting an annular flange and an annular capillary gap, applying brazing flow barrier in the non-brazing area, and making the water distributor assembly undergo preheating, reduction activation, brazing filling, uniform temperature forming and protective cooling in sequence, the invention achieves continuous and stable brazing of multiple copper and steel joints in the liquid-cooled pipeline water distributor.
[0022] 2. This invention solves the problems of oxidation at the joint surface, concentrated escape of organic carriers, and uneven heating of copper branch pipes and carbon steel water distribution main pipes by degreasing and deoxide treatment of the annular flange and copper branch pipe insertion section, low-temperature drying and medium-temperature glue removal of the water distribution unit to be brazed, and controlling the residual oxygen content in the furnace, the protective gas dew point, the mesh belt running speed and the temperature of each temperature zone. This achieves continuous brazing and improves the sealing reliability of the liquid-cooled pipeline water distribution unit. Attached Figure Description
[0023] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used in conjunction with embodiments of the invention to explain the invention and do not constitute a limitation thereof. In the drawings:
[0024] Figure 1 The welding process flow diagram provided by this invention;
[0025] Figure 2The detection results of Examples 1 to 7 and Comparative Examples 1 to 3 provided by the present invention are shown in the figure.
[0026] Figure 3 A physical image of the liquid-cooled pipeline distributor provided by the present invention. Detailed Implementation
[0027] To enable those skilled in the art to better understand the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0028] The liquid-cooled piping manifold includes a carbon steel main distribution pipe and multiple copper branch pipes connected to it. The carbon steel main distribution pipe receives the coolant from the main supply pipe and distributes it to different liquid-cooled branches via the copper branch pipes. Because the copper branch pipes differ from the carbon steel main distribution pipe in material, wall thickness, and thermal conductivity, the shape of the branch joint holes, the insertion depth of the copper branch pipes, the annular capillary gap, the location of the brazing filler metal application, and the temperature of each zone all affect the melting and filling state of the brazing filler metal when multiple copper branch pipes are simultaneously brazed in the furnace. This invention provides continuous control over the flanging of the branch joint holes, the treatment of the joint surface, the setting of the flow-blocking area, the sleeve connection of the copper branch pipes, the application of the brazing filler metal, the zonal heating, and the protective cooling, enabling multiple copper-steel joints to be brazed in the same furnace cycle.
[0029] The complete process flow of this invention is as follows: Figure 1 As shown, the specific steps are as follows.
[0030] S1. Based on the arrangement of each copper branch pipe on the carbon steel water distribution main pipe, machine multiple branch joint holes on the carbon steel water distribution main pipe. After machining the branch joint holes, remove burrs from the hole edges and clean out metal debris from inside the carbon steel water distribution main pipe. Then, turn the edge of the branch joint hole outwards towards the outside of the carbon steel water distribution main pipe to form a continuous annular flange. The annular flange extends 2-5mm outwards along the axial direction of the branch joint hole, and the distance between the outer end of the annular flange and the inner wall of the carbon steel water distribution main pipe along the axial direction of the branch joint hole is 5-10mm. After flangening, round the annular flange to eliminate wrinkles, cracks, and local depressions.
[0031] Oil stains on the annular flange and its surrounding area are removed using an alkaline degreasing solution. After rinsing with water, the inner circumference of the annular flange is pickled for 1–3 minutes using a 5%–10% hydrochloric acid solution. Immediately after pickling, the flange is rinsed with water, neutralized with a weakly alkaline aqueous solution, and then rinsed with deionized water and dried. The concentration of the hydrochloric acid solution and the pickling time are selected based on the degree of oxidation on the surface of the carbon steel water distribution pipe. After pickling, the inner circumference of the annular flange remains intact, without excessive corrosion that could affect the dimensions of the branch joint holes.
[0032] After the copper branch pipes are cut to the designed length, the end faces are trimmed and burrs are removed, and the insertion ends are rounded. Alkaline degreasing solution is used to remove oil stains from the outer circumference of the insertion section of the copper branch pipe. After water washing, it is acid-washed with a 5%–10% sulfuric acid solution for 1–3 minutes, followed by water washing, deionized water rinsing, and drying to obtain the pretreated carbon steel main water distribution pipe and the pretreated copper branch pipe. Subsequent assembly is carried out promptly after surface treatment to reduce re-oxidation of the treated surface.
[0033] S2. Based on the insertion depth of the copper branch pipe, divide the pretreated copper branch pipe insertion section into a brazing zone and a non-brazing zone. The non-brazing zone is located on the outer circumference of the section where the copper branch pipe extends into the carbon steel main water distribution pipe. A boron-based brazing flow inhibitor is uniformly coated in this area, forming an annular region with a width of 1–3 mm. The non-brazing zone is 0.5–1.5 mm away from the inner end of the annular capillary gap. After coating, the pretreated copper branch pipe is placed in an environment of 60–90℃ to dry for 5–15 minutes, allowing the brazing flow inhibitor to adhere to the surface of the copper branch pipe and preventing it from entering the annular capillary gap.
[0034] Insert multiple pretreated copper branch pipes into the corresponding annular flanges on the pretreated carbon steel main water supply pipe. During insertion, keep the pipe ends coaxial with the annular flanges to prevent the inserted sections from scraping the inner circumference of the flanges. Control the single-sided gap between the outer circumference of the inserted section of the pretreated copper branch pipe and the inner circumference of the annular flange to be 0.05–0.15 mm, with the copper branch pipe ends extending 1–3 mm into the carbon steel main water supply pipe. For U-shaped copper branch pipes, simultaneously insert both ends of the same U-shaped copper branch pipe into the corresponding annular flanges, adjusting the insertion depth of each end to prevent the copper branch pipe ends from becoming out of round due to pressure. After all copper branch pipes have been inserted, verify the insertion depth, tilt, and adjacent spacing of each copper branch pipe.
[0035] The solder used is a copper-manganese-nickel solder paste with a solidus temperature of 900–1000℃. The solder paste is continuously applied circumferentially to the outer end of the annular flange along the pretreated copper branch pipe, forming a ring-shaped solder band around the pipe. The solder paste does not enter the non-brazing area of the copper branch pipe extending into the carbon steel main water distribution pipe. After solder application, the water distributor assembly to be brazed is obtained.
[0036] S3. Place the water distributor assembly to be brazed in an environment of 80-110℃ for low-temperature drying for 10-30 minutes to remove residual moisture and some low-boiling-point components from the brazing paste. After low-temperature drying, raise the temperature to 180-250℃ and maintain it for 5-15 minutes to gradually remove the organic carriers in the brazing paste, resulting in a dried and de-adhesive water distributor assembly. Low-temperature drying and medium-temperature de-adhesive removal are performed separately, preventing moisture and organic carriers from escaping in a concentrated manner upon entering the high-temperature zone, thus reducing brazing paste splashing, joint porosity, and carbonization residue.
[0037] S4. Before brazing, nitrogen gas is introduced into the mesh belt continuous brazing furnace. When the residual oxygen content in the furnace drops below 100 ppm, a hydrogen-nitrogen mixed protective gas with a hydrogen gas fraction of 5% to 25% is introduced to continue purging until the residual oxygen content in the furnace does not exceed 10 ppm. At the same time, the dew point of the hydrogen-nitrogen mixed protective gas is controlled at no higher than -40℃.
[0038] Place the drying and debinding water distributor assembly smoothly on the furnace inner conveyor belt, ensuring all copper and steel joints face upwards. Control the running speed of the inner conveyor belt at 220–300 mm / min, and sequentially transport the drying and debinding water distributor assembly through the preheating zone, reduction and activation zone, brazing and filling zone, and homogenization forming zone.
[0039] The temperature in the preheating zone is controlled at 750–850℃. The copper branch pipe and the carbon steel main water distribution pipe are heated synchronously in this temperature zone, and the joints of the carbon steel main water distribution pipe are fully preheated, reducing the instantaneous temperature difference between the thin-walled copper branch pipe and the carbon steel main water distribution pipe.
[0040] The temperature of the reduction and activation zone is controlled at 880–950℃. The copper-manganese-nickel solder paste has not completely melted in this temperature zone. The hydrogen-nitrogen mixed protective gas reduces the residual oxides on the outer circumference of the copper branch pipe insertion section, the inner circumference of the annular flange, and the surface of the solder, so that the joint surface maintains a surface condition suitable for solder spreading.
[0041] The temperature of the brazing filler zone is controlled at 1000–1030℃. After the brazing paste melts upon heating, it enters the annular capillary gap between the pretreated copper branch pipe insertion section and the annular flange from the outer end of the annular flange, and spreads along the circumference and insertion direction of the pretreated copper branch pipe. The brazing paste reaching the inner end of the annular capillary gap is restricted by the brazing flow-blocking agent on the surface of the non-brazing zone, and no longer flows along the outer circumference of the copper branch pipe into the interior of the carbon steel water distribution main pipe.
[0042] The temperature of the homogenization forming zone is controlled at 980–1010℃. The molten brazing filler metal entering the annular capillary gap continues to spread circumferentially within this temperature zone, filling in any incompletely filled areas, while simultaneously preventing the copper branch pipe from remaining at the higher temperature of the brazing filling zone for an extended period. After homogenization forming is completed, the brazed water distributor assembly is obtained.
[0043] S5. The mesh belt inside the furnace feeds the brazing distributor assembly into the protective cooling zone of the mesh belt continuous brazing furnace. Before the brazing filler metal temperature drops below its solidus temperature, a hydrogen-nitrogen mixed protective gas is continuously introduced into the protective cooling zone, allowing the brazing filler metal to solidify in the protective atmosphere. After solidification, the brazing filler metal continues to cool until it reaches a temperature suitable for safe removal from the furnace, at which point it is sent out of the mesh belt continuous brazing furnace.
[0044] After the brazed water distributor assembly is removed from the furnace, loose residues on its surface are cleaned, and residual flow-blocking material in non-brazed areas is removed using a cleaning method compatible with boron-based brazing flow-blocking agents. The interior of the carbon steel main water distributor and copper branch pipes is rinsed with clean water, and then purged and dried with clean compressed air.
[0045] After cleaning, the weld appearance, internal channel inspection, and sealing performance test are performed sequentially. During the weld appearance inspection, it is confirmed that each copper-steel joint forms a continuous brazing seam circumferentially, without missing material, cracks, localized material buildup, or dents or significant misalignment of the copper branch pipes. During the internal channel inspection, it is confirmed that there are no brazing filler nodules, flow-obstructing materials, or metal debris obstructing the flow of coolant around the insertion end of each copper branch pipe. The sealing performance test pressure is no less than 1.5 times the design working pressure of the liquid-cooled piping manifold. The test pressure is maintained for a specified time to check for leaks or abnormal pressure drops at each copper-steel joint. After the test is completed, the liquid-cooled piping manifold is obtained.
[0046] In some embodiments, the annular flange extends 2mm outward from the carbon steel main water supply pipe along the axial direction of the branch connector hole, and the distance between the outer end of the annular flange and the inner wall of the carbon steel main water supply pipe along the axial direction of the branch connector hole is 5mm. This is suitable for manifold structures with thinner carbon steel main water supply pipe walls and smaller spacing between copper branch pipes. In other embodiments, the annular flange extends 5mm outward from the carbon steel main water supply pipe, and the distance between the outer end of the annular flange and the inner wall of the carbon steel main water supply pipe is 10mm. This is suitable for manifold structures that require increased copper branch pipe sleeve length.
[0047] The unilateral gap between the outer circumference of the pretreated copper branch tube insertion section and the inner circumference of the annular flange can be adjusted within 0.05–0.15 mm based on the outer diameter deviation of the copper branch tube and the rounding accuracy of the annular flange. When the gap is close to the lower limit, the coaxiality of the copper branch tube and the annular flange is controlled to avoid scratching the mating surface during insertion. When the gap is close to the upper limit, the solder paste is continuously distributed along the circumference of the pretreated copper branch tube to avoid local lack of solder in the annular capillary gap.
[0048] The operating speed of the conveyor belt inside the furnace is adjusted in conjunction with the temperatures of the four temperature zones. When the conveyor belt operating speed is 220 mm / min, the residence time of the drying glue removal and water distribution unit in each temperature zone is relatively long, and the temperature of each zone is set to the low to medium value of the corresponding range. When the conveyor belt operating speed is 300 mm / min, the residence time in each temperature zone is relatively shortened, while the preheating zone and reduction activation zone still retain sufficient heating length, so that the joint of the carbon steel water distribution main pipe reaches a stable temperature before entering the brazing filling zone.
[0049] Example 1
[0050] In this embodiment, a 1m long, 4mm thick carbon steel main water distribution pipe is connected in batches to ten thin-walled copper branch pipes. The copper branch pipes have an outer diameter of 9.5mm and a wall thickness of 1mm, and the copper branch pipes are arranged according to the designed spacing.
[0051] Ten branch connector holes are machined on the carbon steel water distribution main pipe. The edges of each branch connector hole are turned outward by 3mm towards the outside of the carbon steel water distribution main pipe to form an annular flange. The distance from the outer end of the annular flange to the inner wall of the carbon steel water distribution main pipe along the axis of the branch connector hole is 7mm. After completing the rounding, the oil stains on the inner circumference of the annular flange are removed with an alkaline degreasing solution, and then pickled with an 8% hydrochloric acid solution for 2 minutes. After pickling, the flange is then washed with water, neutralized, rinsed with deionized water, and dried in sequence.
[0052] The insertion ends of ten copper branch pipes were rounded and degreased, then acid-washed with an 8% sulfuric acid solution for 2 minutes, followed by rinsing with water, deionized water, and drying. A boron-based brazing resistant agent was applied to the non-brazing area of each copper branch pipe insertion section, forming a 2mm wide annular region. The non-brazing region was spaced 1mm from the inner end of the annular capillary gap. After coating, the sections were dried at 75℃ for 10 minutes.
[0053] Ten pretreated copper branch pipes were inserted into their respective annular flanges. The gap between the outer circumference of the inserted section of the pretreated copper branch pipe and the inner circumference of the annular flange was 0.10 mm on one side, and the end of the copper branch pipe extended 2 mm into the carbon steel water distribution main pipe. A copper-manganese-nickel solder paste with a solidus temperature of 950℃ was applied continuously around the outer end of each annular flange along the circumference of the copper branch pipe to form an annular solder strip.
[0054] The water distributor components to be brazed were dried at 90℃ for 15 minutes, and then debinded at 200℃ for 8 minutes. Nitrogen was first introduced into the mesh belt continuous brazing furnace. After the residual oxygen content in the furnace was lower than 100 ppm, a hydrogen-nitrogen mixed protective gas with a hydrogen gas fraction of 15% was introduced until the residual oxygen content in the furnace was 8 ppm and the dew point of the protective gas was -45℃.
[0055] The dried glue-removing water distributor assembly is placed on a conveyor belt inside the furnace at a speed of 260 mm / min. The preheating zone temperature is 800℃, the reduction and activation zone temperature is 915℃, the brazing filling zone temperature is 1015℃, and the homogenization forming zone temperature is 995℃. After homogenization forming, the brazed water distributor assembly enters the protective cooling zone, where a hydrogen-nitrogen mixed protective gas is continuously introduced until the brazing filler metal temperature drops below 950℃. It is then further cooled and removed from the furnace.
[0056] After the brazed water distributor assembly is removed from the furnace, it undergoes surface cleaning, internal rinsing, and drying, followed by weld appearance inspection and internal channel inspection. In this embodiment, the design working pressure of the liquid-cooled pipeline water distributor is 1.6 MPa, the sealing performance test pressure is 2.4 MPa, and the pressure holding time is 30 minutes.
[0057] Examples 2 to 7 and Comparative Examples 1 to 3
[0058] Examples 2 to 7 and Comparative Examples 1 to 3 are all based on Example 1. Except for the parameters or processes listed in Table 1, the specifications, surface treatment methods, types of flow retardants, types of brazing filler metal, low-temperature drying conditions, medium-temperature glue removal conditions, protective gas conditions, and post-weld inspection methods of the carbon steel main water distribution pipe and the copper branch pipe are the same as those in Example 1.
[0059] Examples 2 and 3 only adjust the size of the annular flange; Examples 4 and 5 only adjust the annular capillary gap; Examples 6 and 7 only adjust the running speed of the mesh belt inside the furnace. Comparative Example 1 does not flange the branch joint holes; Comparative Example 2 does not set a non-brazing zone and does not apply a brazing flow retardant; Comparative Example 3 eliminates the preheating zone, reduction activation zone, and uniform temperature forming zone, allowing the water distributor assembly to directly enter the heating zone at a temperature of 1015°C.
[0060] Table 1
[0061] Comparative Example 1 does not have an annular flange, and its carbon steel water distribution main pipe has a wall thickness of 4 mm. Therefore, it does not have the distance from the outer end of the annular flange to the inner wall of the carbon steel water distribution main pipe.
[0062] The liquid-cooled manifolds prepared in Examples 1 to 7 and Comparative Examples 1 to 3 were tested under the same conditions. Ten copper-steel joints were set up in each group, and the number of joints with complete annular brazing seams, the number of copper branch pipes with significant skew, and the maximum height of the brazing filler metal inside the carbon steel main manifold were recorded. The sealing performance was tested at a pressure of 2.4 MPa for 30 minutes. The pressure drop during the pressure holding period was used to evaluate the sealing status of the liquid-cooled manifold. The test results are shown in Table 2.
[0063] Table 2
[0064] To facilitate comparison of the test results of Examples 1 to 7 and Comparative Examples 1 to 3, the number of complete annular brazing joints, the number of copper branch pipe deviations, the maximum inner brazing filler metal height, and the pressure drop after 30 minutes of holding pressure in Table 2 are plotted as bar charts, such as... Figure 2 As shown. Among them, Figure 2 A represents the number of complete joints in the annular brazing seam. Figure 2 B indicates the number of copper branch pipes deviated. Figure 2 C represents the maximum height of the inner solder nodule. Figure 2 D represents the pressure drop value after holding the pressure for 30 minutes.
[0065] As shown in Tables 1 and 2, Examples 1 to 3 only changed the outward extension length of the annular flange and the distance between the outer end of the annular flange and the inner wall of the carbon steel water distribution main pipe. All ten copper-steel joints in each group formed complete annular brazing seams, and no pressure drop occurred during the sealing performance test. In Example 2, the lower limit of the annular flange size was used, with a maximum inner brazing filler height of 0.2 mm; in Example 3, the upper limit of the annular flange size was used, with a maximum inner brazing filler height of 0.4 mm. No brazing filler accumulation obstructing the internal flow channel of the water distribution main pipe was formed. When the outward extension length of the annular flange was 2–5 mm and the distance between the outer end of the annular flange and the inner wall of the carbon steel water distribution main pipe was 5–10 mm, the copper branch pipe could maintain its sleeved state.
[0066] In Comparative Example 1, the branch joint hole was not flanged; the connection area between the copper branch pipe and the carbon steel main water supply pipe consisted only of the 4mm thick carbon steel main water supply pipe wall. Only seven out of ten copper-steel joints formed a complete annular brazing seam, and two copper branch pipes showed significant skewness. After holding the pressure for 30 minutes, the pressure dropped by 0.06 MPa. Compared to Example 1, the annular flange extended the connection area between the copper branch pipe and the branch joint hole, ensuring the stability of the copper branch pipe during transport and heating, and providing a continuous annular filling path for the brazing filler metal.
[0067] Examples 1, 4, and 5 only changed the unilateral gap between the outer circumferential surface of the pretreated copper branch pipe insertion section and the inner circumferential surface of the annular flange. When the unilateral gap was 0.05 mm, 0.10 mm, and 0.15 mm, ten complete annular brazing seams were formed in each group, and no pressure drop was observed during the sealing performance test. After the unilateral gap was increased to 0.15 mm, the maximum inner brazing nodule height increased to 0.5 mm, but it did not affect the internal channel of the main water distribution pipe, indicating that the unilateral gap of 0.05–0.15 mm can meet the capillary filling requirements of copper-manganese-nickel brazing paste.
[0068] In Comparative Example 2, no non-brazing zone was provided, and no boron-based brazing stop-off agent was coated on the outer peripheral surface of the insertion section of the copper branch pipe. The inspection results of the annular brazed seam and sealing performance of this group were qualified, but the maximum height of the inner brazing fillet reached 2.4 mm, and the internal channel inspection was unqualified. The molten brazing filler metal continued to flow along the outer peripheral surface of the copper branch pipe into the interior of the carbon steel water distribution main pipe after passing through the annular capillary gap, thereby forming obvious brazing filler metal accumulation. The non-brazing zone provided in Example 1 limits the wetting range of the brazing filler metal on the insertion section of the copper branch pipe, and reduces the amount of brazing filler metal entering the interior of the carbon steel water distribution main pipe.
[0069] Example 1, Example 6 and Example 7 only changed the running speed of the mesh belt in the furnace. When the running speeds of the mesh belt were 220 mm / min, 260 mm / min and 300 mm / min respectively, ten complete annular brazed seams were formed in each group, no deflection of the copper branch pipe or unqualified sealing performance occurred, indicating that under the condition that the temperatures of the four temperature zones remain unchanged, the mesh belt running speed of 220 to 300 mm / min can meet the continuous brazing requirements of the water distributor assembly.
[0070] In Comparative Example 3, the preheating zone, reduction activation zone and temperature equalization forming zone were omitted, so that the water distributor assembly directly entered the heating zone at 1015°C. Among the ten copper-steel joints, only eight formed complete annular brazed seams, three copper branch pipes were deflected, and the pressure dropped by 0.08 MPa after holding the pressure for 30 minutes. After the water distributor assembly directly enters the brazing temperature zone, the thin-walled copper branch pipe heats up faster than the carbon steel water distribution main pipe, the copper branch pipe softens first and changes its position, and part of the joint surfaces are not subjected to sufficient reduction activation treatment. After the preheating zone, reduction activation zone, brazing filling zone and temperature equalization forming zone are sequentially arranged, the copper branch pipe and the carbon steel water distribution main pipe are gradually heated, and the brazing filler metal continues to spread uniformly after completing melting and filling, so that multiple copper-steel joints maintain a consistent forming state.
[0071] A physical form of the liquid-cooled pipeline water distributor prepared by the above process is shown in Figure 3 as shown. The above specific embodiments illustrate the flanging of the branch joint hole, surface treatment, setting of the flow blocking zone, sleeving of the copper branch pipe, application of brazing filler metal, low-temperature drying, medium-temperature binder removal, establishment of protective atmosphere, four-zone continuous brazing, protective cooling and post-brazing inspection. Without changing the above process connection relationship, each parameter can be selected within the stated range according to the wall thickness of the carbon steel water distribution main pipe, the outer diameter of the copper branch pipe, the number of joints and the designed working pressure of the liquid-cooled pipeline water distributor.
[0072] The above are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art, within the technical scope disclosed in the present invention, shall cover all equivalent replacements or modifications made according to the technical solution of the present invention and the inventive concept thereof within the protection scope of the present invention.
Claims
1. A welding process for a liquid-cooled pipeline manifold, characterized in that, Includes the following steps: S1. Machining multiple branch joint holes on the carbon steel water distribution main pipe, turning the edges of the branch joint holes outward to form an annular flange, and degreasing and removing oxides from the inner circumferential surface of the annular flange and the outer circumferential surface of the copper branch pipe insertion section to obtain the pretreated carbon steel water distribution main pipe and the pretreated copper branch pipe. S2. Apply a brazing choke agent to the non-brazing area of the pretreated copper branch pipe insertion section, insert multiple pretreated copper branch pipes into the corresponding annular flanges respectively, retain the annular capillary gap between the pretreated copper branch pipe insertion section and the annular flanges, and apply brazing filler metal to the outer end of the annular flanges to obtain the water distributor assembly to be brazed. S3. The water distributor assembly to be brazed is dried at low temperature and degummed at medium temperature to obtain a dried and degummed water distributor assembly. S4. First, replace the atmosphere in the mesh belt continuous brazing furnace with nitrogen, then introduce a hydrogen-nitrogen mixed protective gas, place the dry glue removal water distributor assembly on the mesh belt in the furnace, and transport it through the preheating zone, reduction and activation zone, brazing filling zone and uniform temperature forming zone in sequence to obtain the brazed water distributor assembly. S5. The brazed water distributor assembly is sent into the protective cooling zone of the mesh belt continuous brazing furnace and cooled in a hydrogen-nitrogen mixed protective atmosphere. After exiting the furnace, a liquid-cooled pipeline water distributor is obtained.
2. The welding process for the liquid-cooled pipeline distributor according to claim 1, characterized in that, In step S1, the annular flange extends 2-5 mm outward from the outer side of the carbon steel water distribution main pipe along the axial direction of the branch joint hole, and the distance between the outer end of the annular flange and the inner wall of the carbon steel water distribution main pipe along the axial direction of the branch joint hole is 5-10 mm.
3. The welding process for the liquid-cooled pipeline distributor according to claim 1, characterized in that, In step S1, the inner circumferential surface of the annular flange is acid-washed with a hydrochloric acid solution with a mass concentration of 5% to 10% for 1 to 3 minutes, and then sequentially washed with water, neutralized, rinsed with deionized water and dried; the outer circumferential surface of the copper branch pipe insertion section is acid-washed with a sulfuric acid solution with a mass concentration of 5% to 10% for 1 to 3 minutes, and then sequentially washed with water, rinsed with deionized water and dried.
4. The welding process for the liquid-cooled pipeline manifold according to claim 1, characterized in that, In step S2, the brazing throttling agent is a boron-based brazing throttling agent, the non-brazing area is an annular region with a width of 1-3 mm, and the non-brazing area is 0.5-1.5 mm away from the inner end of the annular capillary gap; after applying the brazing throttling agent, it is dried at 60-90℃ for 5-15 min.
5. The welding process for the liquid-cooled pipeline distributor according to claim 2, characterized in that, In step S2, the gap between the outer circumferential surface of the pretreated copper branch pipe insertion section and the inner circumferential surface of the annular flange is 0.05 to 0.15 mm on one side, and the end of the pretreated copper branch pipe extends into the interior of the carbon steel water distribution main pipe by 1 to 3 mm.
6. The welding process for the liquid-cooled pipeline distributor according to claim 5, characterized in that, In step S2, the solder is a copper-manganese-nickel solder paste, and the solidus temperature of the solder is 900-1000℃. The solder paste is continuously applied around the circumference of the pretreated copper branch pipe at the outer end of the annular flange to form an annular solder strip.
7. The welding process for the liquid-cooled pipeline manifold according to claim 1, characterized in that, In step S3, the low-temperature drying temperature is 80-110℃ and the time is 10-30 min; the medium-temperature debinding temperature is 180-250℃ and the time is 5-15 min.
8. The welding process for the liquid-cooled pipeline manifold according to claim 1, characterized in that, In step S4, nitrogen is first introduced until the residual oxygen content in the mesh belt continuous brazing furnace is less than 100 ppm, and then a hydrogen-nitrogen mixed protective gas with a hydrogen gas fraction of 5% to 25% is introduced until the residual oxygen content in the furnace does not exceed 10 ppm and the dew point of the hydrogen-nitrogen mixed protective gas is not higher than -40°C.
9. The welding process for the liquid-cooled pipeline distributor according to claim 6, characterized in that, In step S4, the running speed of the mesh belt inside the furnace is 220-300 mm / min; the temperature of the preheating zone is 750-850℃; the temperature of the reduction and activation zone is 880-950℃; the temperature of the brazing and filling zone is 1000-1030℃; and the temperature of the uniform forming zone is 980-1010℃.
10. The welding process for the liquid-cooled pipeline manifold according to claim 1, characterized in that, In step S5, before the temperature of the brazing filler metal drops below its solidus temperature, a hydrogen-nitrogen mixed protective gas is continuously introduced into the protective cooling zone. After the brazed water distributor assembly is taken out of the furnace, it undergoes surface cleaning, internal rinsing, weld appearance inspection, internal channel inspection, and sealing performance testing in sequence. The sealing performance testing pressure is not less than 1.5 times the design working pressure of the liquid-cooled pipeline water distributor.