A method for beveling titanium composite sheet / tube sheet

By employing layered positioning and zoned differentiated cutting processes, combined with low-speed precision machining and passivation polishing, the problems of dissimilar metal cutting interference and low precision in the beveling of titanium composite plates and tubes have been solved, achieving high-precision, damage-free embedded assembly and improving the sealing performance and structural stability of the equipment.

CN123103322APending Publication Date: 2026-11-17LONGHUA TECHNOLOGY GROUP (LUOYANG) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611477995.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing titanium composite plate and tube beveling processes suffer from problems such as dissimilar metal cutting and mixing, titanium alloy coating damage, low beveling accuracy, poor fit of embedded assembly, and insufficient welding reliability, which cannot meet the precision assembly and safe operation requirements of high-end pressure vessel equipment.

Method used

By employing layered positioning and zoned differentiated cutting processes, combined with low-speed, small-feed precision machining, constant-temperature cooling protection, and progressive passivation polishing, a stepped composite bevel is designed to be compatible with embedded assemblies. This, along with precise shaping processes, ensures machining accuracy and structural stability.

Benefits of technology

It achieves high-precision, non-destructive machining of titanium composite plate and tube bevels, improves welding reliability and equipment sealing performance, reduces rework rate, and is compatible with stainless steel housing embedded assembly structures to meet the precision assembly requirements of high-end equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103322A_ABST
    Figure CN123103322A_ABST
Patent Text Reader

Abstract

This invention discloses a beveling method for titanium composite plate tube sheets, belonging to the field of pressure vessel composite component processing technology. This invention employs an integrated processing technology encompassing layered precise positioning, differentiated cutting in different zones, low-speed cooling protection, and precision shaping. First, the titanium composite plate tube sheet is marked and positioned to separate the substrate and cladding areas, distinguishing the cutting areas of the stainless steel base layer and the titanium alloy cladding. Then, through multiple steps including rough machining to reserve machining allowance, layered precision machining, beveling passivation protection, and assembly adaptation shaping, the beveling of the tube sheet's outer edge is completed. This invention effectively avoids the problem of mixing dissimilar metals like titanium and steel during cutting, eliminates defects such as scratches, peeling, and oxidation burns in the titanium alloy cladding, significantly improves the dimensional accuracy, flatness, and roughness accuracy of the beveling, adapts to the embedded assembly structure of the tube sheet, and significantly improves the assembly fit, welding sealing, and structural stability of the tube sheet and the stainless steel shell. It boasts a high processing qualification rate and is suitable for industrial mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of pressure vessel composite component processing technology, specifically relating to a beveling processing method for titanium composite plate tube sheets, applicable to precision beveling processing scenarios where titanium-steel composite plate tube sheets are embedded and assembled with stainless steel shells in chemical, nuclear power, and heat exchange equipment. Background Technology

[0002] Titanium composite tube sheets are core pressure-bearing components of high-end pressure vessels and heat exchangers. They are formed by explosive bonding of a stainless steel base layer and a titanium alloy cladding, combining the structural strength and weldability of stainless steel with the corrosion resistance and high-temperature resistance of titanium alloy. They are widely used in equipment operating under highly corrosive media conditions. In equipment assembly structures, titanium composite tube sheets are often installed using an embedded method, integrally fixed inside the stainless steel shell. The outer edge of the tube sheet and the inner wall of the stainless steel shell are sealed and rigidly connected through bevel welding. The machining accuracy and forming quality of the bevel directly determine the overall sealing performance, structural strength, and service life of the equipment.

[0003] Currently, most existing beveling processes for titanium composite plates and tubes employ a one-piece integral cutting method, which has several technical drawbacks: First, titanium alloy and stainless steel are dissimilar metals with vastly different cutting parameters and performance. Integral cutting easily leads to stainless steel debris becoming embedded in the titanium alloy cladding surface and titanium alloy burrs adhering to the base layer, resulting in defects such as slag inclusions, porosity, and cracks in subsequent welding, severely impacting weld quality. Second, conventional high-speed cutting easily causes localized overheating of the titanium alloy cladding, resulting in oxidation burn-off, coarse grains, and surface hardening. First, the existing processing technology is not adapted to the design of the bevel shape for the embedded assembly structure. The bevel angle and allowance are not uniform, and the gap between the tube sheet and the stainless steel shell is uneven, making assembly difficult and resulting in poor sealing performance. Second, the processing process lacks a layered protection and precise positioning mechanism, which easily leads to over-cutting and under-cutting problems. The bevel size accuracy and flatness are difficult to meet the standards, resulting in a low product processing qualification rate and a high rework rate, which cannot meet the precision assembly and safe operation requirements of high-end pressure vessel equipment.

[0004] In summary, existing beveling methods for titanium composite plates and tubes have technical drawbacks such as interference from cutting dissimilar metals, easy damage to the composite layer, low beveling accuracy, poor assembly adaptability, and insufficient processing stability. There is an urgent need for a targeted precision beveling process that can adapt to the assembly conditions of titanium composite plates and tubes with embedded stainless steel shells, and ensure processing quality and assembly performance. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a beveling method for titanium composite plate tubes, which solves the problems of dissimilar metal cutting and doping, titanium alloy coating damage, low beveling accuracy, poor fit of embedded assembly, and insufficient welding reliability in the existing process. It achieves high-precision, damage-free, and standardized processing of titanium composite plate tube beveling, adapts to the embedded assembly structure of stainless steel shell, and improves the overall sealing performance and structural stability of the equipment.

[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution.

[0007] A beveling method for a titanium composite plate / tube sheet, wherein the titanium composite plate / tube sheet is formed by explosive bonding of a stainless steel base layer and a titanium alloy cladding layer, and the beveling method includes the following steps: S1. Workpiece Pretreatment and Layer Positioning: Select qualified titanium composite tube sheets, which are formed by explosive bonding of stainless steel base and titanium alloy coating. Clean the oxide scale, oil stains and burrs on the outer edge of the tube sheet. Use laser scribing equipment to mark the outer edge of the tube sheet in layers. The layer scribing adopts dual reference positioning of the tube sheet end face and the outer circumference to accurately divide the stainless steel base cutting area, the titanium alloy coating cutting area and the beveling area. Mark the beveling reference line and the machining allowance boundary to ensure that the layer boundary error is ≤0.02mm. After marking, clamp and fix the tube sheet on the CNC machining tool, and correct the workpiece levelness and coaxiality. The clamping and positioning accuracy is ≤0.01mm.

[0008] S2. Zoned Rough Machining Allowance: Based on the layered marking areas, differentiated cutting parameters are used for beveling rough machining to adapt to the cutting characteristics of the stainless steel base and titanium alloy coating respectively. The stainless steel base is machined using conventional cutting parameters, while the titanium alloy coating is machined using low-speed, small-feed cutting parameters. During rough machining, water-based extreme pressure cutting fluid is continuously sprayed to control the temperature, keeping the workpiece cutting temperature ≤60℃. After rough machining, a uniform finishing allowance of 0.3-0.5mm is reserved for the entire beveling, removing excess base material from the outer edge, initially forming the basic outline of the beveling, and ensuring that the rough machined surface is free of obvious steps and chipping defects.

[0009] S3. Layered Precision Machining: Replace with high-precision carbide cutting tools to perform layered precision machining on the stainless steel base bevel and the titanium alloy cladding bevel, strictly distinguishing the cutting paths to avoid cross-cutting of dissimilar metals; during the finishing process, the cutting speed of the titanium alloy cladding is controlled at 15-20m / min, the feed rate at 0.05-0.08mm / r, and the depth of cut at 0.1-0.15mm / cut; the cutting speed of the stainless steel base is controlled at 35-40m / min, and the feed rate at 0.1-0.12mm / r; after finishing, a stepped composite bevel adapted for embedded assembly is formed, with a total bevel angle of 30°-45°, ensuring that the dimensional error of each area of ​​the bevel is ≤0.03mm and the surface roughness Ra≤1.6μm; S4. Bevel passivation and protection treatment: After finishing, use fine-grained diamond polishing pads to passivate and polish the bevel edges and layer junctions to remove cutting burrs and sharp edges. The passivation radius is controlled at 0.2-0.3mm. After polishing, wipe the bevel surface with anhydrous ethanol to remove cutting debris and oil. After air drying, spray an anti-oxidation protective agent on the titanium alloy coated bevel surface to form a uniform protective film and prevent oxidation corrosion before subsequent assembly and welding. S5. Assembly Adaptation, Shaping, and Inspection: Based on the dimensional requirements of the embedded assembly in the stainless steel shell, the formed bevel is slightly modified to correct the coaxiality and flatness of the bevel, ensuring that the assembly gap between the outer edge bevel of the tube sheet and the inner wall of the stainless steel shell is uniform, with the single-sided gap controlled within 0.05-0.1mm; finally, a full-item inspection instrument is used to inspect the bevel angle, dimensional accuracy, surface roughness, and flatness. After passing the inspection, the beveling process is completed.

[0010] In step S1, the total thickness of the titanium composite plate tube is 20-80mm, the thickness of the titanium alloy cladding is 2-5mm, and the thickness of the stainless steel base layer is 18-75mm; the layer marking adopts dual reference positioning of the tube end face and the outer circumferential surface.

[0011] In step S2, the water-based extreme pressure cutting fluid is prepared in the following ratio: deionized water: extreme pressure additive: rust inhibitor = 85:12:3, and the cutting fluid injection pressure is 0.3-0.5 MPa.

[0012] In step S3, the finishing tool is a carbide tool with a tip radius of 0.1 mm. Before machining, the tool dynamic balance is corrected and the speed error is ≤1%.

[0013] In step S3, the total angle of the formed stepped composite bevel is 30°-45°. The titanium alloy cladding side is a sloping bevel, and the stainless steel base side is a straight-edge transition bevel. The layer transition position is smoothly connected without step misalignment. After finishing, the bevel size error is ≤0.03mm, and the surface roughness Ra is ≤1.6μm. The joint section of the titanium alloy cladding and the stainless steel base has a sawtooth joint structure. The cumulative milling depth of the titanium alloy cladding is 0.5-1mm greater than the thickness of the titanium alloy cladding.

[0014] In step S4, the passivation polishing adopts a step-by-step grinding process, using 800-grit, 1200-grit, and 2000-grit diamond polishing pads in sequence.

[0015] Compared with the prior art, the present invention has the following significant advantages: 1. This invention adopts a layered positioning and zoned differentiated cutting process, matching exclusive processing parameters to the dissimilar metal cutting characteristics of stainless steel base and titanium alloy coating, completely solving the problems of metal chip mixing and cross wear caused by traditional integral cutting, avoiding welding slag inclusions and crack defects from the source, and greatly improving the reliability of bevel welding.

[0016] 2. This invention effectively controls the cutting temperature of the titanium alloy coating by using low-speed, small-feed precision machining combined with constant-temperature cooling protection, thus eliminating problems such as oxidation and burn-off of the titanium alloy coating, coarse grains, and surface hardening. At the same time, it avoids peeling and warping of the composite layer interface, and fully preserves the composite structural performance and corrosion resistance of the titanium composite plate.

[0017] 3. The present invention is designed with a stepped composite bevel adapted to embedded assembly. Combined with a precise shaping process, it ensures uniform assembly gap and high fit between the tube sheet and the stainless steel shell, completely solving the problems of uneven assembly gap, difficult alignment and poor sealing of traditional bevel assembly, and significantly improving the embedded assembly accuracy and overall sealing performance of the equipment.

[0018] 4. This invention integrates laser precision positioning, layered fine processing, step-by-step passivation and polishing, and full-item precision testing into a single process. The bevel size error is ≤0.03mm, the surface roughness Ra is ≤1.6μm, the flatness and coaxiality accuracy are greatly improved, the product processing qualification rate can reach more than 99%, the rework rate is significantly reduced, and it is suitable for industrial mass production.

[0019] 5. The process steps of this invention are standardized and highly controllable. No complex special equipment is required. Precision machining can be achieved by relying on conventional CNC machining equipment. The processing efficiency is high and the production cost is low. It is adaptable to the beveling processing of titanium composite plates and tubes of different specifications and has strong versatility. Attached Figure Description

[0020] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.

[0021] Figure 1 This is a flowchart of the overall processing technology of the present invention; Figure 2 This is a schematic diagram of the stepped composite bevel cross-section structure of the present invention.

[0022] In the diagram, 1-stainless steel base layer; 2-titanium alloy cladding; 3-titanium layer bevel; 4-steel layer straight edge transition bevel; 5-layer transition smooth area. Detailed Implementation

[0023] The technical solution of the present invention will be clearly and completely described below with reference to specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example 1

[0024] This embodiment provides a beveling method for titanium composite plate tubes, specifically for processing titanium composite plate tubes with a total thickness of 27mm (24mm stainless steel base and 3mm titanium alloy cladding). A structural schematic diagram of the titanium composite plate tube is shown below. Figure 2 As shown, the titanium composite plate tube is formed by explosive bonding of a stainless steel base layer 1 and a titanium alloy cladding layer 2. The joint cross-section of the titanium alloy cladding layer 2 and the stainless steel base layer 1 has a sawtooth joint structure. The end face of the titanium alloy cladding layer 2 is processed into a titanium layer bevel 3, and the end face of the stainless steel base layer is processed into a steel layer straight edge transition bevel 4. The connection between the two is a layered transition smooth zone 5.

[0025] The process flow diagram of the beveling method is as follows: Figure 1 As shown, the specific steps are as follows: S1. Workpiece pretreatment and layer positioning: Clean the oil and oxide scale on the outer edge of the tube sheet. Use a laser scribing device to accurately divide the stainless steel base and titanium alloy coating cutting areas with the tube sheet end face and outer circumferential surface as dual references. The layer boundary error is controlled within 0.02mm. Clamp the tube sheet on a CNC milling machine and correct the levelness and coaxiality. The clamping and positioning accuracy is 0.01mm.

[0026] S2. Zoned Roughing with Allowance: Differentiated cutting is employed in zones. For the stainless steel base layer, the cutting speed is 30 m / min and the feed rate is 0.1 mm / r. For the titanium alloy coating, the cutting speed is 12 m / min and the feed rate is 0.06 mm / r. Water-based extreme pressure cutting fluid is sprayed throughout the process, with a ratio of deionized water: extreme pressure additive: rust inhibitor = 85:12:3, a spray pressure of 0.4 MPa, and the cutting temperature controlled to ≤60℃. After roughing, a uniform 0.4 mm finishing allowance is left to form the basic bevel contour. The extreme pressure additive is a sulfur-free and chlorine-free borate ester.

[0027] S3. Layered Precision Machining: Replace the carbide cutting tool with a tip radius of 0.1mm and correct the tool dynamic balance; for the titanium alloy cladding, use a cutting speed of 18m / min, feed rate of 0.06mm / r, and single cutting depth of 0.12mm; for the stainless steel base layer, use a cutting speed of 38m / min, feed rate of 0.11mm / r, and single cutting depth of 0.15mm; layered cutting to form a 35° stepped composite bevel, with the titanium alloy cladding having a beveled edge and the steel layer having a straight edge transition bevel, resulting in a smooth layer transition. The milling depth of the titanium alloy cladding is 0.8mm greater than the thickness of the titanium alloy cladding. The dimensional error after machining is ≤0.03mm, and the surface roughness Ra is ≤1.6μm.

[0028] S4. Bevel passivation and protection treatment: The bevel is passivated and polished step by step using 800-mesh, 1200-mesh, and 2000-mesh diamond polishing pads, with a passivation radius of 0.25mm at the bevel edge. The surface is cleaned by wiping with anhydrous ethanol, and after air drying, a titanium alloy-specific anti-oxidation protective agent is sprayed to form a uniform protective film.

[0029] S5. Assembly, Fitting, Shaping, and Inspection: Perform minor shaping according to the embedded dimensions of the stainless steel shell, controlling the assembly gap on one side to 0.08mm; ensure that the bevel angle, dimensions, flatness, and roughness all meet the standards, and complete the processing. Example 2

[0030] This embodiment focuses on beveling a titanium composite plate tube with a total thickness of 60mm (56mm stainless steel base and 4mm titanium alloy cladding). The processing steps are the same as in Embodiment 1, with the following differences in parameter settings: roughing allowance of 0.5mm, finishing beveling angle of 40°, cutting speed of titanium alloy cladding of 20m / min, single-sided assembly gap controlled at 0.1mm, passivation arc radius of 0.3mm, and milling depth of titanium alloy cladding 0.9mm greater than the thickness of titanium alloy cladding. The remaining parameters are consistent with those in Embodiment 1.

[0031] Comparative example (traditional integral cutting process) The same-specification titanium composite plate tube was beveling using a traditional high-speed integral cutting process, without layered or zoned cutting, low-temperature cooling protection, or passivation and shaping procedures. Post-processing inspection results showed: beveling dimensional error of 0.1-0.2mm, surface roughness Ra greater than 3.2μm, slight oxidation discoloration and debris contamination on the titanium alloy cladding surface, minor peeling marks at the composite layer edges, uneven assembly gap between the tube and stainless steel shell (maximum gap deviation 0.3mm), and trace slag inclusions after welding. The product qualification rate was only 85%. Comparison of Implementation Results

[0032] The bevels processed in Embodiments 1 and 2 of this invention are free from oxidation, impurities, and peeling defects. Their dimensional and surface precision are far superior to those of traditional processes. The assembly gaps are uniform, the inlay fit is high, and there are no defects such as slag inclusions, porosity, or cracks after welding. The product qualification rate is over 99%, which fully meets the precision machining and safe use requirements for inlay assembly of high-end pressure vessels.

[0033] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A method for beveling a titanium clad plate pipe plate, characterized by: The titanium composite plate / tube is formed by explosive bonding of a stainless steel base layer and a titanium alloy cladding. The beveling method includes the following steps: S1. Workpiece pretreatment and layered positioning: Clean impurities from the outer surface of the titanium composite plate tube sheet, mark the stainless steel base layer cutting area, titanium alloy cladding cutting area and beveling area by laser scribing, correct the tube sheet clamping accuracy, and complete the positioning and fixing. S2. Sectional rough machining allowance: Different cutting parameters are used for beveling rough machining of stainless steel base and titanium alloy cladding, with cooling and temperature control throughout the process. After rough machining, a uniform finishing allowance is reserved to form the basic outline of the beveling. S3, Layered Precision Machining: Using high-precision carbide tools, the stainless steel base layer and titanium alloy cladding bevel are precision machined in layers and sections to form a stepped composite bevel that is compatible with embedded assembly. S4. Bevel passivation and protection treatment: Passivate and polish the bevel edge and the junction of layers, clean the surface and spray an anti-oxidation protective agent. S5. Assembly Adaptation, Shaping and Inspection: The bevel is slightly modified according to the assembly requirements of the stainless steel shell, the assembly gap is controlled, and the processing is completed after all items pass the inspection.

2. The method of beveling a pipe plate of a titanium clad plate according to claim 1, characterized in that: In step S1, the total thickness of the titanium composite plate tube is 20-80mm, the titanium alloy coating thickness is 2-5mm, and the stainless steel base layer thickness is 18-75mm; the layer marking adopts dual reference positioning of the tube end face and the outer circumferential surface, the layer boundary error is ≤0.02mm, and the tube clamping positioning accuracy is ≤0.01mm.

3. The method of claim 1, wherein the method further comprises: beveling the titanium composite plate pipe plate. In step S2, the roughing process uses zoned differentiated cutting parameters, the stainless steel base layer uses conventional cutting parameters, and the titanium alloy coating uses small feed rate cutting parameters. During the cutting process, water-based extreme pressure cutting fluid is sprayed to control the temperature, and the workpiece cutting temperature is controlled to ≤60℃. After roughing, a finishing allowance of 0.3-0.5mm is reserved.

4. The method of claim 3, wherein the method further comprises: beveling the titanium composite plate pipe plate. The water-based extreme pressure cutting fluid has a mixing ratio of deionized water: extreme pressure additive: rust inhibitor = 85:12:3, and the cutting fluid injection pressure is 0.3-0.5 MPa.

5. The method of claim 1, wherein the method further comprises: beveling the titanium composite plate pipe plate. In step S3, the finishing tool is a carbide tool with a tip radius of 0.1 mm. Before machining, the tool dynamic balance is corrected and the speed error is ≤1%. The cutting speed of the titanium alloy coating is 15-20 m / min, the feed rate is 0.05-0.08 mm / r, and the depth of cut is 0.1-0.15 mm. The cutting speed of the stainless steel base is 35-40 m / min, and the feed rate is 0.1-0.12 mm / r.

6. The method of beveling a titanium clad pipe panel according to claim 1, wherein: In step S3, the total angle of the formed stepped composite bevel is 30°-45°. The titanium alloy cladding side is a sloping bevel, and the stainless steel base side is a straight-edge transition bevel. The layer transition position is smoothly connected without step misalignment. After finishing, the bevel size error is ≤0.03mm, and the surface roughness Ra is ≤1.6μm. The joint section of the titanium alloy cladding and the stainless steel base has a sawtooth joint structure. The cumulative milling depth of the titanium alloy cladding is 0.5-1mm greater than the thickness of the titanium alloy cladding.

7. The method of beveling a titanium clad pipe panel according to claim 1, wherein: In step S4, the passivation polishing adopts a step-by-step grinding process, using 800-grit, 1200-grit, and 2000-grit diamond polishing pads in sequence, and controlling the passivation arc radius of the bevel edge to be 0.2-0.3mm.

8. The method of claim 1, wherein the method further comprises: beveling the titanium composite plate pipe plate. In step S5, the single-sided assembly gap between the outer edge bevel of the tube sheet and the inner wall of the stainless steel shell is controlled at 0.05-0.1mm. The bevel angle, dimensional accuracy, flatness and surface roughness are fully tested by a coordinate measuring machine and a roughness tester.