A continuous production method for butt-welded aluminum-plastic composite pipes via mechanical pressing and anchoring, and the pipe material.

By employing a mechanical pressing and anchoring method in the production of aluminum-plastic composite pipes, utilizing the physical anchoring structure of anchor blind holes and micro-clamps, and combining segmented heating and cooling processes, the problems of complex equipment, high energy consumption, VOC emissions, and adhesive layer aging in existing technologies have been solved. This has achieved high-strength aluminum-plastic interface bonding, improving production efficiency and pipe durability.

CN123104130APending Publication Date: 2026-11-17ZHEJIANG BEIDELUO PIPELINE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611146903.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing butt-welded aluminum-plastic composite pipe production process has problems such as complex equipment, high energy consumption, VOC emissions, adhesive layer aging, and delamination due to hot and cold cycles, making it difficult to meet the long-term durability requirements of high-end fluid transportation pipes.

Method used

A mechanical compression anchoring method is adopted, which involves processing anchoring blind holes and micro-blocks on the surface of aluminum strips, combined with segmented heating, radial constant pressure and gradient cooling processes, to achieve high-strength physical anchoring of the aluminum-plastic interface, eliminating the need for hot melt adhesive bonding.

Benefits of technology

It improves production continuity and stability, reduces scrap rate, enhances peel strength, ensures the gas barrier properties of the aluminum layer, extends pipe life, meets environmental protection requirements, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104130A_ABST
    Figure CN123104130A_ABST
Patent Text Reader

Abstract

This invention discloses a continuous production method and pipe material for butt-welded aluminum-plastic composite pipes via mechanical pressing and anchoring. The invention sequentially executes the following steps along the pipe's travel direction: S1: Inner layer plastic pipe extrusion and sizing process, using a single-screw extruder to extrude the inner layer plastic pipe to be coated, followed by vacuum sizing and cooling to ensure the pipe's outer diameter accuracy and roundness, and then uniformly traction and forward transport; S2: Aluminum strip anchoring blind hole prefabrication process, where multiple anchoring blind holes are formed on the surface of the aluminum strip facing the inner layer plastic pipe. The longitudinal cross-section of each anchoring blind hole is trapezoidal, wider on the inside and narrower on the outside, and the inner wall of the trapezoidal cavity is equipped with micro-blocks. This invention employs three-stage gradient cooling to achieve step-by-step curing and shrinkage of the plastic, utilizing the plastic's own shrinkage characteristics to enhance the anchoring effect. This ensures that the pipe material does not delaminate or detach after 10,000 cycles of hot and cold cycling from 20℃ to 95℃, and also reduces the pipe's oxygen permeability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aluminum-plastic composite pipe manufacturing technology, specifically to a continuous production method and pipe material for butt-welded aluminum-plastic composite pipes via mechanical pressing and anchoring. Background Technology

[0002] Butt-welded aluminum-plastic composite pipes are multi-layered composite pipes formed by argon-arc butt welding of aluminum strips into an aluminum skeleton, with inner and outer plastic layers. Due to the continuous, seamless aluminum layers, high roundness, excellent oxygen barrier properties, and ability to withstand high internal pressure, they have become the mainstream development direction for high-end fluid transportation pipes in fields such as underfloor heating, radiant heating, building hot and cold water supply, and gas transmission. However, existing butt-welded aluminum-plastic composite pipe manufacturing processes and corresponding pipe materials have revealed a series of fundamental defects during long-term service, severely restricting further performance improvements and the expansion of their application range.

[0003] 1. The currently prevalent "two-step" production process in the industry requires coating a layer of hot melt adhesive (such as maleic anhydride-grafted polyethylene) between the aluminum layer and the inner and outer plastic layers. The interlayer bonding is achieved through the adhesive strength of the adhesive layers. This process requires multiple sets of specialized equipment for inner and outer layer coating, as well as drying. The equipment is complex, occupies a large area, and consumes a lot of energy. More importantly, the hot melt adhesive generates volatile organic compounds (VOCs) during production, posing a significant environmental burden. Under long-term alternating hot and cold conditions or high temperature and humidity, the hot melt adhesive is prone to oxidation, aging, and hydrolysis, leading to a continuous decline in adhesive strength. This results in bulging, delamination, and even leakage in the pipes, significantly shortening their service life and failing to meet the long-term durability requirements of high-end piping systems.

[0004] 2. Some existing technologies have through holes that penetrate the thickness of the aluminum strip, intending to allow the inner and outer plastic layers to melt and connect at the through holes to enhance the interlayer bonding. However, the through holes directly penetrate the aluminum layer, destroying the overall gas barrier integrity of the aluminum layer, resulting in a significant increase in the oxygen permeability of the pipe and losing the core oxygen barrier advantage of aluminum-plastic composite pipes. At the same time, such solutions still rely on the bonding effect of hot melt adhesive and have not achieved a truly pure physical composite. The problem of hot melt adhesive aging and delamination still cannot be completely eliminated.

[0005] 3. In existing processes for laminating plastic and aluminum layers, compressed air is typically injected into the tube to expand the inner plastic layer, thereby adhering to the inner wall of the aluminum layer and allowing the plastic to penetrate the hot melt adhesive layer. This process requires sealing plugs at both ends of the tube, and during production, frequent failures such as plug leakage and rapid wear of seals occur. This not only causes production interruptions and high scrap rates, but also the fluctuation of inflation pressure directly affects the uniformity of the composite, making it impossible to achieve high-speed, stable, continuous mass production.

[0006] 4. Regardless of whether through holes are added, the interlayer bonding strength of existing butt-welded aluminum-plastic composite pipes all originates from the chemical adhesive force of hot melt adhesive. Under long-term thermal cycling conditions of 20℃-95℃, the thermal expansion coefficients of plastic and aluminum are significantly different, and thermal stress is repeatedly generated at the interface. In addition, the performance of the adhesive layer itself degrades over time, and the bonding strength shows a significant downward trend. After the peel strength decreases, it is very easy to cause interlayer separation, which cannot meet the performance requirements of high-end application fields for pipes to be unfailed after tens of thousands of thermal cycles. Summary of the Invention

[0007] The purpose of this invention is to provide a continuous production method and pipe material for butt-welded aluminum-plastic composite pipes via mechanical pressing and anchoring, in order to solve the problems mentioned in the background art.

[0008] To achieve the above objectives, the present invention provides the following technical solution: a continuous production method and pipe material for mechanically pressing and anchoring butt-welded aluminum-plastic composite pipes, wherein the following steps are performed sequentially along the pipe's travel direction:

[0009] S1: Inner layer plastic tube extrusion and sizing process, a single screw extruder is used to extrude the inner layer plastic tube to be coated, and vacuum sizing and cooling are used to ensure the accuracy of the outer diameter and roundness of the tube, and it is pulled forward at a uniform speed;

[0010] S2: Aluminum strip anchor blind hole prefabrication process, multiple anchor blind holes are formed on the side surface of the aluminum strip facing the inner plastic tube. The longitudinal cross section of the anchor blind hole is a trapezoid with a wider inner section and a narrower outer section. The inner wall of the trapezoidal cavity is provided with micro-blocks.

[0011] S3: Aluminum strip rolling and butt welding process, the aluminum strip with pre-made anchor blind holes is wrapped around the outer wall of the inner plastic tube, and the butt joint of the aluminum strip is welded to form a sealed aluminum tube layer.

[0012] S4: Segmented induction heating process, which heats only the outer wall of the aluminum tube layer, so that the surface of the inner plastic tube layer is heated to a viscous flow state;

[0013] S5: Radial constant pressure clamping anchoring process, a constant radial surface pressure is applied to the pipe by a clamping mechanism arranged around the circumference of the pipe, so that the inner plastic layer in a viscous flow state fills into the anchoring blind hole;

[0014] S6: The three-stage gradient cooling self-locking process causes the plastic filled in the blind hole to cool and shrink in stages, locking into the trapezoidal blind hole to form a secondary self-locking anchor.

[0015] S7: Outer plastic co-extrusion coating process, an outer barrier plastic layer is coated on the outer wall of the cooled and shaped pipe (4).

[0016] S8: The online inspection process for traction winding, with online diameter measurement, wall thickness, and peel strength sampling stations to monitor product quality in real time, and the final finished product is automatically wound up.

[0017] By adopting the above technical solution, the traditional process of butt-welding aluminum-plastic pipes relying on hot melt adhesive bonding is completely abandoned, eliminating the risks of adhesive layer aging, hydrolysis, and delamination due to hot and cold cycles from the root. The trapezoidal blind hole with a wider inner diameter and a narrower outer diameter, combined with the micro-blocks on the inner wall, forms a natural mechanical self-locking cavity. Combined with the synergistic process of segmented heating, radial constant pressure pressing, and gradient cooling, high-strength physical anchoring of the aluminum-plastic interface can be achieved without the need for air-filled sealing inside the pipe. Production continuity is improved by more than 70%, the scrap rate is reduced by 60%, and there is no VOC emission. The environmental protection and production stability are significantly better than existing technologies.

[0018] Preferably, the depth of the anchoring blind hole is 80-150 μm, the height of the micro-block is 5-20 μm, and the distribution density of the anchoring blind hole is 250-300 holes / cm².

[0019] By adopting the above technical solution, the depth of the anchoring blind hole and the height of the micro-block are adapted to the plastic flow filling characteristics: if the depth is less than 80μm, the anchoring force is insufficient, and if it is greater than 150μm, it will easily weaken the strength of the aluminum strip itself; the height of the micro-block is controlled within the range of 5-20μm, which can form an effective anti-peeling resistance without hindering the plastic filling; the distribution density of 250-300 blocks / cm² ensures the anchoring strength while avoiding the decrease in oxygen barrier performance of the aluminum layer due to too many blind holes, thus taking into account both mechanical properties and functional characteristics.

[0020] Preferably, the opening width of the anchoring blind hole is 30-50μm, the bottom width of the anchoring blind hole is 80-100μm, the depth of the blind hole is preferably 120μm, and the height of the micro-block is preferably 10μm.

[0021] By adopting the above technical solution, the inner width and outer narrowness of the dimensions form the optimal wedge angle. After the plastic filling cools, the structure with the bottom wider than the opening naturally restricts the plastic from coming out. Combined with the 10μm high micro-blocks, a double anchoring is formed: the wedge structure prevents the aluminum-plastic layer from slipping as a whole, and the micro-blocks inhibit local micro-area peeling. Under these optimized parameters, the peel strength of the finished product can reach 42-46 N / cm, which is more than 30% higher than that of traditional adhesive pipes.

[0022] Preferably, in the segmented induction heating process, the outer wall temperature of the aluminum tube layer is controlled at 130-160℃, and the surface temperature of the inner plastic tube is controlled at 120-135℃.

[0023] By adopting the above technical solution, at least two sets of independent temperature-controlled induction coils connected in series are used to target and heat the outer wall of the aluminum tube. The heat is conducted inward through the aluminum tube wall, avoiding overheating and degradation caused by direct heating of the plastic. The outer wall temperature of the aluminum tube at 130-160℃ can ensure that the inner plastic surface layer accurately enters the viscous flow range of 120-135℃, which not only has sufficient fluidity to fill blind holes, but also does not damage the crystal structure and mechanical properties of the inner plastic matrix, thus ensuring the long-term pressure resistance of the tube.

[0024] Preferably, the radial constant pressure tightening and anchoring process uses a high-temperature resistant elastomer pressure roller or a track to apply pressure in a 360° circumferential manner, and the radial surface pressure is controlled at 0.5-1.5 MPa in the radial constant pressure tightening and anchoring process.

[0025] By adopting the above technical solutions, the high-temperature resistant elastomer can buffer local pressure fluctuations, and the 360° circumferential pressure ensures that the plastic fills all blind holes evenly; the floating suspension drive structure compensates for the roundness deviation of the tube in real time, and within the preferred pressure range of 0.5-1.5MPa, the softened plastic can be fully squeezed into the trapezoidal blind holes and micro-block gaps, while avoiding excessive pressure that could cause deformation of the aluminum strip or damage to the inner plastic tube. The consistency of the anchoring structure molding reaches more than 99%.

[0026] Preferably, the three-stage gradient cooling self-locking process includes, in sequence: a high-temperature slow cooling stage, with the water temperature controlled at 80-100℃, used to release the internal stress of the composite interface; a medium-temperature stress release stage, with the water temperature controlled at 40-60℃, used for the initial curing of the plastic; and a room-temperature shaping stage, with the water temperature controlled at 20-30℃, used for the complete cooling and shrinkage of the plastic.

[0027] By adopting the above technical solution, the three-step cooling process is matched with the corresponding length design to achieve step-by-step controllable shrinkage of plastic: the high-temperature slow cooling section slowly releases the interfacial internal stress generated by extrusion, avoiding micro-cracks caused by sudden cooling; the medium-temperature section guides the plastic to initially shape, retaining the potential energy for subsequent shrinkage; the room-temperature section completes the final shrinkage, and the shrinkage characteristics of the plastic itself are used to further enhance the wedge-shaped locking effect. The secondary self-locking anchoring strength is increased by more than 15% compared with the single cooling, and there is no delamination after 10,000 cycles of hot and cold cycles from 20℃ to 95℃.

[0028] Preferably, in the synchronous traction and online detection winding process, the winding equipment is used to synchronize the winding speed with the traction mechanism of each process in the entire line, and the production speed is adjustable in the range of 0.3-0.9m / s; the aluminum strip anchor blind hole prefabrication process uses roll embossing or laser etching to process the anchor blind holes.

[0029] By adopting the above technical solutions, the entire line speed linkage avoids the stretching deformation or accumulation of wrinkles in the pipes. The wide speed range of 0.3-0.9m / s is suitable for the production of various specifications of pipes. Roll embossing is suitable for the mass continuous processing of conventional aluminum strips with a thickness of 0.4-0.5mm, with low cost and high efficiency. Laser etching is suitable for blind hole processing of high-precision, small-diameter pipes, with no mechanical contact damage and an accuracy of ±5μm. The two processes are suitable for different scenario requirements and have strong industrialization potential.

[0030] A butt-welded aluminum-plastic composite pipe includes an inner plastic matrix, an aluminum pipe anchoring layer, and an outer barrier plastic layer: the outer surface of the inner plastic matrix is ​​provided with an aluminum pipe anchoring layer, the inner wall of the aluminum pipe anchoring layer is provided with a plurality of anchoring blind holes evenly distributed, and the outer surface of the aluminum pipe anchoring layer is provided with an outer barrier plastic layer.

[0031] By adopting the above technical solution, the pipe adopts a three-layer composite structure. The aluminum pipe anchoring layer is formed by butt welding, which has good overall airtightness and excellent oxygen barrier performance. The aluminum-plastic interface has no hot melt adhesive interlayer and relies entirely on mechanical structure to achieve composite, which fundamentally avoids the failure risk caused by adhesive layer aging. It is suitable for fluid transportation scenarios with high requirements for durability and oxygen barrier, such as underfloor heating, water supply, and gas.

[0032] Preferably, the cross-section of the anchoring blind hole on the inner wall of the aluminum tube anchoring layer is trapezoidal with a larger inner diameter and a smaller outer diameter, and the inner wall has micro-blocks, and the inner plastic matrix is ​​partially embedded in the anchoring blind hole.

[0033] By adopting the above technical solution, the inner plastic layer embedded in the blind hole forms a wedge-tight fit with the trapezoidal cavity, and the micro-block further locks the position of the plastic, forming a double mechanical anchoring structure of "wedge and block". The interlayer bonding strength is high, and even if it is subjected to long-term cold and heat cycles or pressure fluctuations, there will be no delamination or bulging, thereby improving the service life of the pipe.

[0034] Preferably, the outer barrier plastic layer (4) contains EVOH barrier masterbatch, and the inner plastic matrix is ​​made of PE-RT or PEX modified plastic.

[0035] By adopting the above technical solutions, the inner layer of PE-RT or PEX modified plastic has excellent heat resistance, pressure resistance, and creep resistance, making it suitable for high-temperature hot water transportation scenarios. After adding EVOH barrier masterbatch to the outer layer, it forms a double oxygen barrier with the middle sealed aluminum layer. The overall oxygen permeability of the pipe is ≤0.18mg / (m²·d), which can effectively prevent oxidation and corrosion of metal valves, radiators and other components in the heating system, and extend the service life of the entire pipeline system.

[0036] Compared with the prior art, the beneficial effects of the present invention are:

[0037] 1. This continuous production method and pipe material for butt-welded aluminum-plastic composite pipes, which uses mechanical pressing and anchoring, eliminates the need for hot melt adhesive coating and related equipment throughout the entire process. This eliminates potential failures such as adhesive oxidation and aging, and hydrolysis delamination from the source. At the same time, the production process produces no volatile organic compounds (VOCs) from adhesives, significantly improving the workshop working environment and conforming to the trend of green manufacturing. It also reduces the production and processing costs of composite pipes. In addition, by eliminating the hot melt adhesive heating and drying process, the overall energy consumption of the production line is reduced by about 15%, resulting in outstanding comprehensive economic benefits.

[0038] 2. The continuous production method and pipe material for mechanically pressing and anchoring aluminum-plastic composite pipes involves prefabricating trapezoidal anchoring blind holes with a wider inner side and a narrower outer side on one side of the aluminum strip, and integrally forming micro-barbs (micro-clamping blocks) on the inner wall of the trapezoidal cavity, forming a dual physical anchoring mechanism of "wedge tightening and barbs": the softened plastic fully fills the blind hole under radial constant pressure, and after cooling and shrinking, the trapezoidal cavity with a larger inner side and a smaller outer side forms a natural wedge tightening and self-locking from a geometrical structure, effectively preventing the overall slippage of the aluminum-plastic layer; the micro-barbs provide multi-point anti-peeling resistance at the micro level, inhibiting the generation and expansion of local micro-area delamination. The synergistic effect of the dual protection mechanism improves the peeling strength.

[0039] 3. This continuous production method and pipe material for butt-welded aluminum-plastic composite pipes using mechanical pressing and anchoring involves applying pressure with an external high-temperature resistant elastomer pressure roller or track in a 360° circumferential manner. The pressing mechanism is equipped with a floating suspension servo or hydraulic drive structure, which can adapt to the outer diameter tolerance of the pipe and continuously maintain a constant radial surface pressure of 0.5-1.5MPa (preferably 0.8-0.9MPa). No internal sealing structure is required, which fundamentally eliminates the risk of air leakage. The production line can operate stably for a long time, reducing the scrap rate by more than 60%. The production speed can remain stable within the range of 0.3-0.9m / s, significantly improving mass production efficiency and product consistency.

[0040] 4. The continuous production method and pipe material for mechanical pressing and anchoring of butt-welded aluminum-plastic composite pipes adopt a three-stage gradient cooling process: "high temperature slow cooling → medium temperature stress relief → room temperature shaping". This process allows the plastic filled in the blind holes to cool down and shrink gradually. The high temperature slow cooling stage (80-100℃, preferably 90℃ / 5m) slowly releases the internal stress generated by extrusion at the composite interface, avoiding micro-cracks induced by sudden cooling. The medium temperature stress relief stage (40-60℃, preferably 50℃ / 4m) guides the plastic to initially solidify, retaining the shrinkage potential energy. The room temperature shaping stage (20-30℃, preferably 25℃ / 6m) allows the plastic to cool completely. By utilizing the thermal shrinkage characteristics of polyolefin materials, the tightness of the fit between the plastic and the trapezoidal blind holes is further strengthened, completing the secondary self-locking anchoring and improving the service life of the pipe material.

[0041] 5. The mechanical pressing and anchoring continuous production method and pipe material of this butt-welded aluminum-plastic composite pipe adopt a blind hole structure that does not penetrate the aluminum strip. After butt welding, the aluminum pipe layer remains a complete sealed shell, which fundamentally ensures the gas barrier function of the aluminum layer itself. Combined with the modified plastic layer with added EVOH barrier masterbatch on the outer layer, a double oxygen barrier of "sealed aluminum layer and EVOH oxygen barrier layer" is formed, which further extends the service life of the entire pipeline system. Attached Figure Description

[0042] Figure 1 This is a schematic diagram of the overall process flow of the continuous production method of the present invention;

[0043] Figure 2 This is a schematic diagram of the segmented arrangement of the three-segment gradient cooling unit of the present invention;

[0044] Figure 3 This is a perspective view of the composite pipe of the present invention;

[0045] Figure 4 This is an enlarged structural diagram of the trapezoidal anchorage blind hole cross-section of the present invention;

[0046] Figure 5 This is a schematic diagram of the cross-section of the aluminum tube and the inner plastic anchoring connection of the present invention;

[0047] Figure 6 This is a diagram showing the radial constant pressure tightening and anchoring pipe of the present invention.

[0048] In the diagram: 1. Inner plastic substrate; 2. Aluminum tube anchoring layer; 3. Anchoring blind hole; 4. Outer barrier plastic layer. Detailed Implementation

[0049] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0050] Please see Figure 1-6 The present invention provides an embodiment of a continuous production method and pipe material for mechanically pressing and anchoring butt-welded aluminum-plastic composite pipes, wherein the following steps are performed sequentially along the pipe's travel direction:

[0051] S1: Inner layer plastic tube extrusion and sizing process, a single screw extruder is used to extrude the inner layer plastic tube to be coated, and vacuum sizing and cooling are used to ensure the accuracy of the outer diameter and roundness of the tube, and it is pulled forward at a uniform speed;

[0052] S2: Aluminum strip anchor blind hole 3 prefabrication process, multiple anchor blind holes 3 are formed on the side surface of the aluminum strip facing the inner plastic tube. The longitudinal section of the anchor blind hole 3 is a trapezoid with a wider inner section and a narrower outer section. The inner wall of the trapezoidal cavity is provided with micro-blocks.

[0053] S3: Aluminum strip rolling and butt welding process, the aluminum strip with pre-made anchor blind holes 3 is wrapped around the outer wall of the inner plastic tube, and the butt joint of the aluminum strip is welded to form a sealed aluminum tube layer.

[0054] S4: Segmented induction heating process, which heats only the outer wall of the aluminum tube layer, causing the surface of the inner plastic tube to reach a viscous flow state;

[0055] S5: Radial constant pressure clamping and anchoring process, a constant radial surface pressure is applied to the pipe by a clamping mechanism set around the circumference of the pipe, so that the inner plastic layer in a viscous flow state fills into the anchoring blind hole 3;

[0056] S6: The three-stage gradient cooling self-locking process causes the plastic filled in the blind hole to cool and shrink in stages, locking into the trapezoidal blind hole to form a secondary self-locking anchor.

[0057] S7: Outer plastic co-extrusion coating process, an outer barrier plastic layer is coated on the outer wall of the cooled and shaped pipe (4).

[0058] S8: The online inspection process for traction winding, with online diameter measurement, wall thickness, and peel strength sampling stations to monitor product quality in real time, and the final finished product is automatically wound up.

[0059] Completely abandoning the traditional process of butt-welding aluminum-plastic pipes that relies on hot melt adhesive bonding, this technology eliminates the risks of adhesive layer aging, hydrolysis, and delamination due to hot and cold cycles. The trapezoidal blind hole, wider inside and narrower outside, combined with the micro-blocks on the inner wall, forms a natural mechanical self-locking cavity. Combined with the synergistic process of segmented heating, radial constant pressure pressing, and gradient cooling, high-strength physical anchoring of the aluminum-plastic interface can be achieved without the need for internal air filling and sealing. This improves production continuity by more than 70%, reduces scrap rate by 60%, and eliminates VOC emissions, making it significantly more environmentally friendly and stable than existing technologies.

[0060] In this embodiment, the depth of the anchoring blind hole 3 is 80-150μm, the height of the micro-block is 5-20μm, and the distribution density of the anchoring blind hole 3 is 250-300 holes / cm². The depth of the anchoring blind hole and the height of the micro-block are adapted to the plastic flow filling characteristics: if the depth is less than 80μm, the anchoring force is insufficient, and if it is greater than 150μm, it will easily weaken the strength of the aluminum strip itself. The height of the micro-block is controlled within the range of 5-20μm, which can form an effective anti-peeling resistance without hindering the plastic filling. The distribution density of 250-300 holes / cm² ensures the anchoring strength while avoiding the decrease in oxygen barrier performance of the aluminum layer due to too many blind holes, thus taking into account both mechanical properties and functional characteristics.

[0061] In this embodiment, the opening width of the anchoring blind hole 3 is 30-50μm, the bottom width of the anchoring blind hole 3 is 80-100μm, the depth of the blind hole is preferably 120μm, and the height of the micro-clamp is preferably 10μm. The size ratio of the inner width to the outer width forms the optimal wedge angle. After the plastic filling cools, the structure with the bottom wider than the opening naturally restricts the plastic from coming out. Combined with the 10μm high micro-clamp, a double anchor is formed: the wedge structure prevents the overall slippage of the aluminum-plastic layer, and the micro-clamp inhibits local micro-area peeling. Under these preferred parameters, the peel strength of the finished product can reach 42-46N / cm, which is more than 30% higher than that of traditional adhesive pipes.

[0062] In this embodiment, during the segmented induction heating process, the outer wall temperature of the aluminum tube layer is controlled at 130-160℃, and the surface temperature of the inner plastic tube is controlled at 120-135℃. At least two sets of independently temperature-controlled induction coils connected in series are used to target and heat the outer wall of the aluminum tube. The heat is conducted inward through the aluminum tube wall, avoiding overheating and degradation caused by direct heating of the plastic. The outer wall temperature of the aluminum tube at 130-160℃ ensures that the surface of the inner plastic layer accurately enters the viscous flow range of 120-135℃, which not only provides sufficient fluidity to fill blind holes, but also does not damage the crystal structure and mechanical properties of the inner plastic matrix 1, thus ensuring the long-term pressure resistance of the tube.

[0063] In this implementation, the radial constant pressure clamping and anchoring process uses a high-temperature resistant elastomer pressure roller or track to apply pressure in a 360° circumferential manner. The radial surface pressure is controlled between 0.5-1.5 MPa. The high-temperature resistant elastomer can buffer local pressure fluctuations, and the 360° circumferential pressure ensures that the plastic uniformly fills all blind holes. The clamping mechanism is equipped with a floating suspension drive component, which adapts to the outer diameter tolerance of the pipe to maintain constant pressure. The clamping contact part is made of high-temperature resistant elastomer material, and the floating suspension drive structure compensates for the roundness deviation of the pipe in real time. Within the preferred pressure range of 0.5-1.5 MPa, the softened plastic can be fully squeezed into the trapezoidal blind holes and micro-clamping gaps, while avoiding excessive pressure that could cause deformation of the aluminum strip or damage to the inner plastic tube. The consistency of the anchoring structure formation reaches over 99%.

[0064] In this implementation, the three-stage gradient cooling self-locking process includes: a high-temperature slow cooling stage, with water temperature controlled at 80-100℃, used to release the internal stress of the composite interface; a medium-temperature stress release stage, with water temperature controlled at 40-60℃, used for the initial curing of the plastic; and a room-temperature shaping stage, with water temperature controlled at 20-30℃, used for the complete cooling and shrinkage of the plastic. The three-step cooling is matched with the corresponding length design to achieve step-by-step controllable shrinkage of the plastic: the high-temperature slow cooling stage slowly releases the interfacial internal stress generated by extrusion, avoiding microcracks caused by sudden cooling; the medium-temperature stage guides the initial shaping of the plastic, retaining the potential energy for subsequent shrinkage; and the room-temperature stage completes the final shrinkage, using the shrinkage characteristics of the plastic itself to further strengthen the wedge-shaped locking effect. The secondary self-locking anchoring strength is more than 15% higher than that of single cooling, and there is no delamination or separation after 10,000 cycles of hot and cold cycles at 20℃-95℃.

[0065] In this implementation, during the synchronous traction and online detection winding process, the winding equipment synchronizes the speed of the winding mechanism with the traction mechanism of all processes on the entire line, with an adjustable production speed range of 0.3–0.9 m / s. The prefabrication process of the aluminum strip anchor blind hole 3 uses either roll embossing or laser etching to process the anchor blind hole 3. The speed linkage of the entire line avoids the stretching deformation or accumulation of wrinkles in the tube, and the wide speed range of 0.3–0.9 m / s is suitable for the production of various specifications of tubes. Roll embossing is suitable for the mass continuous processing of 0.4–0.5 mm thick conventional aluminum strips, with low cost and high efficiency. Laser etching is suitable for the blind hole processing of high-precision, small-diameter tubes, with no mechanical contact damage and an accuracy of ±5 μm. The two processes are suitable for different scenario requirements and have strong industrialization potential.

[0066] A butt-welded aluminum-plastic composite pipe includes an inner plastic matrix 1, an aluminum pipe anchoring layer 2, and an outer barrier plastic layer 4. The outer surface of the inner plastic matrix 1 is provided with the aluminum pipe anchoring layer 2, and multiple anchoring blind holes 3 are evenly distributed on the inner wall of the aluminum pipe anchoring layer 2. The outer surface of the aluminum pipe anchoring layer 2 is provided with the outer barrier plastic layer 4. The pipe adopts a three-layer composite structure. The aluminum pipe anchoring layer 2 is formed by butt welding, which has good overall airtightness and excellent oxygen barrier performance. There is no hot melt adhesive interlayer at the aluminum-plastic interface. The composite is achieved entirely by mechanical structure, which fundamentally avoids the failure risk caused by adhesive aging. It is suitable for fluid transportation scenarios with high requirements for durability and oxygen barrier performance, such as underfloor heating, water supply, and gas supply.

[0067] In this embodiment, the cross-section of the anchoring blind hole 3 on the inner wall of the aluminum tube anchoring layer 2 is trapezoidal with a larger inner diameter and a smaller outer diameter, and the inner wall has micro-blocks. The inner plastic matrix 1 is partially embedded in the anchoring blind hole 3. The inner plastic embedded in the blind hole forms a wedge-tight fit with the trapezoidal cavity, and the micro-blocks further lock the position of the plastic, forming a double mechanical anchoring structure of "wedge-tight and block". The interlayer bonding strength is high, and even if it is subjected to long-term cold and heat cycles or pressure fluctuations, there will be no delamination or bulging, thereby improving the service life of the pipe.

[0068] In this embodiment, EVOH barrier masterbatch is added to the outer barrier plastic layer 4, and the inner plastic matrix 1 is made of PE-RT or PEX modified plastic. The inner PE-RT or PEX modified plastic has excellent heat resistance, pressure resistance and creep resistance, and is suitable for high-temperature hot water transportation scenarios. After adding EVOH barrier masterbatch to the outer layer, it forms a double oxygen barrier with the middle sealed aluminum layer. The overall oxygen permeability of the pipe is ≤0.18mg / (m²·d), which can effectively prevent oxidation and corrosion of metal valves, radiators and other components in the heating system and extend the service life of the entire pipeline system.

[0069] Example 1, as Figure 1-2 As shown, in the production of PE-RT adhesive-free anchored aluminum-plastic composite pipes, the inner layer is extruded as follows: a 75mm single-screw extruder produces the PE-RT inner tube with a wall thickness of 2.5mm and a traction speed of 0.6m / s; aluminum strip processing: 0.4mm thick aluminum strip is rolled to create trapezoidal blind holes with an opening of 40μm, a bottom width of 90μm, a depth of 120μm, a barb height of 10μm, and a hole density of 300 holes / cm²; welding and forming: the aluminum strip is argon-arc butt-welded around the inner tube to form a sealed aluminum layer; induction heating... Three-section coil temperature control, aluminum tube outer wall stable at 145℃; radial compression: constant 0.8MPa elastic track ring pressure, softening PE-RT to fully fill trapezoidal blind holes; gradient cooling: slow cooling at 90℃ for 5m → stress release at 50℃ for 4m → room temperature setting at 25℃ for 6m; outer layer co-extruded and coated with EVOH modified PE-RT outer layer, synchronously wound; finished product testing: peel strength 43N / cm, oxygen permeability 0.17mg / (m²・d), no delamination after 10,000 cold and hot cycles. In the production of PEX glue-free anchored aluminum-plastic composite pipe, the inner layer is extruded with modified PEX pipe with a wall thickness of 2.0 mm and a traction speed of 0.5 m / s; 0.5 mm trapezoidal blind holes are laser-etched on the aluminum strip with a hole density of 250 holes / cm²; the aluminum pipe is heated to 150℃ and the clamping pressure is 0.9 MPa. The remaining process parameters are the same as in Example 1; the finished product test results show a peel strength of 46 N / cm, an oxygen permeability of 0.14 mg / (m²・d), and no degradation in anchoring performance under long-term high-temperature conditions.

[0070] Example 2, as Figure 3-6 As shown, anchoring blind holes 3 can be opened on the outer surface of the aluminum tube anchoring layer 2. During the radial constant pressure tightening anchoring process, the outer barrier plastic layer 4 should be softened at high temperature. The softened plastic is uniformly squeezed and filled into the anchoring blind holes 3 on the outer surface of the aluminum tube anchoring layer 2 to form a mechanical anchoring structure. Alternatively, the aluminum tube anchoring layer 2 can be made directly from aluminum tubes. A stamping device is used to roll the aluminum tubes so that concave rings are arranged at equal intervals on the outer surface of the aluminum tubes. Then, subsequent processes are carried out in sequence, and the fastening effect can still be achieved.

[0071] For those skilled in the art, the present invention is not limited to the details of the exemplary embodiments described above, and the invention can be implemented in other specific forms without departing from the spirit or scope thereof. Therefore, the embodiments of the present invention are exemplary and not restrictive. The scope of the invention is defined by the appended claims rather than the foregoing description, and therefore all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the invention. No reference numerals in the claims should be construed as limiting the scope of the claims.

Claims

1. A method for continuous production of a mechanically compressed and anchored formed butt welded aluminium plastic composite pipe, characterized in that, The following procedures shall be performed sequentially along the direction of pipe travel: S1: Inner layer plastic tube extrusion and sizing process, a single screw extruder is used to extrude the inner layer plastic tube to be coated, and vacuum sizing and cooling are used to ensure the accuracy of the outer diameter and roundness of the tube, and it is pulled forward at a uniform speed; S2: Aluminum strip anchor blind hole (3) prefabrication process, multiple anchor blind holes (3) are formed on the side surface of the aluminum strip facing the inner plastic tube. The longitudinal section of the anchor blind hole (3) is a trapezoid with a wider inner section and a narrower outer section. The inner wall of the trapezoidal cavity is provided with micro-blocks. S3: Aluminum strip rolling and butt welding process, the aluminum strip with pre-made anchor blind holes (3) is wrapped around the outer wall of the inner plastic tube, and the butt joint of the aluminum strip is welded to form a closed aluminum tube layer. S4: Segmented induction heating process, which heats only the outer wall of the aluminum tube layer, so that the surface of the inner plastic tube layer is heated to a viscous flow state; S5: Radial constant pressure clamping anchoring process, a constant radial surface pressure is applied to the pipe by a clamping mechanism arranged around the circumference of the pipe, so that the inner plastic layer in a viscous flow state fills into the anchoring blind hole (3); S6: The three-stage gradient cooling self-locking process causes the plastic filled in the blind hole to cool and shrink in stages, locking into the trapezoidal blind hole to form a secondary self-locking anchor. S7: Outer plastic co-extrusion coating process, an outer barrier plastic layer is coated on the outer wall of the cooled and shaped pipe (4). S8: The online inspection process for traction winding, with online diameter measurement, wall thickness, and peel strength sampling stations to monitor product quality in real time, and the final finished product is automatically wound up.

2. The method for continuously producing the mechanically compressed and anchored formed butt welded aluminum plastic composite pipe according to claim 1, characterized in that: The depth of the anchoring blind hole (3) is 80-150μm, the height of the micro-block is 5-20μm, and the distribution density of the anchoring blind hole (3) is 250-300 holes / cm².

3. The method of continuously producing a mechanically compressed and anchored butt welded aluminum-plastic composite pipe according to claim 1, characterized in that: The opening width of the anchoring blind hole (3) is 30-50μm, the bottom width of the anchoring blind hole (3) is 80-100μm, the depth of the blind hole is preferably 120μm, and the height of the micro-block is preferably 10μm.

4. The method of continuously producing a mechanically compressed and anchored butt welded aluminum-plastic composite pipe according to claim 1, characterized in that: In the segmented induction heating process, the outer wall temperature of the aluminum tube layer is controlled at 130-160℃, and the surface temperature of the inner plastic tube layer is controlled at 120-135℃.

5. The method of continuously producing a mechanically compressed and anchored butt welded aluminum-plastic composite pipe according to claim 1, characterized in that: The radial constant pressure tightening and anchoring process uses a high-temperature resistant elastomer pressure roller or track to apply pressure in a 360° circumferential manner, and the radial surface pressure is controlled at 0.5-1.5 MPa in the radial constant pressure tightening and anchoring process.

6. The method of continuously forming a mechanically compressed and anchored butt welded aluminum-plastic composite pipe of claim 1, wherein: The three-stage gradient cooling self-locking process includes, in sequence: a high-temperature slow cooling stage, with the water temperature controlled at 80-100℃, used to release the internal stress of the composite interface; a medium-temperature stress release stage, with the water temperature controlled at 40-60℃, used for the initial curing of the plastic; and a room-temperature shaping stage, with the water temperature controlled at 20-30℃, used for the complete cooling and shrinkage of the plastic.

7. The method of continuously forming a mechanically compressed and anchored butt welded aluminum-plastic composite pipe of claim 1, wherein: In the synchronous traction and online detection winding process, the winding equipment is used to wind and synchronize the speed of the traction mechanism of each process in the whole line. The production speed is adjustable in the range of 0.3-0.9m / s. The aluminum strip anchor blind hole (3) prefabrication process uses roll embossing or laser etching to process the anchor blind hole (3).

8. A butt-welded aluminium plastic composite pipe comprising an inner plastic matrix (1), an aluminium pipe anchoring layer (2) and an outer barrier plastic layer (4), characterised in that: An aluminum tube anchoring layer (2) is provided on the outer surface of the inner plastic matrix (1). Multiple anchoring blind holes (3) are evenly distributed on the inner wall of the aluminum tube anchoring layer (2). An outer barrier plastic layer (4) is provided on the outer surface of the aluminum tube anchoring layer (2).

9. The butt welded aluminum-plastic composite pipe according to claim 8, characterized in that: The cross-section of the anchoring blind hole (3) on the inner wall of the aluminum tube anchoring layer (2) is a trapezoid with a larger inner diameter and a smaller outer diameter, and the inner wall has a micro-block. The inner plastic matrix (1) is partially embedded in the anchoring blind hole (3).

10. The butt welded aluminum-plastic composite pipe according to claim 8, characterized in that: The outer barrier plastic layer (4) contains EVOH barrier masterbatch, and the inner plastic matrix (1) is made of PE-RT or PEX modified plastic.