A radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices and its preparation method
By using a layered composite structure and a high-melting-point transition layer design, the structural stability and radiation resistance of aerospace electronic devices under high-temperature service environments have been solved, achieving stability of thermal conductivity and radiation resistance, and ensuring protection against overflow and degradation of liquid metal.
Patent Information
- Application Number
- CN202611561015.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing thermal interface materials for aerospace electronic devices lack structural stability under high-temperature service environments. Liquid metals are prone to overflow and lack radiation-resistant designs, failing to meet the requirements for long-term on-orbit service of spacecraft.
A layered composite structure is adopted, including a lower surface anti-radiation passivation protective film, a lower low-melting-point metal layer, an intermediate indium-based alloy foil reinforcement layer, an upper low-melting-point metal layer, and an upper surface anti-radiation passivation protective film. A high-melting-point transition layer and an atomic layer deposited alumina film are generated in situ to form a gradient composite structure of low-melting-point metal layer-high-melting-point transition layer-intermediate reinforcement layer-high-melting-point transition layer-low-melting-point metal layer, which prevents liquid metal overflow and radiation degradation.
Maintain thermal conductivity at the service temperature of aerospace devices, suppress liquid metal overflow and irradiation degradation, ensure structural stability and thermal conductivity retention rate ≥92%, and contact thermal resistance ≤0.05 K·cm2/W.
Smart Images

Figure CN123104181A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of thermal interface materials, and more specifically, to a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices and its preparation method. Background Technology
[0002] With the rapid development of aerospace electronics technology, the power density and integration of spaceborne electronic devices are constantly increasing, placing increasingly stringent demands on heat dissipation systems. During spacecraft operation in orbit, the heat generated by electronic devices needs to be efficiently transferred to the heat dissipation structure through thermal interface materials to ensure stable operation of the devices within their rated temperature range. Thermal interface materials are used to fill the microscopic interface gaps between the heat source and the heat sink, increasing the actual contact area and thus effectively reducing contact thermal resistance. Currently, commonly used thermal interface materials in the aerospace field mainly include thermally conductive silicone grease, thermally conductive pads, phase change materials, and metallic thermal interface materials. Among these, non-metallic thermal interface materials such as thermally conductive silicone grease and thermally conductive pads generally have low thermal conductivity, typically below 10 W / mK, making it difficult to meet the heat dissipation requirements of high-power devices. While phase change materials can reduce contact thermal resistance after becoming liquid above their phase change temperature, they are prone to pumping out and aging failure during long-term thermal cycling.
[0003] Existing technologies use indium foil layers as intermediate reinforcement layers to improve the mechanical stability of liquid metals. However, the low-melting-point metal layers completely melt at service temperatures, leaving the liquid metal at risk of overflow and migration. Furthermore, these technologies lack radiation protection design, failing to meet the long-term on-orbit service requirements of spacecraft. Another existing technology employs a three-layer foil structure, with the top and bottom layers and the middle layer all composed of indium-bismuth-tin alloys. However, each layer of this material is a low-melting-point alloy, which may soften or melt under the high-temperature conditions of spaceflight, resulting in insufficient structural stability and a lack of radiation protection design. Summary of the Invention
[0004] To overcome the above shortcomings, this invention provides a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices and its preparation method, aiming to improve the problems of insufficient thermal conductivity, poor radiation resistance, easy overflow of liquid metal, and corrosion of aluminum substrate in the extreme environment of aerospace.
[0005] This invention is implemented as follows: This invention provides a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices and its preparation method. The material has a layered composite structure, comprising, from bottom to top: The lower surface layer is a radiation-resistant passivation protective film; Lower low-melting-point metal layer; Intermediate indium-based alloy foil reinforcement layer; Top low-melting-point metal layer; Top surface anti-radiation passivation protective film; Both the upper low-melting-point metal layer and the lower low-melting-point metal layer are gallium-indium-tin-zinc-aluminum pentagonal alloy layers, respectively covering the upper and lower surfaces of the intermediate indium-based alloy foil reinforcement layer. The intermediate indium-based alloy foil reinforcement layer is an indium-tin-bismuth-silver quaternary alloy foil. An upper interface high-melting-point transition layer is provided at the interface between the intermediate indium-based alloy foil reinforcement layer and the upper low-melting-point metal layer, and a lower interface high-melting-point transition layer is provided at the interface between the intermediate indium-based alloy foil reinforcement layer and the lower low-melting-point metal layer. Both the upper interface high-melting-point transition layer and the lower interface high-melting-point transition layer are In-Ga-Zn ternary alloy layers, which are generated by in-situ alloying reaction between the intermediate indium-based alloy foil reinforcement layer and the adjacent low-melting-point metal layer, and their solidus temperature is ≥250℃. The upper surface anti-radiation passivation protective film and the lower surface anti-radiation passivation protective film are respectively aluminum oxide thin films deposited on the outer surface of the upper low melting point metal layer and the outer surface of the lower low melting point metal layer by atomic layer deposition technology; The material forms a gradient composite structure consisting of a low-melting-point metal layer, a high-melting-point transition layer, an intermediate reinforcing layer, a high-melting-point transition layer, and a low-melting-point metal layer.
[0006] By adopting the above technical solution, the upper and lower low-melting-point metal layers cover the upper and lower surfaces of the intermediate indium-based alloy foil reinforcement layer, respectively, forming a sandwich composite structure with the intermediate reinforcement layer as the supporting skeleton. The solidus temperature of the In-Ga-Zn ternary high-melting-point transition layer generated in situ at the interface is ≥250℃, and it remains solid at the device service temperature. It acts as a diffusion barrier to prevent the low-melting-point components from excessively penetrating into the intermediate layer, and as a physical barrier to inhibit the lateral migration and longitudinal overflow of liquid metal. The atomic layer deposition of alumina film on the upper and lower outer surfaces completely encloses the internal metal layer, blocking the direct bombardment of the internal liquid metal layer by high-energy particles in space, and preventing the liquid metal components from deteriorating and oxidizing under irradiation. This balances the interfacial wettability of the low-melting-point metal layer with the overall structural stability, and solves the problems of insufficient thermal conductivity, poor radiation resistance, and easy overflow of liquid metal in the existing technology.
[0007] Preferably, the gallium-indium-tin-zinc-aluminum pentagonal alloy layer is composed of the following components: Ga 45-60 wt%, In 15-25 wt%, Sn 5-12 wt%, Zn 1-5 wt%, Al 5-20 wt%. The indium-tin-bismuth-silver quaternary alloy foil is composed of the following components by mass percentage: In 40-65 wt%, Sn 10-25 wt%, Bi 15-35 wt%, Ag 0.5-5 wt%.
[0008] By adopting the above technical solutions, the low-melting-point metal layer, with Ga as the main component and incorporating In and Sn, can adjust the liquidus temperature to the range of 10-40℃, enabling the material to maintain excellent wettability and fluidity at typical operating temperatures of aerospace electronic devices to fill interfacial micro-voids. The introduction of Zn provides a component source for the in-situ alloying reaction at the interface to generate the In-Ga-Zn ternary high-melting-point transition layer, which helps to increase the solidus temperature of the transition layer. An appropriate amount of Al has excellent wettability and compatibility with aluminum-based heat sinks commonly used in aerospace, effectively avoiding intergranular corrosion of the aluminum substrate by pure gallium-based liquid metal. The intermediate indium-based alloy foil reinforcement layer, with In as the matrix, and the composite of Sn and Bi, allows the foil to be hot-rolled in the two-phase region at 150-200℃ and has a solidus temperature of 120-180℃, maintaining a solid state at device service temperatures to provide support and compressive strength. The introduction of Ag helps to improve the strength and creep resistance of the foil.
[0009] Preferably, the liquidus temperatures of the upper and lower low-melting-point metal layers are 10-40°C, and their thicknesses are each independently 30-150 μm; the solidus temperature of the intermediate indium-based alloy foil reinforcement layer is 120-180°C, and its thickness is 20-80 μm; the thicknesses of the upper and lower high-melting-point transition layers are both 2-8 μm; the thicknesses of the upper and lower surface radiation-resistant passivation protective films are each independently 10-50 nm; and the total thickness of the composite thermal interface material is 100-500 μm.
[0010] By adopting the above technical solution, the strictly limited thickness of each layer and the phase transition temperature range enable the low-melting-point metal layer to maintain excellent wettability and fluidity to fill the microscopic gaps at the interface under the typical operating temperature of aerospace electronic devices, while the intermediate reinforcement layer remains solid to provide support and compressive strength. The total thickness is controlled at 100-500 μm to effectively adapt to the assembly gap between the chip and the heat sink, avoiding the increase in thermal resistance due to excessive thickness or the inadequacy of filling due to insufficient thickness. The thickness of the high-melting-point transition layer is controlled at 2-8 μm, which can form a continuous and complete barrier layer sufficient to block diffusion and overflow, without excessively consuming the intermediate layer and low-melting-point metal layer and increasing the interface thermal resistance due to excessively thick transition layer.
[0011] This invention also provides a method for preparing a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices, comprising the following steps: S1. Low melting point metal smelting: Under vacuum or inert atmosphere protection, raw materials are weighed in the proportion of Ga 45-60 wt%, In 15-25 wt%, Sn 5-12 wt%, Zn 1-5 wt%, Al 5-20 wt%, and vacuum induction smelting is carried out to obtain low melting point metal ingots. S2. Preparation of intermediate indium-based alloy foil: Weigh the raw materials according to the ratio of In 40-65 wt%, Sn 10-25 wt%, Bi 15-35 wt%, Ag 0.5-5 wt%, melt and cast into ingots under a protective atmosphere, and obtain an intermediate indium-based alloy foil reinforcement layer with a thickness of 20-80 μm after hot rolling and annealing. S3, Low-temperature lamination composite: The low-melting-point metal ingot obtained in S1 is heated and softened at 40-80℃, and the upper and lower surfaces of the intermediate indium-based alloy foil reinforcement layer obtained in S2 are respectively covered with low-melting-point metal layers to form a three-layer composite structure. S4. Vacuum annealing alloying: The three-layer composite structure obtained in S3 is vacuum annealed at 80-150℃ for 2-10h, so that the intermediate indium-based alloy foil reinforcing layer and the low melting point metal layer undergo an alloying reaction at the interface, and an upper interface high melting point transition layer and a lower interface high melting point transition layer are generated in situ. The upper interface high melting point transition layer and the lower interface high melting point transition layer are In-Ga-Zn ternary alloys. S5. Surface atomic layer deposition passivation: Alumina films are deposited on the upper and lower surfaces of the composite structure obtained in S4 using atomic layer deposition technology to obtain a radiation-resistant passivation protective film. S6. Cutting and Inspection: Cut the composite thermal interface material obtained in S5 to the required size, and package and store it after passing the inspection.
[0012] By employing the above technical solution, the method of this invention obtains a low-melting-point alloy ingot with uniform composition through vacuum induction melting, obtains an intermediate alloy foil with precisely controllable thickness through hot rolling and annealing processes, achieves physical pre-composite bonding through low-temperature lamination, and then generates a high-melting-point transition layer in situ at the interface through vacuum annealing. Finally, a dense alumina protective film with nanoscale thickness is achieved using atomic layer deposition technology. This preparation process is logically sequenced and compatible, ensuring the accuracy of the thickness and composition of each layer while achieving interlayer metallurgical bonding through interfacial reactions, significantly improving the structural integrity and service reliability of the material. The in-situ generated In-Ga-Zn ternary transition layer has a solidus line significantly higher than the service temperature, remaining solid throughout the operating temperature range of aerospace devices. It acts as a diffusion barrier to prevent excessive penetration of low-melting-point components into the intermediate layer and as a physical barrier to effectively suppress the lateral migration and longitudinal overflow of liquid metal, fundamentally solving the problem of liquid metal overflow.
[0013] Preferably, the specific process of vacuum induction melting described in S1 is as follows: Al is placed at the bottom of the crucible, Sn, In, and Zn are added in sequence, and Ga is finally placed at the top, and the vacuum is evacuated to a vacuum degree ≤ 1×10⁻⁶. -2Pa, fill with high-purity argon gas to atmospheric pressure, heat to 300-500℃, and after all the metals have completely melted, hold at that temperature for 10-30 minutes, cool to room temperature, and repeat the melting-cooling cycle 2-4 times.
[0014] By adopting the above technical solution, Al has the highest melting point and the largest density. Placing it at the bottom can prevent the low melting point Ga from directly contacting the bottom of the crucible in the early stage of melting, which would cause local overheating and corrosion. Placing Ga at the top layer is conducive to its preferential melting and wetting of other metals from top to bottom, thereby improving the melting efficiency. Multiple melting-cooling cycles can effectively eliminate the component segregation caused by the difference in specific gravity, ensuring the macroscopic uniformity of the alloy ingot.
[0015] Preferably, the smelting process in S2 is as follows: smelting at 250-400℃ under vacuum or inert atmosphere protection, holding for 10-20 min, and casting into ingots; the hot rolling process is as follows: performing multiple hot rolling passes at 150-200℃, with a reduction of 10-20% per pass, a total reduction of ≥80%, and annealing at 120-180℃ for 1-4 h after rolling.
[0016] By adopting the above technical solutions, the appropriate melting temperature and holding time are conducive to obtaining pure and uniform indium-based alloy ingots; hot rolling in the two-phase region at 150-200℃ can avoid rolling cracks; controlling the reduction amount in each pass to 10-20% can prevent edge cracks; and the total reduction amount ≥80% ensures the density and thickness uniformity of the foil. Subsequent annealing can eliminate work hardening and restore the flexibility of the foil.
[0017] Preferably, the covering method in S3 is roll forming or molding, the composite temperature is 40-80℃, the composite pressure is 5-20 MPa, and the thickness of the low melting point metal layer is 30-150 μm.
[0018] By adopting the above technical solution, the composite temperature of 40-80℃ is in the softening range of low melting point metals, which can ensure that it has sufficient fluidity to form a dense interface, but does not melt completely and cause overflow; the pressure of 5-20 MPa is sufficient to achieve tight bonding between layers, while avoiding excessive pressure that could cause deformation or breakage of the intermediate foil; the rolling or molding method facilitates continuous or batch production.
[0019] Preferably, the vacuum degree of the vacuum annealing in S4 is ≤1×10⁻⁶. -1 Pa, the annealing heating rate is 2-10℃ / min, and after annealing, it is cooled to room temperature at a rate of 1-5℃ / min; the thickness of the high melting point transition layer at the upper interface and the high melting point transition layer at the lower interface generated in situ are both 2-8 μm.
[0020] By adopting the above technical solutions, a suitable vacuum level avoids interfacial oxidation, and a moderate heating rate ensures that the interfacial reaction proceeds fully while preventing the liquid metal from overflowing too quickly or flowing unevenly. A slow cooling rate reduces residual thermal stress and prevents warping or interlayer cracking of the composite structure during cooling. The thickness of the transition layer is controlled at 2-8 μm, forming a continuous, dense, silver-gray reaction layer with no obvious interface boundary between it and the substrates on both sides, exhibiting a gradual change in composition. This achieves interlayer metallurgical bonding and forms a complete barrier without increasing interfacial thermal resistance due to excessive alloying.
[0021] Preferably, the atomic layer deposition process conditions in S5 are as follows: deposition temperature is 100-200℃, the precursor is trimethylaluminum and water or ozone, the deposition thickness of each atomic layer deposition cycle is 0.08-0.12 nm, and the number of cycles is 100-600.
[0022] By adopting the above technical solution, the deposition temperature of 100-200℃ is well compatible with the temperature resistance range of the composite material, which will not cause the low melting point metal layer to melt or oxidize, and can ensure the normal progress of the ALD reaction. The ALD process with trimethylaluminum and water / ozone as precursors is mature and reliable. The self-limiting growth characteristic of 0.08-0.12 nm per cycle ensures that the film thickness is precisely controllable at the atomic level. 100-600 cycles correspond to a film thickness of 10-50 nm, which can meet the requirements of radiation resistance and oxidation resistance, and will not significantly increase the interfacial thermal resistance due to excessive film thickness.
[0023] Preferably, the purity of the raw materials mentioned in S1 and S2 is not less than 99.9%.
[0024] By adopting the above technical solutions, high-purity raw materials are the foundation for ensuring the excellent thermal conductivity and reliable service life of alloy materials. They can effectively prevent impurity elements from segregating at grain boundaries or forming high-resistivity phases, thus ensuring the stability and repeatability of thermal conductivity.
[0025] The beneficial effects of this invention are: 1. This invention provides an intermediate indium-based alloy foil reinforcement layer between two low-melting-point metal layers, and after initial heating, generates an In-Ga-Zn ternary high-melting-point stable alloy transition layer at the interface between the intermediate layer and the low-melting-point metal layer. This forms a gradient composite structure of low-melting-point metal layer-high-melting-point transition layer-intermediate reinforcement layer-high-melting-point transition layer-low-melting-point metal layer. The high-melting-point transition layer remains solid at the device service temperature, with a solidus temperature ≥250℃, effectively preventing lateral migration and longitudinal overflow of liquid metal.
[0026] 2. The present invention sets an aluminum oxide passivation protective film prepared by atomic layer deposition technology on the upper and lower outer surfaces of the composite thermal interface material, which can effectively block the direct bombardment of the internal liquid metal layer by high-energy particles in space, and effectively prevent the liquid metal components from deteriorating and oxidizing under irradiation environment. The thermal conductivity retention rate is ≥92% after simulated space irradiation environment test.
[0027] 3. The low-melting-point metal layer of this invention contains an appropriate amount of Al element, exhibiting excellent wettability and compatibility with aluminum-based heat sinks commonly used in aerospace applications. This effectively avoids the corrosion problem of pure gallium-based liquid metal on the aluminum substrate, with a contact thermal resistance ≤0.05 K·cm. 2 / W, thermal conductivity 30-70 W / mK. Attached Figure Description
[0028] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained from these drawings without creative effort.
[0029] Figure 1 This is a schematic diagram of the structure of a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices provided by an embodiment of the present invention; Figure 2 This is a schematic diagram of the preparation method of the present invention.
[0030] In the figure: 1. Upper surface anti-radiation passivation protective film; 2. Upper low melting point metal layer; 3. Upper interface high melting point transition layer; 4. Middle indium-based alloy foil reinforcement layer; 5. Lower interface high melting point transition layer; 6. Lower low melting point metal layer; 7. Lower surface anti-radiation passivation protective film. Detailed Implementation
[0031] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0032] Example 1 Reference Figure 1 and Figure 2This embodiment provides a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices. The material has a layered composite structure, consisting of a lower surface radiation-resistant passivation protective film 7, a lower low-melting-point metal layer 6, an intermediate indium-based alloy foil reinforcing layer 4, an upper low-melting-point metal layer 2, and an upper surface radiation-resistant passivation protective film 1, from bottom to top.
[0033] The composite thermal interface material is in the form of sheets or foils, with each layer stacked along the thickness direction, forming a symmetrical laminated structure.
[0034] The sheet-like shape is used to fill the planar gap between the chip and the heat sink in aerospace electronic devices. The symmetrical laminated structure in the thickness direction causes equal and opposite thermal stresses to be generated on both sides of the middle layer when the material is heated and expanded. These stresses cancel each other out and effectively suppress the overall warping deformation.
[0035] The upper low-melting-point metal layer 2 and the lower low-melting-point metal layer 6 have the same planar dimensions, completely covering the upper and lower surfaces of the middle indium-based alloy foil reinforcing layer 4. The four edges are aligned without any gaps or misalignments, ensuring uniform pressure transmission and consistent bonding force between each layer during lamination.
[0036] The upper low-melting-point metal layer 2 and the lower low-melting-point metal layer 6 are symmetrically arranged about the intermediate indium-based alloy foil reinforcement layer 4 in the thickness direction. This symmetrical structure is used to cancel out the stress on both sides of the intermediate indium-based alloy foil reinforcement layer 4 when it is heated and expanded, so as to prevent the composite interface material from warping and deforming during service thermal cycles.
[0037] The upper surface anti-radiation passivation protective film 1 and the lower surface anti-radiation passivation protective film 7 completely cover the exposed surfaces of the upper low melting point metal layer 2 and the lower low melting point metal layer 6, forming a fully enclosed coating to prevent the liquid components in the low melting point metal layer from volatilizing or oxidizing under high temperature or irradiation conditions.
[0038] Preferably, both the upper low-melting-point metal layer 2 and the lower low-melting-point metal layer 6 are gallium-indium-tin-zinc-aluminum pentagonal alloy layers, which are composed of the following components by mass percentage: Ga 55 wt%, In 22 wt%, Sn 10 wt%, Zn 5 wt%, Al 8 wt%.
[0039] The thickness of both the upper low-melting-point metal layer 2 and the lower low-melting-point metal layer 6 is 80 μm, and the liquidus temperature is 25℃.
[0040] Preferably, the intermediate indium-based alloy foil reinforcing layer 4 is an indium-tin-bismuth-silver quaternary alloy foil, composed of the following components by mass percentage: In 50 wt%, Sn 18 wt%, Bi 28 wt%, Ag 4 wt%, with a thickness of 50 μm and a solidus temperature of 150℃.
[0041] Preferably, both the upper surface anti-radiation passivation protective film 1 and the lower surface anti-radiation passivation protective film 7 are aluminum oxide thin films with a thickness of 30 nm.
[0042] The specific preparation method in this embodiment is as follows: S1. Low-melting-point metal smelting: Place Al at the bottom of the crucible, then add Sn, In, and Zn in sequence, and finally place Ga on top. Evacuate the crucible to a vacuum degree ≤ 1 × 10⁻⁶. -2 Pa, fill with high-purity argon gas to atmospheric pressure, heat to 300-500℃, and after all the metals have completely melted, hold at that temperature for 10-30 minutes, cool to room temperature, and repeat the melting-cooling cycle 2-4 times.
[0043] It is important to use high-purity argon gas for protection. Ga has a low melting point and high reactivity, so placing it on the top layer allows it to melt preferentially and wet other metals from top to bottom, improving smelting efficiency while reducing direct contact with the bottom of the crucible.
[0044] Placing Al at the bottom of the crucible utilizes its high melting point and relatively high density to prevent low-melting-point Ga from directly contacting the bottom of the crucible when it melts and floats to the surface in the early stages of heating, thus avoiding corrosion of the crucible material by Ga under localized overheating conditions.
[0045] By employing 2-4 repeated melting-cooling cycles, each cycle allows for the redistribution of elements during solidification, gradually eliminating compositional segregation bands caused by differences in specific gravity, and ultimately obtaining an alloy ingot with a macroscopically uniform composition.
[0046] The low-melting-point metal ingots obtained by vacuum induction melting are block or rod-shaped ingots with a uniform pentagonal or near-eutectic structure inside.
[0047] This low-melting-point metal ingot is solid at room temperature, and appears as a silvery-white, metallic-lustered block. It is relatively soft and can be cut and processed with a knife.
[0048] The eutectic structure has a single lowest melting point, ensuring that the entire structure softens and melts synchronously when heated to 40-80℃, with no high-melting-point primary phase residue. This avoids scratching the surface of the intermediate indium-based alloy foil reinforcement layer 4 by local unmelted solid particles, and ensures that there are no particle inclusion defects between the layers after lamination.
[0049] The uniform and fine eutectic structure ensures that the low-melting-point metal layer has good fluidity during subsequent low-temperature lamination, and can be uniformly spread on the surface of the intermediate indium-based alloy foil reinforcement layer 4 under low pressure, avoiding the impact of interlayer bonding quality due to local solidification point differences caused by microstructure segregation.
[0050] S2. Preparation of intermediate indium-based alloy foil: Weigh high-purity metal raw materials according to the ratio of In 50 wt%, Sn 18 wt%, Bi 28 wt%, and Ag 4 wt%.
[0051] Melt the material at 250-400℃ under vacuum or inert atmosphere protection, hold for 10-20 min, and cast it into an ingot. Then, perform multi-pass hot rolling at 150-200℃, with a reduction of 10-20% per pass and a total reduction of ≥80%. After rolling, anneal at 120-180℃ for 1-4 h to obtain an intermediate indium-based alloy foil reinforcement layer 4 with a thickness of 20-80 μm.
[0052] Pay attention to controlling the hot rolling temperature within the alloy two-phase region, ensuring moderate reduction per pass to prevent edge cracking, and performing annealing in a protective atmosphere.
[0053] The intermediate indium-based alloy foil reinforcement layer 4, obtained after hot rolling and annealing, is a strip-shaped foil with a certain degree of flexibility, and its upper and lower surface roughness Ra≤0.4μm.
[0054] The strip foil has a silver-gray metallic appearance and can be naturally unrolled when rolled up without brittle cracks.
[0055] A surface roughness of Ra≤0.4μm is the appropriate range required for mechanical interlocking. If the roughness is too large, the low melting point metal cannot completely fill the pits during stacking, forming interfacial voids and increasing thermal resistance. If the roughness is too small, the friction coefficient is too low and the interlayer shear bonding force is insufficient.
[0056] This surface roughness range is used to form a mechanically interlocked interface between the low-melting-point metal layer and the low-temperature lamination, increasing the actual contact area between layers, which helps to improve the interfacial bonding strength, while avoiding interlayer slippage and separation due to an overly smooth surface.
[0057] S3. Low-temperature lamination composite: The low-melting-point metal ingot is heated and softened at 40-80℃, and then covered on the upper and lower surfaces of the intermediate indium-based alloy foil reinforcement layer 4 by rolling or molding. The composite temperature is 40-80℃, the composite pressure is 5-20 MPa, and the thickness of the low-melting-point metal layer is 30-150 μm.
[0058] Note that the heating temperature should not exceed the liquidus line, the composite pressure should be uniform, and the operation should be carried out in a protective atmosphere.
[0059] The three-layer composite structure formed after low-temperature lamination is the initial preform, and the upper low-melting-point metal layer 2 and the lower low-melting-point metal layer 6 are physically pressed into contact with the middle indium-based alloy foil reinforcing layer 4.
[0060] The total thickness of the preform is controlled to be the sum of the thicknesses of each layer after stacking. The outer surfaces of the upper low-melting-point metal layer 2 and the lower low-melting-point metal layer 6 have a metallic luster and are free from oxidation discoloration or obvious scratches.
[0061] The physical pressing contact interface relies on van der Waals forces and mechanical anchoring effects to maintain interlayer bonding. After subsequent vacuum annealing, the interface is transformed in situ into a metallurgical bonding interface, and the bonding strength is improved from physical adsorption to chemical bonding.
[0062] The overall thickness tolerance of the preform is controlled within ±5μm to ensure that the diffusion reaction in each region of the interface proceeds synchronously during the subsequent vacuum annealing alloying process, and to avoid local over-alloying or insufficient diffusion due to uneven thickness.
[0063] S4. Vacuum annealing alloying: The three-layer composite structure is placed in a vacuum annealing furnace with a vacuum degree ≤1×10⁻⁶. -1 Pa, heat to 80-150℃ at 2-10℃ / min, hold for 2-10 h, so that the high melting point transition layer 3 on the upper interface and the high melting point transition layer 5 on the lower interface of the In-Ga-Zn ternary high melting point stable alloy are generated in situ at the interface. After annealing, cool to room temperature at 1-5℃ / min.
[0064] It is important to note that the heating rate should not be too fast to prevent liquid metal from overflowing. The annealing time should be sufficient to ensure complete interfacial reaction, but should not be too long to avoid increasing thermal resistance.
[0065] The high-melting-point transition layer 3 at the upper interface and the high-melting-point transition layer 5 at the lower interface formed after vacuum annealing are continuous and dense silver-gray reaction layers with a thickness of 2-8 μm. There is no obvious interface boundary between them and the substrates on both sides, and they exhibit a gradual change in composition gradient.
[0066] The solidus temperature of this transition layer is ≥250℃, and it remains solid at the device service temperature. Its high hardness effectively resists external vibration and impact loads and prevents interface delamination.
[0067] S5. Surface atomic layer deposition passivation: Alumina films are deposited on the upper and lower surfaces of the composite structure using atomic layer deposition technology. The deposition temperature is 100-200℃, and the precursor is trimethylaluminum and water or ozone. The deposition thickness of each atomic layer is 0.08-0.12 nm, and the cycle is 100-600 times to obtain the upper surface anti-radiation passivation protective film 1 and the lower surface anti-radiation passivation protective film 7.
[0068] Before deposition, ensure the surface is cleaned to guarantee film adhesion. The deposition temperature should be controlled within the thermal stability range of the composite structure, and the film thickness should be controlled between 10-50 nm.
[0069] The upper surface anti-radiation passivation protective film 1 and the lower surface anti-radiation passivation protective film 7, prepared by atomic layer deposition, are pinhole-free, highly dense amorphous aluminum oxide thin films.
[0070] The alumina film is transparent and colorless, uniformly covering the surface of the low-melting-point metal layer, with complete coverage of the edges and sidewalls, without any exposed substrate or accumulation.
[0071] The self-limited growth characteristics of atomic layer deposition ensure that the thickness deviation of the film is less than ±1nm within an area of 100mm×100mm, the density is close to the theoretical density, and the defect density is extremely low.
[0072] The hardness of the amorphous alumina film is about 20 GPa, which can resist minor scratches during assembly operations and protect the internal soft, low-melting-point metal layer from mechanical damage.
[0073] The film has a characteristic monolayer growth structure in the thickness direction, with layers bonded by Al-O covalent bonds to form a dense ionic crystal barrier layer.
[0074] This barrier layer is used to block the penetration of high-energy protons, electrons and atomic oxygen in space. At the same time, it utilizes the high dielectric constant and wide bandgap of alumina to dissipate the energy deposited by high-energy particles, avoiding energy focusing on the internal low-melting-point metal layer and causing local overheating and decomposition.
[0075] S6. Cutting and Inspection: Cut the composite thermal interface material to the required size, inspect each piece for appearance defects and thickness uniformity, and vacuum seal and store after passing the inspection.
[0076] Note that precision cutting or laser cutting should be used to prevent edge damage, and the product should be thoroughly dried before packaging to prevent moisture from entering.
[0077] The cut individual materials are in the form of square or round sheets with straight edges and no burrs. The aluminum oxide film at the edges completely covers the low-melting-point metal layer cross-section to prevent the exposed metal layer edges from becoming a preferred entry channel for moisture or radiation damage.
[0078] Vacuum sealing uses an aluminum-plastic composite bag with a desiccant inside. After vacuuming to ≤100Pa, it is heat-sealed to prevent moisture adsorption on the material surface during transportation and storage.
[0079] Testing showed that the composite thermal interface material prepared in this embodiment has a total thickness of approximately 220-230 μm, a room temperature thermal conductivity of 52 W / mK, and a contact thermal resistance of 0.035 K·cm under a pressure of 1 MPa. 2 / W. 100 kGy 60 After Co γ-ray irradiation, the thermal conductivity retention rate is 94%.
[0080] After undergoing 1000 thermal cycles at 80-125℃, no liquid metal spilled out.
[0081] Example 2 The difference between this embodiment and Embodiment 1 lies in the different proportions of each group and the different process parameters.
[0082] Reference Figure 1In this embodiment, the upper low-melting-point metal layer 2 and the lower low-melting-point metal layer 6 are composed of the following components by mass percentage: Ga 48 wt%, In 25 wt%, Sn 8 wt%, Zn 5 wt%, Al 14 wt%, and the thickness of each is 70 μm.
[0083] The intermediate indium-based alloy foil reinforcing layer 4 is composed of the following components by mass percentage: In 45 wt%, Sn 22 wt%, Bi 30 wt%, Ag 3 wt%, with a thickness of 40 μm.
[0084] The thickness of both the upper surface anti-radiation passivation protective film 1 and the lower surface anti-radiation passivation protective film 7 is 40 nm.
[0085] Regarding the preparation method, S1 is heated to 380℃ and held for 25 min, and the melting-cooling cycle is repeated 3 times.
[0086] The ingot is heated to 300℃ in S2 and held for 15 minutes. The ingot is then hot-rolled at 170℃ and annealed at 140℃ for 3 hours after rolling.
[0087] The composite temperature in S3 is 55℃, the composite pressure is 12 MPa, and the thickness of the low-melting-point metal layer is 70 μm.
[0088] In S4, the temperature is increased to 110℃ at 4℃ / min and held for 8 hours, then cooled to room temperature at 2℃ / min.
[0089] The deposition temperature in S5 is 140℃, and the cycle is 400 times.
[0090] Testing revealed that the composite thermal interface material prepared in this embodiment has a total thickness of approximately 190-200 μm, a room temperature thermal conductivity of 48 W / mK, and a contact thermal resistance of 0.040 K·cm under a pressure of 1 MPa. 2 / W. 100 kGy 60 After Co γ-ray irradiation, the thermal conductivity retention rate is 93%.
[0091] After undergoing 1000 thermal cycles at 80-125℃, no liquid metal spilled out.
[0092] Example 3 The difference between this embodiment and Embodiment 1 lies in the different proportions of each group and the different process parameters.
[0093] Reference Figure 1 In this embodiment, the upper low-melting-point metal layer 2 and the lower low-melting-point metal layer 6 are composed of the following components by mass percentage: Ga 60 wt%, In 18 wt%, Sn 12 wt%, Zn 3 wt%, Al 7 wt%, and each has a thickness of 90 μm.
[0094] The intermediate indium-based alloy foil reinforcing layer 4 is composed of the following components by mass percentage: In 58 wt%, Sn 14 wt%, Bi 24 wt%, Ag 4 wt%, with a thickness of 60 μm.
[0095] The thickness of both the upper surface anti-radiation passivation protective film 1 and the lower surface anti-radiation passivation protective film 7 is 25 nm.
[0096] Regarding the preparation method, S1 is heated to 420℃ and held for 15 min, and the melting-cooling cycle is repeated 4 times.
[0097] The ingot is heated to 260°C in S2 and held for 20 minutes. The ingot is then hot-rolled at 190°C and annealed at 160°C for 2 hours after rolling.
[0098] The composite temperature in S3 is 65℃, the composite pressure is 8 MPa, and the thickness of the low-melting-point metal layer is 90 μm.
[0099] In S4, the temperature is increased to 130℃ at 6℃ / min and held for 5 h, then cooled to room temperature at 4℃ / min.
[0100] The deposition temperature in S5 was 160℃, and the cycle was 250 times.
[0101] Testing showed that the composite thermal interface material prepared in this embodiment has a total thickness of approximately 290 μm, a room temperature thermal conductivity of 55 W / mK, and a contact thermal resistance of 0.032 K·cm under a pressure of 1 MPa. 2 / W.
[0102] After 100 kGy 60 After Co γ-ray irradiation, the thermal conductivity retention rate is 95%.
[0103] After undergoing 1000 thermal cycles at 80-125℃, no liquid metal spilled out.
[0104] Comparative Example A single gallium-based liquid metal alloy foil (with a thickness similar to that of the example) without an aluminum oxide passivation protective film and without an intermediate indium-based alloy foil reinforcement layer 4 was used as a comparative example.
[0105] This liquid metal paste is liquid at room temperature and has a thermal conductivity of 26 W / mK.
[0106] After 100 kGy 60 After Co gamma ray irradiation, the thermal conductivity dropped to below 18 W / mK, and the retention rate was less than 70%. After thermal cycling tests at 80-125℃, liquid metal was clearly spilled out.
[0107] Performance comparison test To further verify the beneficial effects of the technical solution of the present invention, the composite thermal interface materials prepared in Examples 1-3 were subjected to a systematic performance comparison test with typical thermal interface materials in the prior art. The specific results are as follows.
[0108] Performance comparison test To further verify the beneficial effects of the technical solution of the present invention, the composite thermal interface materials prepared in Examples 1-3 were subjected to a systematic performance comparison test with typical thermal interface materials in the prior art. The specific results are as follows.
[0109] Table 1 compares the thermal conductivity of the composite thermal interface material of the present invention with that of existing typical thermal interface materials.
[0110] Among them, Ga 75 In 25 The liquid metal has a thermal conductivity of 26.6 W / m·K and a thermal resistance of 2.8 mm. 2 ·K / W; Ga 62.5 In 21.5 Sn 16 The liquid metal has a thermal conductivity of 44.48 W / m·K and a contact thermal resistance of 4.044 mm. 2 The thermal conductivity of the GBLM-CF composite material is 51.58 ± 0.01 W / m·K, which is 212.6% higher than that of GBLM.
[0111] The composite thermal interface material of the present invention maintains the high thermal conductivity of liquid metal while achieving lower contact thermal resistance through a multi-layer composite structure design.
[0112] Table 1 Comparison of thermal conductivity properties of different thermal interface materials
[0113] Note: The unit of contact thermal resistance in this invention differs from that in the literature. The conversion relationship is: 1 K·cm 2 / W = 100 K·mm 2 / W. The contact thermal resistance of this invention is ≤0.05 K·cm. 2 / W, i.e., ≤5 K·mm 2 / W.
[0114] Table 2 compares the stability performance of different liquid metal thermal interface materials after thermal cycling tests.
[0115] BiInSn liquid metal phase change material showed alloy leakage after one cycle at 25℃-100℃; BiInSn-AlN composite material also showed leakage after three cycles.
[0116] Conventional Ga-In and Galinstan liquid metal alloys exhibit performance degradation due to oxidation during thermal cycling tests from -10°C to 60°C.
[0117] The composite thermal interface material of the present invention generates an In-Ga-Zn high-melting-point stable alloy transition layer in situ at the interface between the intermediate indium-based alloy foil reinforcement layer 4 and the low-melting-point metal layer. No liquid metal overflows after 1000 thermal cycles at 80-125°C.
[0118] Table 2 Comparison of overflow / leakage after thermal cycling of different liquid metal thermal interface materials
[0119] Table 3 compares the performance retention of the composite thermal interface material of the present invention with that of conventional liquid metal materials under simulated space irradiation environment.
[0120] Conventional gallium-based liquid metals exhibit Ga-O bond breakage under space proton irradiation, forming GaOx, which leads to material performance degradation; Ga 20 In 80 Although alloys have a certain radiation shielding ability, liquid metals lacking passivation protection typically retain less than 70% of their thermal conductivity after 100 kGy γ irradiation.
[0121] This invention effectively blocks high-energy particles from bombarding the internal liquid metal layer by setting atomic layer deposited alumina passivation protective film on the upper and lower outer surfaces, and the thermal conductivity retention rate is ≥92% after irradiation.
[0122] Table 3 Comparison of thermal conductivity retention before and after irradiation
[0123] Table 4 provides a comprehensive comparison of various thermal interface materials from five dimensions: thermal conductivity, contact thermal resistance, radiation resistance, overflow suppression capability, and interface compatibility.
[0124] While traditional thermal grease and thermal pads have mature manufacturing processes, they have low thermal conductivity and high contact thermal resistance. Conventional liquid metals have excellent thermal conductivity, but they have poor radiation resistance, are prone to overflow, and corrode aluminum substrates. Existing three-layer liquid metal foils have some structural improvements, but they lack radiation resistance design and each layer is a low-melting-point alloy.
[0125] This invention has significant advantages in all five dimensions.
[0126] Table 4 Comparison of comprehensive performance of different thermal interface materials
[0127] Table 5 summarizes the preparation parameters and performance test results of the three embodiments of the present invention. The three embodiments differ in aspects such as the composition of the low-melting-point metal layer, the composition of the intermediate alloy foil, and the annealing temperature and time, but all achieve excellent comprehensive performance, verifying the universality and repeatability of the technical solution of the present invention.
[0128] Table 5. Performance Summary of Various Embodiments of the Invention
[0129] Based on the above comparative data, the radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices provided by this invention is significantly superior to existing technologies in terms of thermal conductivity, radiation resistance, suppression of liquid metal overflow, and interface compatibility. It is particularly suitable for thermal management applications of electronic devices in extreme aerospace environments.
[0130] Industrial applicability The radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices and its preparation method provided by this invention can be widely used in interface heat conduction scenarios of devices such as aerospace chips, high-power single-unit satellites, and spacecraft thermal control systems.
[0131] The material of this invention exhibits excellent thermal conductivity and long-term stability in extreme aerospace environments, which is of great value for improving the reliability and service life of aerospace electronic devices.
[0132] The working principle of a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices and its preparation method: When the material is heated for the first time, the intermediate indium-based alloy foil reinforcing layer 4 undergoes an alloying reaction with the upper low-melting-point metal layer 2 and the lower low-melting-point metal layer 6 at the interface, and an In-Ga-Zn ternary high-melting-point upper interface high-melting-point transition layer 3 and a lower interface high-melting-point transition layer 5 are generated in situ. The microstructure of the upper interface high melting point transition layer 3 and the lower interface high melting point transition layer 5 is a fine equiaxed crystal structure with a grain size ≤10μm, which is continuously distributed along the interface to form a complete barrier layer. The continuous and dense barrier layer acts as a diffusion barrier, preventing the low-melting-point components in the upper low-melting-point metal layer 2 and the lower low-melting-point metal layer 6 from continuously diffusing into the interior of the intermediate indium-based alloy foil reinforcement layer 4, thus preventing the intermediate indium-based alloy foil reinforcement layer 4 from losing its supporting strength due to over-alloying. On the other hand, as a wetting transition layer, its surface tension is between that of liquid metal and solid metal, which is used to anchor the liquid components in the interface region after the liquid metal melts, thereby reducing the macroscopic fluidity of the liquid metal. The solidus temperature of the transition layer is ≥250℃, and it remains solid at the device service temperature, forming a physical barrier to prevent the lateral migration and longitudinal overflow of liquid metal. The upper and lower surface aluminum oxide films are prepared using atomic layer deposition technology to block high-energy particles in space from bombarding the internal liquid metal layer, thus preventing the liquid metal components from undergoing radiation decomposition and oxidation degradation. The upper surface anti-radiation passivation protective film 1 and the lower surface anti-radiation passivation protective film 7 both serve as moisture barrier layers, with a water vapor transmission rate (WVTR) ≤ 10. -3 g / (m 2 •d) is used to prevent ground and launch phase environmental moisture from penetrating the interior of the low-melting-point metal layer, avoiding the formation of the GaOOH brittle phase due to hydrolysis of gallium-based alloys, and ensuring the stability of thermal conductivity of the material during long-term storage and use; The Al element in the low-melting-point metal layer improves the wettability and compatibility of the material with aerospace aluminum-based heat sinks, and avoids intergranular corrosion of the aluminum substrate by gallium, thereby achieving efficient heat transfer and long-term reliable service.
[0133] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the invention by those skilled in the art. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the invention should be included within the scope of protection of the invention.
Claims
1. A radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices, characterized in that, The material has a layered composite structure, comprising, from bottom to top: Lower surface anti-radiation passivation protective film (7); Lower low-melting-point metal layer (6); Intermediate indium-based alloy foil reinforcement layer (4); (2) A low-melting-point metal layer is applied. Top surface anti-radiation passivation protective film (1); The upper low-melting-point metal layer (2) and the lower low-melting-point metal layer (6) are both gallium-indium-tin-zinc-aluminum pentagonal alloy layers, and respectively cover the upper and lower surfaces of the intermediate indium-based alloy foil reinforcement layer (4). The intermediate indium-based alloy foil reinforcement layer (4) is an indium-tin-bismuth-silver quaternary alloy foil. An upper interface high-melting-point transition layer (3) is provided at the interface between the intermediate indium-based alloy foil reinforcement layer (4) and the upper low-melting-point metal layer (2), and a lower interface high-melting-point transition layer (5) is provided at the interface between the intermediate indium-based alloy foil reinforcement layer (4) and the lower low-melting-point metal layer (6). The upper interface high melting point transition layer (3) and the lower interface high melting point transition layer (5) are both In-Ga-Zn ternary alloy layers, which are generated by the in-situ alloying reaction of the intermediate indium-based alloy foil reinforcement layer (4) and the adjacent low melting point metal layer, and their solidus temperature is ≥250℃. The upper surface anti-radiation passivation protective film (1) and the lower surface anti-radiation passivation protective film (7) are respectively aluminum oxide films deposited on the outer surface of the upper low melting point metal layer (2) and the outer surface of the lower low melting point metal layer (6) by atomic layer deposition technology; The material forms a gradient composite structure consisting of a low-melting-point metal layer, a high-melting-point transition layer, an intermediate reinforcing layer, a high-melting-point transition layer, and a low-melting-point metal layer.
2. The radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices according to claim 1, characterized in that, The gallium-indium-tin-zinc-aluminum pentagonal alloy layer is composed of the following components: Ga 45-60 wt%, In 15-25 wt%, Sn 5-12 wt%, Zn 1-5 wt%, Al 5-20 wt%. The indium-tin-bismuth-silver quaternary alloy foil is composed of the following components by mass percentage: In 40-65 wt%, Sn 10-25 wt%, Bi 15-35 wt%, Ag 0.5-5 wt%.
3. The radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices according to claim 1, characterized in that, The liquidus temperature of the lower low-melting-point metal layer (6) and the upper low-melting-point metal layer (2) is 10-40℃, and their thicknesses are 30-150 μm, respectively. The solidus temperature of the intermediate indium-based alloy foil reinforcement layer (4) is 120-180℃, and the thickness is 20-80 μm; The thickness of the lower surface anti-radiation passivation protective film (7) and the upper surface anti-radiation passivation protective film (1) are each independently 10-50 nm; The total thickness of the composite thermal interface material is 100-500 μm.
4. The method for preparing a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices as described in claim 2, characterized in that, Includes the following steps: S1. Low melting point metal smelting: Under vacuum or inert atmosphere protection, raw materials are weighed in the proportion of Ga 45-60 wt%, In 15-25 wt%, Sn 5-12 wt%, Zn 1-5 wt%, Al 5-20 wt%, and vacuum induction smelting is carried out to obtain low melting point metal ingots. S2. Preparation of intermediate indium-based alloy foil: Weigh the raw materials according to the ratio of In 40-65 wt%, Sn 10-25 wt%, Bi 15-35 wt%, Ag 0.5-5 wt%, melt and cast into ingots under a protective atmosphere, and obtain an intermediate indium-based alloy foil reinforcement layer with a thickness of 20-80 μm after hot rolling and annealing (4). S3, Low-temperature lamination composite: The low-melting-point metal ingot obtained in S1 is heated and softened at 40-80℃, and the low-melting-point metal layer is respectively covered on the upper and lower surfaces of the intermediate indium-based alloy foil reinforcement layer (4) obtained in S2 to form a three-layer composite structure. S4, Vacuum annealing alloying: The three-layer composite structure obtained in S3 is vacuum annealed at 80-150℃ for 2-10 h, so that the intermediate indium-based alloy foil reinforcing layer (4) and the low melting point metal layer undergo an alloying reaction at the interface, and an upper interface high melting point transition layer (3) and a lower interface high melting point transition layer (5) are generated in situ. The upper interface high melting point transition layer (3) and the lower interface high melting point transition layer (5) are In-Ga-Zn ternary alloys. S5. Surface atomic layer deposition passivation: Alumina films are deposited on the upper and lower surfaces of the composite structure obtained in S4 using atomic layer deposition technology to obtain a radiation-resistant passivation protective film. S6. Cutting and Inspection: Cut the composite thermal interface material obtained in S5 to the required size, and package and store it after passing the inspection.
5. The method for preparing a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices according to claim 4, characterized in that, The specific process of vacuum induction melting described in S1 is as follows: Al is placed at the bottom of the crucible, Sn, In, and Zn are added in sequence, and Ga is placed at the top. Vacuum is then drawn until the vacuum degree is ≤1×10⁻⁶. -2 Pa, fill with high-purity argon gas to atmospheric pressure, heat to 300-500℃, and after all the metals have completely melted, hold at that temperature for 10-30 minutes, cool to room temperature, and repeat the melting-cooling cycle 2-4 times.
6. The method for preparing a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices according to claim 4, characterized in that, The smelting process described in S2 is as follows: smelting at 250-400℃ under vacuum or inert atmosphere protection, holding for 10-20 min, and casting into ingots; the hot rolling process is as follows: performing multiple hot rolling passes at 150-200℃, with a reduction of 10-20% per pass, a total reduction of ≥80%, and annealing at 120-180℃ for 1-4 h after rolling.
7. The method for preparing a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices according to claim 4, characterized in that, The covering method described in S3 is roll pressing or molding, the composite temperature is 40-80℃, the composite pressure is 5-20MPa, and the thickness of the low melting point metal layer is 30-150 μm.
8. The method for preparing a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices according to claim 4, characterized in that, The vacuum degree of vacuum annealing described in S4 is ≤1×10⁻⁶. -1 Pa, the annealing heating rate is 2-10℃ / min, and after annealing, it is cooled to room temperature at a rate of 1-5℃ / min; the thickness of the high melting point transition layer (3) of the upper interface and the high melting point transition layer (5) of the lower interface generated in situ are both 2-8 μm.
9. The method for preparing a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices according to claim 4, characterized in that, The atomic layer deposition process conditions described in S5 are as follows: deposition temperature is 100-200℃, the precursor is trimethylaluminum and water or ozone, the deposition thickness of each atomic layer deposition cycle is 0.08-0.12 nm, and the number of cycles is 100-600.
10. The method for preparing a radiation-resistant liquid metal composite thermal interface material for aerospace electronic devices according to claim 4, characterized in that, The purity of the raw materials mentioned in S1 and S2 is not less than 99.9%.