A sulfur / TiN / MXene lithium-sulfur battery cathode modified composite material and its preparation method
By preparing a sulfur/TiN/MXene composite material, the problems of poor conductivity and volume expansion in lithium-sulfur batteries were solved by utilizing the chemical adsorption of MXene nanosheets and the polarization effect of TiN, thus achieving high-efficiency electrochemical performance and stable cycle performance.
Patent Information
- Application Number
- CN202611395673.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-17
AI Technical Summary
Lithium-sulfur batteries suffer from poor conductivity of sulfur cathodes, large volume expansion during charging and discharging, severe polysulfide shuttle effect, and slow reaction kinetics, resulting in short cycle life and poor rate performance, which restricts their commercial application.
A sulfur/TiN/MXene composite material was prepared by coating sulfur/TiN with MXene nanosheets. The polar functional groups of MXene adsorb polysulfide intermediates, and TiN provides polarization to construct an efficient ion/electron transport network, thereby suppressing the shuttle effect and volume expansion.
It significantly improves the electrochemical performance of lithium-sulfur batteries, with high initial discharge specific capacity, good cycle stability, and good specific capacity even at high rates. It solves the polysulfide shuttle problem in lithium-sulfur batteries and improves the overall performance of the battery.
Smart Images

Figure CN123105565A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-sulfur battery technology, specifically to a sulfur / TiN / MXene lithium-sulfur battery cathode modified composite material and its preparation method. Background Technology
[0002] With the rapid iteration of portable electronic devices (such as smartphones and laptops) and the continued growth in energy demand from electric vehicles, this demand is driving the rapid development of electrochemical energy storage technology. Although lithium-ion batteries are widely used, their energy density is gradually approaching its theoretical limit, making it difficult to meet the needs of future long-range, high-power devices. Lithium-sulfur batteries, with their theoretical specific capacity of up to 1675 mAh / g and energy density of 2567 Wh / kg, as well as abundant sulfur reserves and environmental friendliness, have become a research hotspot for next-generation energy storage technology. However, sulfur cathodes suffer from poor conductivity, large volume expansion during charge and discharge, severe polysulfide shuttle effect, and slow reaction kinetics, resulting in short battery cycle life and poor rate performance, which restricts their commercial application. Summary of the Invention
[0003] To address the aforementioned problems, this invention provides a sulfur / TiN / MXene lithium-sulfur battery cathode modified composite material and its preparation method.
[0004] This invention involves coating a prepared monolayer of MXene nanosheets onto the exterior of a sulfur / TiN (S@TiN) composite material to obtain a sulfur / TiN / MXene (S@TiN / MXene) composite material. MXene, as a novel two-dimensional carbon material, possesses abundant polar functional groups on its surface that can effectively adsorb polysulfide intermediates through chemical bonding or dipole interactions, thereby suppressing the shuttle effect. Simultaneously, MXene exhibits high electrical conductivity, enabling the construction of efficient ion / electron transport networks. The transition metal nitride TiN can polarize with polysulfides, suppressing the shuttle effect. This invention utilizes TiN as a carrier of the active material sulfur, with the outer MXene nanosheets serving as a coating layer. Through the synergistic effect of these two components, physical confinement and chemical adsorption of polysulfides are achieved, thereby improving the electrochemical performance of lithium-sulfur batteries.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing a sulfur / TiN / MXene lithium-sulfur battery cathode modified composite material includes the following steps: (1) Titanium nitride powder was etched with hydrofluoric acid to obtain etched TiN powder; (2) Preparation of MXene: Ti3AlC2 powder was added to hydrofluoric acid for etching, and washed until neutral to obtain multilayer MXene nanosheet material; the multilayer MXene nanosheet material was then exfoliated by ultrasonic peeling in an ice bath, the supernatant was collected by centrifugation, and freeze-dried to obtain single-layer MXene powder; (3) Preparation of sulfur / TiN composite material: The TiN powder obtained in step (1) is mixed with elemental sulfur in a certain mass ratio, ground and then melt-sulfurized under an inert atmosphere to obtain S@TiN composite material; (4) Preparation of sulfur / TiN / MXene composite material: The S@TiN composite material obtained in step (3) and the MXene powder obtained in step (2) are added to deionized water, ultrasonically dispersed and magnetically stirred for 20-24 hours. After pre-freezing, vacuum freeze-drying and grinding, the S@TiN / MXene composite material is obtained.
[0006] In this invention, the amount of titanium nitride powder used in step (1) is 1.0~1.5 g, and the amount of hydrofluoric acid is 30~50 mL.
[0007] In this invention, the hydrofluoric acid etching temperature in step (1) is 40~45℃ and the etching time is 22~24 h.
[0008] In this invention, further, in step (2), the amount of Ti3AlC2 used is 1.5~2.5 g, the amount of hydrofluoric acid used is 40~60 mL, the etching temperature is 40~45 ℃, and the etching time is 40~48 h.
[0009] In this invention, furthermore, before centrifugation in step (2), the Ti3AlC2 powder etched by ice bath ultrasonic peeling is also included. By ice bath ultrasonic peeling, the multilayer MXene can be separated to obtain a few-layer / monolayer Ti3C2T x Nanosheets.
[0010] In this invention, the ice bath ultrasonic time is 0.5~1.5 h, the centrifugation speed is 3000~4000 r / min, and the centrifugation time is 20~40 min.
[0011] In this invention, further, in step (3), the mass ratio of sulfur to TiN is 3:2~2.5, the grinding time is 20~30 min, the sulfidation temperature is 150~160℃, the holding time is 16~20 h, and the heating rate is 2.5~3 ℃ / min.
[0012] In this invention, further, in step (4), the mass ratio of S@TiN to MXene is 9.5~10:1~1.5, the ultrasonic dispersion time is 20~40 min, the pre-freezing time is 12 h, and the vacuum freeze-drying time is 40~48 h.
[0013] The present invention also provides a sulfur / TiN / MXene lithium-sulfur battery cathode modified composite material prepared according to the method described above.
[0014] In this invention, hydrofluoric acid etching of the original titanium nitride powder not only removes the surface oxide layer and impurities but also increases the surface defects and active sites of TiN, facilitating a stronger interfacial bond when combined with MXene. Simultaneously, after hydrofluoric acid etching, the aluminum atom layer of Ti3AlC2 is selectively removed, resulting in a large number of polar functional groups such as -F, -OH, and -O on the surface of the prepared MXene. Subsequent ice-bath ultrasonic exfoliation further dissociates the multilayered MXene into few-layer / monolayer nanosheets, fully exposing the surface polar active sites. This allows them to effectively adsorb polysulfide intermediates through chemical bonding or dipole interactions, thereby suppressing the shuttle effect in lithium-sulfur batteries. The MXene nanosheets are then ultrasonically dispersed and magnetically stirred with S@TiN for 20-24 hours. Prolonged stirring promotes full contact and uniform composite formation of the two components, preventing nanosheet agglomeration. Subsequent pre-freezing and vacuum freeze-drying yield a structurally stable composite electrode material while preserving the layered structure and surface functional groups. The exfoliated MXene exhibits excellent conductivity and dispersibility, which is beneficial for constructing an efficient ion / electron transport network within the composite material and improving the wettability of the electrolyte to the electrode. Meanwhile, the polar surface of TiN can effectively anchor polysulfides through chemical interaction, and its spherical morphology helps alleviate the volume expansion effect of sulfur during the charging and discharging process of lithium-sulfur batteries. A significant synergistic effect exists between MXene and TiN, effectively solving the polysulfide shuttle problem in lithium-sulfur batteries and thus significantly improving the overall electrochemical performance of the battery.
[0015] By adopting the above technical solution, the beneficial effects of the present invention are as follows: Electrochemical tests show that the sulfur / TiN / MXene lithium-sulfur battery cathode modified composite material prepared in this invention exhibits excellent electrochemical performance in lithium-sulfur batteries, with an initial discharge specific capacity of 1501.74 mAh g⁻¹ under 0.1 C conditions. -1 It can still maintain 986.16 mAh g after 100 cycles. -1 This demonstrates its stable cycling performance. After 200 cycles at a high rate of 1 C, it still retains approximately 619.58 mAh g⁻¹. -1 It exhibits excellent cycle stability. Attached Figure Description
[0016] Figure 1 The XRD diffraction patterns are of the TiN, MXene, sulfur / TiN, and sulfur / TiN / MXene composite materials obtained in this invention.
[0017] Figure 2 This is a SEM image of TiN obtained in this invention.
[0018] Figure 3 This is a SEM image of MXene obtained in this invention.
[0019] Figure 4 This is a SEM image of the sulfur / TiN / MXene composite material obtained in this invention.
[0020] Figure 5 The image shows the EDS elemental distribution of the sulfur / TiN / MXene composite material obtained in this invention.
[0021] Figure 6 The diagram shows the cycling performance of the sulfur / TiN / MXene composite material obtained in this invention.
[0022] Figure 7 This is a comparison chart of the cycling performance of embodiments and comparative examples of the present invention under different current densities.
[0023] Figure 8 This is a comparison chart of the rate performance of the embodiments and comparative examples of the present invention under different current densities. Detailed Implementation
[0024] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0025] Example 1 This embodiment provides a method for preparing a sulfur / TiN / MXene lithium-sulfur battery cathode modified composite material, including the following steps: (1) Preparation of TiN powder material: First, 1.0 g of raw commercial TiN powder (approximately 30 nm in diameter) was carefully dissolved in a plastic container containing 50 mL of hydrofluoric acid (5 wt%) for etching. The plastic container was placed in a water bath and stirred at 45 °C for 24 h. Subsequently, the solution was repeatedly washed with deionized water until neutral. The obtained sample was dried in an oven at 80 °C for 12 h.
[0026] (2) Preparation of monolayer MXene nanosheets: 2 g of Ti3AlC2 powder was slowly added to a plastic beaker containing 50 mL of hydrofluoric acid solution (40 wt%) in a fume hood. The mixture was placed on a magnetic stirrer set at 45 ℃ and stirred continuously for 48 h. After the etching reaction was completed, the mixture was centrifuged and the lower precipitate was collected. Sufficient high-purity water was added to the precipitate, and the mixture was washed and centrifuged again until the pH of the supernatant reached neutral. The precipitate after washing to neutrality was the multilayer MXene nanosheet material. Subsequently, the obtained multilayer MXene nanosheets were dispersed in 300 mL of deionized water and subjected to ice bath ultrasonic treatment for 1 h. After ultrasonic exfoliation, the suspension was centrifuged at 3500 r / min for 30 min, and the dark supernatant containing monolayer MXene nanosheets was collected. Finally, the collected supernatant was freeze-dried to obtain fluffy monolayer MXene nanosheet powder.
[0027] (3) Preparation of sulfur / TiN composite material: TiN powder obtained after etching was weighed with sublimed sulfur at a mass ratio of 2:3. Then, the two were placed in an agate mortar and ground by hand for 30 minutes to ensure thorough mixing of the two phases. The mixture was then transferred to a corundum crucible and placed in the constant temperature zone of a tube furnace; after sealing, high-purity nitrogen was introduced to replace the internal air. The temperature was increased to 160 °C at a rate of 3 °C / min and held at that temperature for 18 h. Finally, the black product was collected after natural cooling to room temperature, thus obtaining the S@TiN composite material.
[0028] (4) Preparation of lithium-sulfur battery composite cathode material: 0.1 g of the monolayer MXene obtained in step (2) was dispersed in 20 mL of high-purity water and ultrasonically treated for 30 min. Subsequently, 1 g of S@TiN powder was added to the dispersion system. The mixture was continuously magnetically stirred at room temperature for 24 h to allow the S@TiN particles to fully contact and self-assemble with the MXene solution. After stirring, the mixture was transferred to a glass petri dish, sealed, and pre-frozen at -20 ℃ for 12 h. The pre-frozen sample was transferred to a vacuum freeze dryer and freeze-dried for 48 h to completely remove moisture and maintain the three-dimensional network structure. Finally, the resulting fluffy solid was taken out and ground in an agate mortar for 30 min to obtain the sulfur / TiN / MXene composite material (S@TiN / MXene).
[0029] Battery preparation: 0.21 g of the positive electrode modified composite material prepared in step (4), 0.06 g of acetylene black and 0.03 g of PVDF (polyvinylidene fluoride) were mixed and NMP (N-methyl-2-pyrrolidone) solvent was added. The mixture was stirred into a paste and uniformly coated onto an aluminum foil with a thickness of 10 μm. The aluminum foil was then placed in a forced-air drying oven and dried at 60 ℃ for 6 h. The aluminum foil was then transferred to a vacuum drying oven and dried at 70 ℃ for 24 h. The foil was punched into a 14 mm circular electrode using a manual punching machine. The circular electrode was used as the positive electrode, the lithium sheet as the negative electrode, the microporous polypropylene membrane as the separator, and 1 mol / L LiTFSI / DOL+DME (volume ratio 1:1) as the electrolyte. A button cell with the simulated model CR2032 was assembled in an argon-filled glove box. After sealing, the cell was placed in a ventilated place and left to stand for 12 h.
[0030] During electrochemical performance testing, the battery's test voltage range is 1.5-2.8 V, and the test current is determined based on the mass of the active material on the electrode material.
[0031] Figure 1 The XRD diffraction patterns of TiN, MXene, sulfur / TiN and sulfur / TiN / MXene composites obtained in Example 1 are shown. The sulfur / TiN / MXene composite material simultaneously exhibits characteristic peaks of S, TiN and MXene, and the intensity of each peak is reduced, proving that the three components were successfully composited. The composite process did not introduce new crystal phases or destroy the original crystal structure, which provides a structural basis for its electrochemical performance. Figures 2 to 5 The images show SEM images of TiN, MXene, the sulfur / TiN / MXene composite material, and the electron spectra of the sulfur / TiN / MXene composite material obtained in this invention. It can be seen that the etched TiN exhibits a spherical morphology, which significantly increases the specific surface area of the material. The monolayer MXene exhibits typical two-dimensional lamellar characteristics; its layers are flexible, transparent at the edges, and separated from each other. The MXene layers coat the outer layer of the S@TiN particles; this structure helps to mitigate the volume expansion of sulfur and improves the overall conductivity. Figure 5 The uniform distribution of elements such as C, S, Ti, O, and N can be observed, further confirming the successful composite and good dispersion of the components in the composite material. Figure 6 The electrode was subjected to 200 cycles at a high current density of 1 C. The initial discharge specific capacity was 869.57 mAh / g. After 200 consecutive charge-discharge cycles, the reversible specific capacity was still maintained at 619.58 mAh / g, with a capacity retention rate of 71.2%, demonstrating excellent cycle stability.
[0032] Example 2 This embodiment provides a method for preparing a sulfur / TiN / MXene lithium-sulfur battery cathode modified composite material, including the following steps: (1) Preparation of TiN powder material: First, 1.0 g of raw commercial TiN powder (approximately 30 nm in diameter) was carefully dissolved in a plastic container containing 50 mL of hydrofluoric acid (5 wt%) for etching. The plastic container was placed in a water bath and stirred at 45 °C for 24 h. Subsequently, the solution was repeatedly washed with deionized water until neutral. The obtained sample was dried in an oven at 80 °C for 12 h.
[0033] (2) Preparation of monolayer MXene nanosheets: 2 g of Ti3AlC2 powder was slowly added to a plastic beaker containing 50 mL of hydrofluoric acid solution (40 wt%) in a fume hood. The mixture was placed on a magnetic stirrer set at 45 ℃ and stirred continuously for 48 h. After the etching reaction was completed, the mixture was centrifuged and the lower precipitate was collected. Sufficient high-purity water was added to the precipitate, and the mixture was washed and centrifuged again until the pH of the supernatant reached neutral. The precipitate after washing to neutrality was the multilayer MXene nanosheet material. Subsequently, the obtained multilayer MXene nanosheets were dispersed in 300 mL of deionized water and subjected to ice bath ultrasonic treatment for 1 h. After ultrasonic exfoliation, the suspension was centrifuged at 3500 r / min for 30 min, and the dark supernatant containing monolayer MXene nanosheets was collected. Finally, the collected supernatant was freeze-dried to obtain fluffy monolayer MXene nanosheet powder.
[0034] (3) Preparation of sulfur / TiN composite material: TiN powder obtained after etching was weighed with sublimed sulfur at a mass ratio of 2:3. Then, the two were placed in an agate mortar and ground by hand for 30 minutes to ensure thorough mixing of the two phases. The mixture was then transferred to a corundum crucible and placed in the constant temperature zone of a tube furnace; after sealing, high-purity nitrogen was introduced to replace the internal air. The temperature was increased to 160 °C at a rate of 3 °C / min and held at that temperature for 18 h. Finally, the black product was collected after natural cooling to room temperature, thus obtaining the S@TiN composite material.
[0035] (4) Preparation of lithium-sulfur battery composite cathode material: 0.15 g MXene was dispersed in 20 mL of high-purity water and ultrasonically treated for 30 min. Subsequently, 1 g S@TiN powder was added to the dispersion system. The mixture was continuously magnetically stirred at room temperature for 24 h to allow the S@TiN particles to fully contact and self-assemble with the MXene solution. After stirring, the mixture was transferred to a glass petri dish, sealed, and pre-frozen at -20℃ for 12 h. The pre-frozen sample was transferred to a vacuum freeze dryer and freeze-dried for 48 h to completely remove moisture and maintain the three-dimensional network structure. Finally, the resulting fluffy solid was taken out and ground in an agate mortar for 30 min to obtain the sulfur / TiN / MXene composite material (S@TiN / MXene).
[0036] Example 3 This embodiment provides a method for preparing a sulfur / TiN / MXene lithium-sulfur battery cathode modified composite material, including the following steps: (1) Preparation of TiN powder material: First, 1.0 g of raw commercial TiN powder (approximately 30 nm in diameter) was carefully dissolved in a plastic container containing 50 mL of hydrofluoric acid (5 wt%) for etching. The plastic container was placed in a water bath and stirred at 45 °C for 24 h. Subsequently, the solution was repeatedly washed with deionized water until neutral. The obtained sample was dried in an oven at 80 °C for 12 h.
[0037] (2) Preparation of monolayer MXene nanosheets: 2 g of Ti3AlC2 powder was slowly added to a plastic beaker containing 50 mL of hydrofluoric acid solution (40 wt%) in a fume hood. The mixture was placed on a magnetic stirrer set at 45 ℃ and stirred continuously for 48 h. After the etching reaction was completed, the mixture was centrifuged and the lower precipitate was collected. Sufficient high-purity water was added to the precipitate, and the mixture was washed and centrifuged again until the pH of the supernatant reached neutral. The precipitate after washing to neutrality was the multilayer MXene nanosheet material. Subsequently, the obtained multilayer MXene nanosheets were dispersed in 300 mL of deionized water and subjected to ice bath ultrasonic treatment for 1 h. After ultrasonic exfoliation, the suspension was centrifuged at 3500 r / min for 30 min, and the dark supernatant containing monolayer MXene nanosheets was collected. Finally, the collected supernatant was freeze-dried to obtain fluffy monolayer MXene nanosheet powder.
[0038] (3) Preparation of sulfur / TiN composite material: TiN powder obtained after etching was weighed with sublimed sulfur at a mass ratio of 2:3. Then, the two were placed in an agate mortar and ground by hand for 30 minutes to ensure thorough mixing of the two phases. The mixture was then transferred to a corundum crucible and placed in the constant temperature zone of a tube furnace; after sealing, high-purity nitrogen was introduced to replace the internal air. The temperature was increased to 160 °C at a rate of 3 °C / min and held at that temperature for 18 h. Finally, the black product was collected after natural cooling to room temperature, thus obtaining the S@TiN composite material.
[0039] (4) Preparation of lithium-sulfur battery composite cathode material: 0.1 g MXene was dispersed in 20 mL of high-purity water and ultrasonically treated for 30 min. Subsequently, 1.5 g S@TiN powder was added to the dispersion system. The mixture was continuously magnetically stirred at room temperature for 24 h to allow the S@TiN particles to fully contact and self-assemble with the MXene solution. After stirring, the mixture was transferred to a glass petri dish, sealed, and pre-frozen at -20℃ for 12 h. The pre-frozen sample was transferred to a vacuum freeze dryer and freeze-dried for 48 h to completely remove moisture and maintain the three-dimensional network structure. Finally, the resulting fluffy solid was taken out and ground in an agate mortar for 30 min to obtain the sulfur / TiN / MXene composite material (S@TiN / MXene).
[0040] In Examples 2 and 3, the battery assembly and electrochemical testing were the same as in Example 1.
[0041] Comparative Example To verify the electrochemical performance of the composite cathode material prepared in this invention, the applicant also prepared S@MXene composite material and sulfur / TiN composite material, and conducted electrochemical tests on the S@MXene composite material and sulfur / TiN composite material as cathode materials for lithium-sulfur batteries, so as to compare the electrochemical performance (cycle performance) of the S@MXene composite material and sulfur / TiN composite material with the composite material obtained in Example 1 above.
[0042] In this comparative example, the preparation methods for MXene and sulfur / TiN composite materials are the same as those in Examples 1 to 3.
[0043] The preparation method of S@MXene composite material is as follows: 0.1 g of MXene was dispersed in 20 mL of high-purity water and sonicated for 30 min. Then, 1.5 g of sulfur powder was added to the dispersion. The mixture was continuously magnetically stirred at room temperature for 24 h to ensure sufficient contact and self-assembly of the sulfur powder and MXene solution. After stirring, the mixture was transferred to a glass petri dish, sealed, and pre-frozen at -20 °C for 12 h. The pre-frozen sample was then transferred to a vacuum freeze dryer and freeze-dried for 48 h to completely remove moisture and maintain the three-dimensional network structure. Finally, the resulting fluffy solid was removed and ground in an agate mortar for 30 min to obtain the sulfur@MXene composite material (S@MXene).
[0044] The testing conditions for the cathode material obtained in the comparative example are the same as those in Example 1.
[0045] from Figure 7 It is evident that the S@TiN / MXene electrode exhibits superior cycling performance compared to both the S@MXene and S@TiN electrodes. After 100 constant-current charge-discharge cycles at a current density of 0.1 C, the discharge specific capacity of the S@TiN / MXene electrode increased from the initial 1501.74 mAh g⁻¹. -1 Reduced to 986.16 mAh g -1 The S@MXene electrode showed a specific capacity of only 606.43 mAh g after 100 cycles of testing. -1 The S@TiN electrode has a capacity of only 533.06 mAh g. -1 The capacity is significantly lower than that of the S@TiN / MXene electrode. This phenomenon can be attributed to the structural advantages of the TiN / MXene support: the polar surface of TiN can effectively anchor polysulfides through chemisorption, suppressing their shuttle effect; while the three-dimensional conductive network constructed by MXene provides a fast channel for electron transport, and its layered structure can buffer the volume expansion of sulfur, thereby maintaining the stability of the electrode structure and slowing down the rapid capacity decay during cycling.
[0046] The applicant also compared the rate performance of the S@MXene composite material, the S@TiN composite material, and the composite material obtained in Example 1 above.
[0047] like Figure 8 As shown in the figure, the sulfur / TiN / MXene composite electrode provided in Example 1 of the present invention exhibits an average discharge specific capacity of 1411.93 mAh g⁻¹ at different current densities of 0.1, 0.2, 0.5, and 1 C. -1 1134.73 mAh g -1 999.94 mAh g -1and 858.03 mAh g -1 When the current density recovers to 0.1 C, its discharge specific capacity can still reach 1029.28 mAh g. -1 The efficiency was significantly higher than that of the S@MXene composite electrode and the sulfur / TiN composite electrode. This indicates that the sulfur / TiN / MXene composite electrode can maintain a stable electrode structure and reversible reactivity after high-rate current cycling, and its structural integrity is not severely compromised.
[0048] The above indicates that the introduction of MXene enhances the conductivity of the electrode, enabling the battery to maintain good specific capacity output even at high discharge rates. In contrast, the sulfur / TiN composite electrode performs worse at high rates than the sulfur / TiN / MXene composite electrode, suggesting that although TiN improves conductivity, TiN alone cannot provide sufficient structural stability to support high-rate charge and discharge. Therefore, the high-rate performance of sulfur / TiN / MXene benefits from the three-dimensional conductive network formed by the synergistic effect of TiN and MXene, which greatly improves the ion and electron transport efficiency of the battery during charge and discharge.
[0049] The above description is a detailed description of the preferred embodiments of the present invention. However, the embodiments are not intended to limit the scope of the patent application of the present invention. All equivalent changes or modifications made under the technical spirit of the present invention should fall within the patent scope covered by the present invention.
Claims
1. A method for preparing a sulfur / TiN / MXene lithium-sulfur battery cathode modified composite material, characterized in that, Includes the following steps: (1) Titanium nitride powder was etched with hydrofluoric acid to obtain etched TiN powder; (2) Preparation of MXene: Ti3AlC2 powder was added to hydrofluoric acid for etching, washed until neutral, ultrasonically peeled in an ice bath, the supernatant was collected by centrifugation, and freeze-dried to obtain monolayer MXene powder; (3) Preparation of sulfur / TiN composite material: The TiN powder obtained in step (1) is mixed with elemental sulfur in a certain mass ratio, ground and then melt-sulfurized under an inert atmosphere to obtain S@TiN composite material; (4) Preparation of sulfur / TiN / MXene composite material: The S@TiN composite material obtained in step (3) and the MXene powder obtained in step (2) are added to deionized water, ultrasonically dispersed and magnetically stirred for 20-24 hours. After pre-freezing, vacuum freeze-drying and grinding, the S@TiN / MXene composite material is obtained.
2. The preparation method according to claim 1, characterized in that, The amount of titanium nitride powder used in step (1) is 1.0~1.5 g, and the amount of hydrofluoric acid is 30~50 mL.
3. The preparation method according to claim 1, characterized in that, The hydrofluoric acid etching temperature in step (1) is 40~45℃ and the etching time is 22~24 h.
4. The preparation method according to claim 1, characterized in that, In step (2), the amount of Ti3AlC2 used is 1.5~2.5 g, the amount of hydrofluoric acid used is 40~60 mL, the etching temperature is 40~45 ℃, and the etching time is 40~48 h.
5. The preparation method according to claim 1, characterized in that, The centrifugation in step (2) includes the Ti3AlC2 powder that has been etched by ultrasonic stripping in an ice bath.
6. The preparation method according to claim 5, characterized in that, The ice bath ultrasonication time is 0.5~1.5 h, the centrifugation speed is 3000~4000 r / min, and the centrifugation time is 20~40 min.
7. The preparation method according to claim 1, characterized in that, In step (3), the mass ratio of sulfur to TiN is 3:2~2.5, the grinding time is 20~30 min, the sulfidation temperature is 150~160℃, the holding time is 16~20 h, and the heating rate is 2.5~3 ℃ / min.
8. The preparation method according to claim 1, characterized in that, In step (4), the mass ratio of S@TiN to MXene is 9.5~10:1~1.5, the ultrasonic dispersion time is 20~40 min, the pre-freezing time is 12 h, and the vacuum freeze-drying time is 40~48 h.
9. A sulfur / TiN / MXene lithium-sulfur battery cathode modified composite material prepared by the method according to any one of claims 1 to 8.