Negative electrode material, negative electrode sheet and secondary battery
By setting a carbon cladding layer on the surface of the core part of the silicon negative electrode material, the problem of easy falling off of the material surface cladding layer is solved, cycling stability and conductivity are improved, and the performance of lithium-ion batteries is improved.
Patent Information
- Application Number
- CN202411381391.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-29
AI Technical Summary
The existing silicon negative electrode materials are prone to falling off in lithium-ion batteries, resulting in poor expansion performance and capacity and attenuation of material properties.
By providing a carbon cladding layer on the surface of the core body, the gas production and carbon residual ratio of the negative electrode material are adjusted, and the density of the carbon cladding layer is improved, thereby reducing expansion and improving cycling stability.
It has achieved the reduction of gas production and expansion of the negative electrode material, improved the cycle stability and conductivity of the secondary battery, and improved the charging and discharging efficiency and capacity.
Smart Images

Figure CN119050331A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical energy storage, and in particular to a negative electrode material, a negative electrode sheet and a secondary battery. Background Art
[0002] Silicon negative electrode materials have a high theoretical energy density and are therefore generally considered to have the potential to improve the performance of lithium-ion batteries. Existing silicon materials are often compounded with metals, oxides, organic polymers, carbon and other materials to obtain negative electrode materials with better conductivity and lower expansion effect. For example, negative electrode materials based on amorphous silicon and carbon matrix are considered to have the advantages of high initial efficiency, high capacity, low expansion and good cycle stability. However, in practice, it has been found that such materials have the problem of easy detachment of the surface coating layer, which results in the material's expansion performance and capacity being not as expected, and the material performance decaying. Summary of the invention
[0003] In view of this, the present application provides a negative electrode material to solve at least one of the above problems.
[0004] To achieve the above object, the present application provides a negative electrode material, comprising a core and a carbon coating layer covering at least a portion of the surface of the core, wherein the core comprises a matrix and an active substance. The gas production A of the negative electrode material in 10 days is less than or equal to 100 mL / kg. The residual carbon rate of the negative electrode material is defined as The residual carbon rate γ is less than or equal to 20%. The test method for the 10-day gas production A includes: placing 50g of negative electrode material in a 300mL slurry stirring tank, adding 50g of 5% sodium carboxymethyl cellulose and 100mL of pure water to the stirring tank, stirring at a frequency of 50Hz and a stirring time of 1h to obtain a slurry, placing the slurry in an aluminum-plastic film, and measuring the 10-day gas production A of the slurry by the drainage method. The test method for m2 includes: placing the negative electrode material in a slurry stirring tank and stirring at a frequency of 50Hz and a stirring time of 1h, taking out the stirred negative electrode material with a mass of m1 and placing it in a hydrofluoric acid solution with a mass fraction of 20% for 1h, taking out the soaked negative electrode material, washing and drying it, and measuring the mass of m2. The test method for m3 includes: taking a negative electrode material with a mass of m1 and placing it in a hydrofluoric acid solution with a mass fraction of 20% for 1h, taking out the soaked negative electrode material, washing and drying it, and measuring the mass of m3.
[0005] In some possible implementations, in some possible implementations, the powder conductivity of the negative electrode material at 20 kN is 0.5 S / cm to 9.5 S / cm.
[0006] In some possible implementations, the ID / IG of the negative electrode material is 0.5 to 5.0.
[0007] In some possible implementations, the specific surface area of the negative electrode material is less than or equal to 5 m 2 / g.
[0008] In some possible implementations, the total pore volume of the negative electrode material is 0.001 cm 3 / g to 0.1cm 3 / g.
[0009] In some possible implementations, the compaction density of the negative electrode material is 0.8 g / cm 3 Up to 1.2g / cm 3 .
[0010] In some possible implementations, the negative electrode material includes micropores, mesopores and macropores. Based on the total pore volume of the negative electrode material, the volume proportion of micropores is less than or equal to 5%, the volume proportion of mesopores is 87% to 97%, and the volume proportion of macropores is less than or equal to 13%.
[0011] In some possible implementations, the particle size D10 of the negative electrode material is 1 μm to 5 μm, in some possible implementations, the particle size D50 of the negative electrode material is 6 μm to 16 μm, and in some possible implementations, the particle size D90 of the negative electrode material is 16 μm to 24 μm.
[0012] In some possible implementations, the thickness of the carbon coating layer is 10 nm to 1000 nm.
[0013] In some possible implementations, the active material includes one or more of Si, Sn, Ge, Pb, Ag, Mg, Zn, Ga, In, Sb, Bi and alloys thereof.
[0014] In some possible implementations, the active material includes a silicon material, the silicon material includes silicon particles, and the silicon particles include one of amorphous silicon and a composite of crystalline silicon and amorphous silicon.
[0015] In some possible implementations, the silicon material includes at least one of silicon oxide and silicon alloy.
[0016] In some possible implementations, the silicon material includes silicon particles and a silicon oxide layer located on the surface of the silicon particles, and the silicon oxide layer includes silicon oxide.
[0017] In some possible implementations, the average particle size of the active material is 0.1 nm to 500 nm.
[0018] In some possible implementations, the total pore volume of the matrix is 0.5 cm 3 / g to 2.0cm 3 / g.
[0019] In some possible implementations, the specific surface area of the substrate is 600 m 2 / g to 3000m 2 / g.
[0020] In some possible implementations, the matrix includes a carbon matrix, and the carbon matrix includes one or more of amorphous carbon, graphitized carbon, mesophase carbon microbeads, and carbon gel.
[0021] In some possible implementations, the matrix includes a non-carbon matrix, and the non-carbon matrix includes one or more of metal oxides, silicides, silicates, phosphates, titanates, and aluminum borates.
[0022] In some possible implementations, the matrix of the negative electrode material includes a carbon matrix, the active material of the negative electrode material includes a silicon material, and based on the mass of the negative electrode material, the mass proportion of the carbon element of the negative electrode material is 40% to 60%, or the mass proportion of the silicon element of the negative electrode material is 35% to 55%.
[0023] The present application also provides a negative electrode sheet, comprising a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, wherein the negative electrode active material layer comprises the above-mentioned negative electrode material.
[0024] The present application also provides a secondary battery, comprising the above-mentioned negative electrode sheet.
[0025] In the present application, by providing a carbon coating layer on at least part of the surface of the core body, the carbon coating layer can protect the core body, so that the gas production A of the negative electrode material is reduced, and it is also beneficial to reduce the expansion of the negative electrode material during the cycle, thereby improving the cycle stability of the secondary battery based on this negative electrode material. At the same time, under the premise that the negative electrode material has a certain amount of carbon coating to reduce the gas production, the residual carbon rate γ of the negative electrode material is less than or equal to 20%, so the density of the carbon coating layer is also higher, and the arrangement between carbon atoms is closer, which is conducive to forming sufficient conductive channels, which is conducive to the transmission of electrons in the carbon coating layer, thereby maintaining good conductivity. Materials with high conductivity usually have better ion conductivity, which helps to reduce the internal resistance of the battery and improve the charging and discharging efficiency, thereby helping to improve the capacity and first coulomb efficiency of the resulting secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1A A schematic diagram of the structure of a secondary battery provided in one embodiment of the present application during charging.
[0027] Figure 1B A schematic diagram of the structure of a secondary battery provided in one embodiment of the present application during discharge.
[0028] Main component symbols
[0029] Electrode assembly 100
[0030] Positive electrode 101
[0031] Negative electrode 102
[0032] Isolation film 103 DETAILED DESCRIPTION
[0033] The embodiments of the present application are described in detail below. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application; it should be noted that, unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by technicians in the technical field of the present application; in the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other; many specific details are elaborated in the following description to facilitate a full understanding of the present application, and the described embodiments are only part of the embodiments of the present application, not all of the embodiments.
[0034] The negative electrode materials obtained by combining silicon materials and carbon materials have excellent electrochemical properties. For example, amorphous silicon-carbon materials have the advantages of high initial efficiency, high capacity, low expansion and good cycle stability. However, the coating layer on the surface of amorphous silicon-carbon materials is easy to fall off, resulting in material performance degradation. Therefore, how to prepare low-expansion, high-capacity silicon-carbon composite materials with a stable coating outer layer has become one of the development directions of negative electrode materials.
[0035] The present application study found that improving the preparation process of the negative electrode material can help achieve a coating layer with better density, thereby reducing the shedding of the coating layer on the surface of the negative electrode material.
[0036] Based on this, an embodiment of the present application provides a secondary battery, comprising a housing, an electrode assembly and an electrolyte. The electrode assembly and the electrolyte are both located in the housing.
[0037] The outer shell can be a packaging bag encapsulated by an encapsulation film (such as an aluminum-plastic film), for example, a soft-pack battery. In other embodiments, it can also be a steel shell battery, an aluminum shell battery, etc.
[0038] See also Figure 1A or Figure 1B The electrode assembly 100 includes a positive electrode sheet 101, a negative electrode sheet 102 and a separator 103. The separator 103 is disposed between the positive electrode sheet 101 and the negative electrode sheet 102. When an electrolyte (not shown) is provided, when charging, please refer to Figure 1A , active ions (such as lithium ions) are deintercalated from the lattice of the positive electrode material (such as the lithiated intercalation compound) of the positive electrode sheet 101, pass through the separator 103 through the electrolyte, reach the negative electrode sheet 102 and insert into the lattice of the negative electrode material. Figure 1B, active ions (such as lithium ions) are deintercalated from the lattice of the negative electrode material of the negative electrode sheet 102, pass through the isolation membrane 103 through the electrolyte, reach the positive electrode sheet 101 and are embedded in the lattice of the positive electrode material (such as the lithiated intercalation compound), and generate electrons that reach the positive electrode sheet 101 from the negative electrode sheet 102 through the external circuit. The reverse movement of the electrons forms an electric current, which can be used by electrical appliances.
[0039] In some embodiments, the electrode assembly 100 may be a laminated structure, which is formed by alternately stacking the positive electrode sheet 101, the separator 103, and the negative electrode sheet 102. In other embodiments, the electrode assembly 100 may also be a wound structure, which is formed by stacking the positive electrode sheet 101, the separator 103, and the negative electrode sheet 102 in sequence and then winding them.
[0040] Positive electrode
[0041] The positive electrode sheet 101 includes a positive electrode current collector and a positive electrode material active layer provided on at least one surface of the positive electrode current collector. The positive electrode current collector may be made of aluminum foil or nickel foil, or may be any composite current collector disclosed in the prior art, such as but not limited to the current collector formed by combining the aforementioned conductive foil and a polymer substrate. The positive electrode material active layer includes a positive electrode active material, and the positive electrode active material includes a compound that can reversibly embed and deintercalate lithium ions (i.e., a lithiated intercalation compound). In some embodiments, the positive electrode active material may include a lithium transition metal composite oxide. The lithium transition metal composite oxide contains lithium and at least one element selected from cobalt, manganese and nickel. In some embodiments, the positive electrode active material may include but is not limited to lithium cobalt oxide (LiCoO2), lithium nickel manganese cobalt ternary material (NCM), lithium manganese oxide (LiMn2O4), lithium nickel manganese oxide (LiNi 0.5 Mn 1.5 O4) or at least one of lithium iron phosphate (LiFePO4).
[0042] The positive electrode material active layer also includes a binder to bond the positive electrode active material particles to facilitate the formation of a film layer, and at the same time, it can also improve the bonding force between the positive electrode material active layer and the positive electrode current collector. In some embodiments, the binder may include but is not limited to at least one of polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylic (ester) styrene-butadiene rubber, epoxy resin or nylon.
[0043] The positive electrode material active layer may also include a conductive material, including but not limited to a carbon-based material, a metal-based material, a conductive polymer, or any combination thereof. In some embodiments, the carbon-based material may include but is not limited to natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, the metal-based material may include but is not limited to metal powder or metal fiber, such as copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer may be a polyphenylene derivative.
[0044] Negative plate
[0045] The negative electrode sheet 102 includes a negative electrode current collector and a negative electrode material active layer disposed on at least one surface of the negative electrode current collector. The negative electrode current collector may be at least one of copper foil, nickel foil, stainless steel foil, titanium foil or a carbon-based current collector, or may be any composite current collector disclosed in the prior art, such as but not limited to a current collector formed by combining the aforementioned conductive foil and a polymer substrate.
[0046] The negative electrode material active layer includes a negative electrode material, the negative electrode material includes a core body and a carbon coating layer covering at least part of the surface of the core body, and the core body includes a matrix and an active substance. The 10-day gas production A of the negative electrode material is less than or equal to 100 mL / kg. For example, the 10-day gas production A of the negative electrode material can be 100 mL / kg, 85 mL / kg, 70 mL / kg, 65 mL / kg, 30 mL / kg, 20 mL / kg, 5 mL / kg, 4 mL / kg, 3 mL / kg or any value within the range formed by any two of the above values. Among them, the test method of the 10-day gas production A includes: placing 50g of the negative electrode material in a 300mL slurry stirring tank, adding 50g of sodium carboxymethyl cellulose with a mass fraction of 5% and 100mL of pure water to the stirring tank, stirring, the stirring frequency is 50Hz, the stirring time is 1h, and a slurry is obtained, the slurry is placed in an aluminum-plastic film, and the 10-day gas production A of the slurry is measured by a drainage method.
[0047] The present application provides a carbon coating layer on at least part of the surface of the core body. The carbon coating layer can protect the core body, reduce the gas production A of the negative electrode material, and also help reduce the expansion of the negative electrode material during the cycle, thereby improving the cycle stability of the secondary battery based on this negative electrode material.
[0048] Defining the residual carbon rate of negative electrode materials The residual carbon rate γ is less than or equal to 20%. For example, the residual carbon rate γ of the negative electrode material can be 20%, 16%, 15%, 12%, 9%, 8%, 5%, 4%, 3% or any value within the range formed by any two of the above values. Among them, the test method of m2 includes: placing the negative electrode material in a slurry stirring tank and stirring, the stirring frequency is 50Hz, the stirring time is 1h, taking out the stirred negative electrode material with a mass of m1 and placing it in a hydrofluoric acid solution with a mass fraction of 20% and soaking it for 1h, taking out the soaked negative electrode material, washing and drying it, and measuring the mass as m2. The test method of m3 includes: taking a negative electrode material with a mass of m1 and placing it in a hydrofluoric acid solution with a mass fraction of 20% and soaking it for 1h, taking out the soaked negative electrode material, washing and drying it, and measuring the mass as m3.
[0049] The embodiment of the present application improves the coating treatment process of the negative electrode material and adjusts the compactness of the obtained negative electrode material coating layer, thereby achieving the purpose of reducing the above-mentioned residual carbon rate. In the present application, the above-mentioned residual carbon rate represents the proportion of the mass of the part of the core body coated by the unstable carbon coating layer in the negative electrode material to the total mass of the negative electrode material. Among them, the present application stirs the negative electrode material, changes the coating effect of the carbon coating layer by external force, causes part of the carbon coating layer to lose its protective effect on the coated core body, and then causes part of the core body to dissolve or react by soaking in an acid solution, and escapes from the negative electrode material, so that the negative electrode material loses part of its mass. In this process, the carbon coating layer, which is relatively stable under the action of external force, still has a protective effect on the coated core body, thereby reducing the dissolution or reaction of part of the core body in the acid solution, and is retained in the negative electrode material, participating in the formation of the remaining mass of the negative electrode material. Therefore, the present application characterizes the "mass of the part of the core covered by the unstable carbon coating layer" in the negative electrode material by the part of the mass lost by the above-mentioned negative electrode material, and constructs the calculation formula of the above-mentioned residual carbon rate γ to further characterize the coating density of the carbon coating layer of the negative electrode material.
[0050] The present application further discovered that, under the premise that the negative electrode material has a certain amount of carbon coating to reduce the gas production, in the negative electrode material with the above-mentioned residual carbon rate γ less than or equal to 20%, the carbon coating layer has a better protective effect on the core body, so that the gas production behavior of the negative electrode material is significantly reduced, and the expansion effect is also significantly reduced. The cycle stability of the secondary battery based on this negative electrode material is significantly improved; and in the negative electrode material with a residual carbon rate γ less than or equal to 20%, the density of the carbon coating layer is also higher, and the arrangement between carbon atoms is close enough to form sufficient conductive channels and maintain the movement of electrons in the carbon layer, thereby maintaining good electrical conductivity. Materials with high electrical conductivity usually have better ion conductivity, which helps to reduce the internal resistance of the battery and improve the charging and discharging efficiency, thereby helping to improve the capacity and first coulombic efficiency of the resulting secondary battery. When the residual carbon rate γ is greater than 20%, the protective effect of the carbon coating on the core of the negative electrode material is reduced, resulting in intense gas production in the negative electrode material, and the density of the carbon layer is reduced, resulting in reduced efficiency of electrons passing through the carbon layer. As a result, the expansion effect of the negative electrode material cannot be effectively alleviated, reducing the cycle stability of the secondary battery, and the capacity and first coulomb efficiency of the secondary battery are also negatively affected to a certain extent.
[0051] The negative electrode material of the present application simultaneously satisfies the above-mentioned 10-day gas production A and residual carbon rate γ falling within the preset range. Such a setting can also avoid the phenomenon that the negative electrode material with a very low coating amount also has a low residual carbon rate γ, but the gas production of the negative electrode material with a very low coating amount is large and does not have good performance.
[0052] In some embodiments, the residual carbon rate γ of the negative electrode material is less than or equal to 10%, and the 10-day gas production A is less than or equal to 50 mL / kg. For example, the residual carbon rate γ of the negative electrode material can be 9%, 8%, 5%, 4%, 3% or any value within the range formed by any two of the above values; the 10-day gas production A can be 50 mL / kg, 30 mL / kg, 20 mL / kg, 5 mL / kg, 4 mL / kg, 3 mL / kg or any value within the range formed by any two of the above values. Negative electrode materials with a residual carbon rate γ less than or equal to 10% show a more reduced gas production behavior. At this time, the protective effect of the carbon coating layer coating the core body is more obvious, which can further reduce the contact between the core body and external substances. The 10-day gas production A of the negative electrode material is controlled within the above range, which shows that the negative electrode material itself has a certain coating amount, and on this basis, a coating layer with excellent density is formed through process improvement.
[0053] In some embodiments, the powder conductivity of the negative electrode material at 20kN is 0.5S / cm to 9.5S / cm. For example, the powder conductivity can be 0.5S / cm, 1.0S / cm, 1.5S / cm, 2.0S / cm, 3.0S / cm, 4.5S / cm, 5.5S / cm, 6.5S / cm, 7.5S / cm, 8.5S / cm, 9.5S / cm, or any value within the range formed by any two of the above values. The powder conductivity within the above range indicates that the negative electrode material has good electrical conductivity and good electron permeability in the carbon coating layer, which helps to improve the capacity and first coulomb efficiency of the resulting secondary battery.
[0054] In some embodiments, the ID / IG of the negative electrode material is 0.5 to 5.0. ID is the D peak intensity in the Raman spectrum of the negative electrode material, and IG refers to the G peak intensity in the Raman spectrum of the negative electrode material. The ID / IG value can be used to characterize the degree of surface defects of the negative electrode material. In the present application, when the ID / IG value meets the above range, it means that the degree of graphitization of the carbon material in the carbon coating layer is higher, that is, the carbon atoms are arranged more orderly, thereby forming more sp 2 Hybridized carbon atoms vibrate in the plane (G peak). This ordered structure is conducive to the transmission of electrons and improves the conductivity of the material. Since carbon atoms are rearranged to form a more stable layered structure during the carbonization process, which reduces voids and defects, the carbon coating with a higher degree of graphitization tends to have a tighter structure, that is, higher density. Therefore, controlling ID / IG within the above range is conducive to improving the density of the carbon coating, thereby helping to reduce the residual carbon rate γ.
[0055] In some embodiments, the specific surface area of the negative electrode material is less than or equal to 5 m 2 / g, specifically 0.5m 2 / g, 1m 2 / g, 1.5m 2 / g, 2m 2 / g, 2.5m 2 / g, 3m 2 / g, 3.5m 2 / g, 4m 2 / g, 4.5m 2 / g, 5m 2 / g or any value within the range formed by any two of the above values. It can be understood that the specific surface area of the negative electrode material will affect the contact area between the negative electrode material and the electrolyte. The specific surface area of the negative electrode material within the above range can reduce the amount of lithium ions consumed by the SEI film formed in the battery prepared by the negative electrode material during the first charge and discharge process, and reduce the irreversible capacity loss of the battery.
[0056] In some embodiments, the particle size D10 of the negative electrode material is 1 μm to 5 μm. For example, the particle size D10 of the negative electrode material can be 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, or any value within the range formed by any two of the above values.
[0057] In some embodiments, the particle size D50 of the negative electrode material is 6 μm to 16 μm. For example, the particle size D50 of the negative electrode material can be 6 μm, 6.5 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 14 μm, 16 μm, or any value within the range formed by any two of the above values.
[0058] In some embodiments, the particle size D90 of the negative electrode material is 16 μm to 24 μm. For example, the particle size D90 of the negative electrode material can be 16 μm, 16.5 μm, 17 μm, 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 24 μm, or any value within the range formed by any two of the above values.
[0059] The measured volume-based cumulative particle size distribution D10 represents the particle size corresponding to when the cumulative particle size distribution percentage of the powder reaches 10%, D50 represents the particle size corresponding to when the cumulative particle size distribution percentage reaches 50%, and D90 represents the particle size corresponding to when the cumulative particle size distribution percentage reaches 90%. When the particle size of the negative electrode material is within the above range, the diffusion path of lithium ions is short, which can ensure the time for lithium ion embedding and detachment, so that the negative electrode material can achieve a state of rapid and sufficient lithium embedding, thereby ensuring the charge and discharge performance of the battery. In addition, when the particle size distribution of the negative electrode material is within the above range, the large particles with larger particle size and the small particles with smaller particle size of the negative electrode material can cooperate with each other, and the small particles fill the pores between the large particles, thereby increasing the tap density of the negative electrode material, which is beneficial to increase the compactness between the positive electrode material particles, improve the transmission of active particles and the conduction of electrons, and increase the energy density of the resulting secondary battery, extend the cycle life, and improve safety performance.
[0060] In some embodiments, the thickness of the carbon coating layer is 10nm to 1000nm. For example, the thickness of the carbon coating layer can be 0.1nm, 0.5nm, 1nm, 30nm, 60nm, 100nm, 150nm, 200nm, 300nm, 500nm, 800nm, 1000nm or any value within the range formed by any two of the above values. The carbon coating layer can coat the active material exposed on the surface of the core body, reduce the direct contact between the active material and the electrolyte, thereby reducing the solubility of the negative electrode material, and reducing the gas production of the dissolved active material (such as silicon particles) and the electrolyte reaction, and reducing the risk of a large amount of SEI generated during the charge and discharge process due to the exposed active material. Controlling the thickness of the carbon coating layer within the above range is conducive to maintaining the stability of the particle structure of the negative electrode material during the cycle, and maintaining the good conductivity of the negative electrode material, thereby helping to improve the specific capacity and cycle stability of the resulting secondary battery.
[0061] In some embodiments, the carbon coating layer may be a single-layer carbon coating layer formed of the above single material, or a carbon coating layer formed of a combination of the above multiple materials, or a single-layer carbon coating layer, or a multiple-layer carbon coating layer, etc. The layer structure of the carbon coating layer may be selected according to actual needs. It is understandable that when the carbon coating layer is a multi-layer coating structure, its density is higher.
[0062] In some embodiments, the active material includes one or more of Si, Sn, Ge, Pb, Ag, Mg, Zn, Ga, In, Sb, Bi and alloys thereof.
[0063] In some embodiments, the active material includes a silicon material, the silicon material includes silicon particles, and the silicon particles include one of amorphous silicon, crystalline silicon, and a composite of crystalline silicon and amorphous silicon. When the active material includes a silicon material, the silicon material is used as a component of the negative electrode active material, which can increase the specific capacity of the negative electrode material, thereby increasing the energy density of the secondary battery. Preferably, the silicon material includes amorphous silicon. When the active material further includes amorphous silicon, the amorphous silicon expands isotropically during the lithium insertion process, which can reduce the collapse of the pores and thus help reduce the expansion effect, and can inhibit the rapid decay of the specific capacity of the negative electrode material, which is beneficial to improving the lithium insertion cycle performance of the negative electrode material, thereby helping to improve the first coulombic efficiency, capacity and cycle stability of the resulting secondary battery.
[0064] In some embodiments, the silicon material includes at least one of silicon oxide and a silicon alloy.
[0065] In some embodiments, the silicon material includes silicon particles and a silicon oxide layer located on the surface of the silicon particles. The silicon oxide layer includes silicon oxide, and the general formula of silicon oxide is SiOx, wherein 0.5≤x<2. Specifically, SiOx can be SiO0.5 、SiO 0.7 、SiO 0.9 、SiO、SiO 1.2 、SiO 1.5 、SiO 1.8 、SiO 1.9 Etc., not limited here. In some embodiments, taking the mass of the silicon material as 100%, the mass percentage of oxygen atoms in the silicon material is 1% to 18%. Specifically, the mass percentage of oxygen atoms in the silicon material can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18% or any value within the range formed by any two of the above values. Controlling the mass percentage of oxygen atoms in the silicon material within the above range is conducive to the formation of a stable silicon oxide layer on the surface of silicon particles, which can reduce the direct contact between silicon particles and the electrolyte, thereby reducing the side reaction between the silicon material and the electrolyte, and improving the cycle stability of the negative electrode material; it can also ensure that the silicon material has stable activity and improve the specific capacity of the negative electrode material.
[0066] In some embodiments, the active material includes silicon material, and the mass content of silicon in the negative electrode material is 35% to 55%, specifically 35%, 38%, 40%, 43%, 45%, 48%, 50%, 52%, 55%, or any value within the range formed by any two of the above values. When the mass proportion of silicon is within this range, the secondary battery can store a higher amount of electricity, that is, the first discharge specific capacity is higher.
[0067] In some embodiments, the average particle size of the active material is 0.1nm to 500nm. For example, the average particle size of the active material can be 0.1nm, 0.5nm, 1nm, 5nm, 10nm, 30nm, 50nm, 100nm, 150nm, 200nm, 300nm, 400nm, 500nm or any value within the range formed by any two of the above values. For example, the active material can be a silicon material, i.e., silicon particles. By setting the average particle size of the silicon particles within the above range, the mechanical stress of the silicon particles when the volume expands can be reduced, so that the secondary battery maintains a good battery capacity, and reduces the irreversible capacity loss, and can also shorten the electron and ion transmission path. At the same time, the size of the silicon particles is reduced, and the gap between adjacent silicon particles is increased, which can reserve space for the volume expansion of the silicon particles, which helps to reduce the risk of pulverization and breakage of the resulting negative electrode material due to the expansion effect.
[0068] In some embodiments, the morphology of the silicon particles includes at least one of a dot shape, a sphere shape, an ellipsoid shape, and a flake shape.
[0069] In some embodiments, the purity of the silicon particles is greater than 99%. High-purity silicon particles are more conducive to Li-Si alloying with lithium, thereby improving the cycle performance of lithium-ion batteries.
[0070] In some embodiments, the total pore volume of the matrix is 0.5 cm 3 / g to 2.0cm 3 / g. For example, the total pore volume of the matrix can be 0.5 cm 3 / g, 0.8cm 3 / g, 1cm 3 / g, 1.2cm 3 / g, 1.5cm 3 / g, 1.8cm 3 / g, 2.0cm 3 / g or any value within the range formed by any two of the above values. The total pore volume of the matrix within the above range indicates that the matrix has abundant pores, which can accommodate the active material and reserve space for the volume expansion of the accommodated active material, thereby effectively reducing the risk of pulverization and crushing of the obtained negative electrode material due to the expansion effect.
[0071] In some embodiments, the total pore volume of the negative electrode material is 0.001 cm 3 / g to 0.1cm 3 For example, the total pore volume of the negative electrode material can be 0.001 cm 3 / g, 0.002cm 3 / g, 0.005cm 3 / g, 0.008cm 3 / g, 0.01cm 3 / g, 0.02cm 3 / g, 0.03cm 3 / g, 0.04cm 3 / g, 0.05cm 3 / g, 0.06cm 3 / g, 0.07cm 3 / g, 0.08cm 3 / g, 0.09cm 3 / g, 0.1cm 3 / g or any value within the range formed by any two of the above values.
[0072] Compared with the negative electrode material after removing the active substance such as silicon particles, that is, the matrix, the pore volume of the negative electrode material containing the active substance is significantly reduced, indicating that the density of the negative electrode material is increased, and the specific capacity of the negative electrode material can be effectively improved. The present application controls the total pore volume of the negative electrode material filled with active substances such as silicon particles and the negative electrode material after removing the active substances such as silicon particles within the above range, which can not only improve the specific capacity of the negative electrode material, but also ensure that the negative electrode material can reserve an appropriate amount of pores to alleviate the volume expansion caused by the process of active substances such as silicon particles and lithium insertion, which is beneficial to improve the cycle performance of the negative electrode material.
[0073] In some embodiments, taking silicon particles as the active material as an example, 150 mL of a 20% mass fraction HF acid solution is dripped dropwise into 10 g of a negative electrode material under stirring, which will produce SiF4 and H2 gases and release heat. After no gas is generated, the supernatant acid solution is removed by centrifugation, and 150 mL of a 20% mass fraction HF acid solution is added to the negative electrode material again. After stirring for 12 hours, the supernatant acid solution is removed by centrifugation again, and then the negative electrode material is washed with pure water until it is neutral and dried to obtain the negative electrode material after removing the silicon material, i.e., the matrix.
[0074] In some embodiments, the average pore size of the pores of the negative electrode material is 0.5 nm to 20 nm. Specifically, the average pore size of the pores of the negative electrode material can be 0.5 nm, 0.8 nm, 1.0 nm, 1.3 nm, 1.5 nm, 1.8 nm, 2.0 nm, 3.0 nm, 4.0 nm, 5.0 nm, 6.0 nm, 7.0 nm, 10 nm, 12 nm, 15 nm, 18 nm, 20 nm, or any value within the range formed by any two of the above values. Controlling the average pore size of the pores in the negative electrode material is beneficial to buffering the volume expansion of the active material and improving the structural stability of the negative electrode material while improving the rate performance of the negative electrode material.
[0075] In some embodiments, the compaction density of the negative electrode material is 0.8 g / cm 3 Up to 1.2g / cm 3 , specifically 0.8g / cm 3 , 0.9g / cm 3 , 1.0g / cm 3 , 1.1g / cm 3 , 1.2g / cm 3 Or any value within the range formed by any two of the above values.
[0076] In some embodiments, the pores in the negative electrode material include micropores, wherein the volume proportion of the micropores in all pores is less than or equal to 5%. In some embodiments, the pores in the negative electrode material include mesopores, wherein the volume proportion of the mesopores in all pores is 87% to 97%. In some embodiments, the pores in the negative electrode material include macropores, wherein the volume proportion of the macropores in all pores is less than or equal to 13%.
[0077] Understandably, since active substances such as silicon particles fill a large number of pores in carbon materials, especially micropores, the pores of the negative electrode material are mainly mesopores and macropores. Understandably, since the molecular size generated by the electrolyte is generally less than or equal to the pore size of the micropores, under the action of the strong capillary adsorption capacity of the micropores, the adsorption capacity of the negative electrode material is largely proportional to the pore volume of the micropores. For example, as the volume of the micropores increases, the adsorption capacity of the negative electrode material increases, thereby increasing the side reactions between the negative electrode material and the electrolyte. Therefore, the volume proportion of micropores, mesopores, and macropores in the negative electrode material is controlled within this range, which can improve the uniformity of the distribution of silicon materials inside the negative electrode material. Specifically, the micropores are basically filled with active substances, and most of the remaining pores are mesopores, which can effectively alleviate the volume expansion of the active substances and reduce the excessive local expansion stress of the negative electrode material due to the uneven volume change of the active substances during the cycle, resulting in the rupture and pulverization of the negative electrode material.
[0078] In some embodiments, the specific surface area of the substrate is 600 m 2 / g to 3000m 2 / g. The matrix that meets the above specific surface area range has well-developed pores and a large number of micropores, which is conducive to the deposition of active substances.
[0079] In some embodiments, the matrix includes a carbon matrix, and the carbon matrix includes one or more of amorphous carbon, graphitized carbon, mesocarbon microspheres, and carbon gel. The carbon matrix is selected from the above materials, which can provide distribution sites for active substances and form a conductive network.
[0080] In some embodiments, the matrix includes a carbon matrix, and the mass content of carbon elements in the negative electrode material is 40% to 60%, specifically 40%, 42%, 43%, 45%, 48%, 50%, 52%, 55%, 57%, 59%, 60% or any value within the range formed by any two of the above values. Among them, the carbon element includes a carbon matrix and a carbon coating. When the mass proportion of the carbon element is within this range, a sufficient carbon-based substrate can be established to provide sufficient distribution sites for the active material, which is conducive to forming an effective conductive network and improving electrical conductivity and cycle stability. In some embodiments, the matrix includes a non-carbon matrix, and the non-carbon matrix includes one or more of metal oxides, silicides, silicates, phosphates, titanates and aluminum borates. The non-carbon matrix adopts the above materials, which can play the role of supporting the skeleton, and compared with the existing conductive carbon matrix, the non-carbon matrix used in this application has better strength and rigidity, so that the negative electrode material can have a higher compaction density during the battery preparation process, which can improve the structural stability of the negative electrode material, reduce the particle crushing and pulverization of the negative electrode material, and is conducive to improving the cycle performance of the negative electrode material. At the same time, the non-carbon matrix usually has good ionic conductivity due to its electronic insulation, which can play a role similar to that of an artificial SEI film, can slow down the formation of subsequent natural SEI films, reduce the direct contact between the negative electrode material and the electrolyte, and reduce the occurrence of side reactions. In addition, the non-carbon matrix has a lower cost advantage than the carbon matrix. The existing carbon matrix has a high energy consumption and environmental cost due to the complexity of the activation pore-forming process; and if a porous ceramic or other material with natural porous pores is used, the pore-forming process is omitted, so that the cost can be significantly reduced compared to the porous carbon matrix.
[0081] The negative electrode material active layer also includes a binder to bind the negative electrode active material particles to facilitate the formation of a film layer, and can also improve the binding force between the negative electrode material active layer and the negative electrode current collector. In some embodiments, the binder may include but is not limited to polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylic (ester) styrene butadiene rubber, epoxy resin or nylon, etc.
[0082] The negative electrode material active layer may also include a conductive material, including but not limited to a carbon-based material, a metal-based material, a conductive polymer, or any combination thereof. In some embodiments, the carbon-based material may include but is not limited to natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, the metal-based material may include but is not limited to metal powder or metal fiber, such as copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer may be a polyphenylene derivative.
[0083] Isolation film
[0084] The isolation membrane 103 includes a membrane layer with a porous structure, and its material includes but is not limited to at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide or aramid. For example, the isolation membrane 103 can be a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite membrane.
[0085] Electrolytes
[0086] The electrolyte has the function of conducting ions between the positive electrode sheet 101 and the negative electrode sheet 102. The state of the electrolyte can be one or more of a gel state, a solid state and a liquid state. In some embodiments, the electrolyte is an electrolyte. The electrolyte plays the role of conducting active ions between the positive electrode sheet 101 and the negative electrode sheet 102. In some embodiments, the electrolyte includes a lithium salt and an organic solvent. The lithium salt can be selected from but not limited to lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium perchlorate (LiClO4), lithium tetraphenylborate (LiB(C6H5)4), lithium methanesulfonate (LiCH3SO3), lithium bis(trifluoromethanesulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethylsulfonyl)imide (LiN(SO2CF3)2, tris(trifluoromethylsulfonyl)methyl lithium (LiC(SO2CF3)3), lithium bis(oxalatoborate) (LiBOB) and lithium difluorophosphate (LiPO2F2) One or more. For example, the lithium salt is selected from LiPF6 because it can give high ionic conductivity and improve cycle characteristics. The organic solvent can be a carbonate compound, a carboxylate compound, an ether compound, Compounds, nitrile compounds, other organic solvents or combinations thereof. Examples of carbonate compounds include, but are not limited to, diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), ethylmethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylethylene carbonate (VEC), fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate or combinations thereof.
[0087] Another embodiment of the present application further provides a method for preparing a negative electrode material, comprising:
[0088] The first step: activating the matrix precursor material to obtain a porous matrix.
[0089] In some embodiments, the matrix precursor material includes one or more of nutshell carbon, straw carbon, resin carbon, pitch carbon and sugars. A porous carbon matrix can be obtained based on the above materials.
[0090] In some embodiments, the activation treatment includes one of water vapor activation and carbon dioxide activation, and the activation treatment includes introducing water vapor or carbon dioxide gas under high temperature conditions, and forming a porous material through subsequent treatment.
[0091] In some embodiments, before the base precursor material is activated, the base precursor material is also pre-carbonized, including heat treating the base precursor material at 300°C to 500°C for about 3 hours to break the material. Pre-carbonization is beneficial to making the material structure more stable, thereby improving the quality and performance of the subsequent activated product. Breaking the pre-carbonized material is beneficial to expanding the contact area of the material in the subsequent activation treatment, improving the activation effect, and obtaining a porous material with good performance.
[0092] In some embodiments, the temperature of the activation treatment is 800°C to 1100°C. In some embodiments, the pressure of the activation treatment is 0.01 kPa to 10 kPa. In some embodiments, the total airflow of the activation treatment is 10 L / min to 100 L / min. In some embodiments, the activation treatment lasts for about 12 hours. In some embodiments, subsequent treatment includes acid washing, water washing, drying, crushing and screening.
[0093] Step 2: Compound the porous matrix with the active material to obtain a core body.
[0094] In some embodiments, the composite of the porous matrix and the active material comprises vapor deposition, including mixing the porous matrix with a vapor carrier of the active material under high temperature conditions, decomposing the vapor carrier of the active material at high temperature, and depositing the active material components on the porous matrix.
[0095] In some embodiments, the vapor deposition is performed in a plasma enhanced chemical vapor deposition device, and the reaction conditions of the vapor deposition include a pressure of 1.0 kPa to 10.0 kPa, a microwave operating frequency of 2.5 GHz, a power of 2600 W to 3200 W, a temperature of 400° C. to 700° C., and a total gas flow rate of 50 Sccm to 500 Sccm. In some embodiments, the vapor deposition is performed in an inert gas atmosphere.
[0096] The third step: In a plasma enhanced chemical vapor deposition device, under the conditions of a rotation frequency of 5 Hz to 40 Hz and a temperature of 550°C to 700°C, the core body is mixed with a reaction gas, the reaction gas includes an inert gas and a gaseous carbon source, and the concentration of the gaseous carbon source in the reaction gas is 10% to 70%, so that the gaseous carbon source is cracked to form a carbon coating layer to obtain a coated core body.
[0097] During the above-mentioned coating process, the rotational speed frequency of the equipment will affect the deposition effect during the coating process. When the reactor speed is too slow, heat will be concentrated when acetylene is cracked, and the local temperature will be higher than the set value, which will cause the material crystal form to change to crystal. Although the density of the coating layer is improved, the performance of the negative electrode material is reduced; when the reactor speed is too fast, the collision between particles is intensified, and the violent collision is easy to destroy part of the coating layer structure that has been formed, or make it difficult for the carbon source to be cracked and deposited uniformly on the surface of the particles, thereby affecting the growth of the coating layer and the density of the coating layer. Therefore, controlling the rotational speed frequency of the above-mentioned equipment within the above-mentioned range is conducive to maintaining the crystal form of the material and promoting the growth and density of the coating layer, thereby reducing the residual carbon rate. It can be understood that controlling the reaction temperature within the above-mentioned range is also conducive to maintaining the crystal form of the material, such as maintaining the silicon material as amorphous silicon, and improving the density of the coating layer, which is conducive to reducing the residual carbon rate.
[0098] At the same time, the concentration of the gaseous carbon source in the reaction gas will also affect the deposition effect during the coating process. When the concentration of the gaseous carbon source is too low, the coating amount is insufficient, the performance improvement of the material is limited, and a longer coating treatment time is required. When the concentration of the gaseous carbon source is too high, the carbon source cracking is more intense, and the carbon source decomposes in large quantities in a short period of time. On the one hand, it may cause excess carbon source in some areas, forming an overly thick coating layer, while other areas may not be fully coated due to insufficient carbon source, forming a thinner coating layer or even a bare area; on the one hand, a large amount of gas and impurities may also be generated. If these gases and impurities cannot be effectively discharged during the formation of the coating layer, defects such as pores and cracks will be formed, thereby reducing the quality and density of the coating layer; on the other hand, since the carbon source needs to interact with the surface of the substrate during the coating process (such as chemical bonding, adsorption, etc.) to form a strong coating layer, this violent cracking may destroy this interaction, causing the bonding force between the coating layer and the substrate to decrease, affecting the stability and performance of the coating layer.
[0099] In some embodiments, in a plasma enhanced chemical vapor deposition device, the coating treatment conditions also include a pressure of 5.0 kPa to 20.0 kPa, a microwave operating frequency of 2.0 GHz to 2.5 GHz, a power of 2500 W to 3500 W, and a total gas flow rate of 50 Sccm to 500 Sccm.
[0100] In some embodiments, the gas-phase carbon source includes one or more of methane, acetylene, propylene, benzene, ethanol, methanol, ethylene, propane, and butane.
[0101] Step 4: crush and screen the coated core to obtain the negative electrode material.
[0102] The scheme of the present application will be explained below in conjunction with the embodiments. Those skilled in the art will understand that the following examples are only used to explain the present application and cannot be construed as limiting the present application. Unless otherwise stated, the reagents, software and instruments not specifically stated in the following embodiments are all conventional commercial products or open source.
[0103] Embodiment 1:
[0104] A negative electrode material based on a carbon matrix and silicon particles, the preparation method comprising:
[0105] S1, place 10kg of fruit shell carbon in a kiln, heat it to 300℃ to 500℃, pre-carbonize it for 3h, and crush it mechanically. Place the crushed material in a reaction furnace, set the pressure to 0.01kpa to 10.0kpa, and introduce water vapor at 900℃ with a total airflow of 30L / min. The reaction time is 12h. After the reaction is completed, the reaction material is pickled, washed with water, dried, crushed, and sieved to obtain a porous carbon precursor.
[0106] S2, place 100g of porous carbon precursor in a reactor, set the pressure to 1.0kPa to 10.0kPa, the microwave operating frequency to 2.5GHz, and the power range to 3000W; when the reactor temperature reaches 500℃, introduce nitrogen and disilane, the concentration of disilane is 30%, the total gas flow rate is 300Sccm, and the holding time is 6h to obtain a core body.
[0107] S3, placing the core body in a reactor, setting the pressure to 5.0 kPa to 20.0 kPa, the microwave operating frequency to 2.0 GHz, the power range to 3000 W, and the rotation speed frequency to 15 Hz; when the reactor temperature reaches 550 ° C, nitrogen and acetylene are introduced, the acetylene concentration is 30%, the total gas flow rate is 200 Sccm, and the holding time is 6 hours to obtain a coated core body.
[0108] S4, screening and grading the obtained coated core bodies to obtain negative electrode materials.
[0109] Embodiment 2:
[0110] The difference from Example 1 is that in S3, the ultimate temperature of the reactor is adjusted to 600°C.
[0111] Embodiment 3:
[0112] The difference from Example 1 is that in S3, the ultimate temperature of the reactor is adjusted to 650°C.
[0113] Embodiment 4:
[0114] The difference from Example 1 is that in S3, the ultimate temperature of the reactor is adjusted to 700°C.
[0115] Embodiment 5:
[0116] The difference from Example 3 is that in S3, the concentration of acetylene is adjusted to 10% and the holding time is adjusted to 18 hours.
[0117] Embodiment 6:
[0118] The difference from Example 3 is that in S3, the concentration of acetylene is adjusted to 50%, and the holding time is adjusted to 3.6 h.
[0119] Embodiment 7:
[0120] The difference from Example 3 is that in S3, the concentration of acetylene is adjusted to 70%, and the holding time is adjusted to 2.6 h.
[0121] Embodiment 8:
[0122] The difference from the third embodiment is that in S3, the rotation speed frequency is adjusted to 5 Hz.
[0123] Embodiment 9:
[0124] The difference from the third embodiment is that in S3, the rotation speed frequency is adjusted to 25 Hz.
[0125] Embodiment 10:
[0126] The difference from the third embodiment is that in S3, the rotation speed frequency is adjusted to 40 Hz.
[0127] Embodiment 11:
[0128] The difference from Example 3 is that in S3, the microwave operating frequency is 2.5 GHz and the power range is 3500 W.
[0129] Comparative Example 1:
[0130] The difference from Example 1 is that in S3, the ultimate temperature of the reactor is adjusted to 480°C.
[0131] Comparative Example 2:
[0132] The difference from Example 7 is that in S3, the concentration of acetylene is adjusted to 90%, and the holding time is adjusted to 2 hours.
[0133] Comparative Example 3:
[0134] The difference from Example 10 is that in S3, the rotation speed frequency is adjusted to 50 Hz.
[0135] The physical and electrochemical properties of the negative electrode materials obtained in the above examples 1-11 and comparative examples 1-3 were tested, and the testing methods were as follows:
[0136] 1. γ test of residual carbon rate of negative electrode material:
[0137] (1) The negative electrode material is placed in a slurry stirring tank and stirred at a frequency of 50 Hz for 1 h. The stirred negative electrode material having a mass of m1 is taken out and placed in a hydrofluoric acid solution having a mass fraction of 20% for 1 h. The soaked negative electrode material is taken out, washed and dried, and the mass is measured to be m2;
[0138] (2) Take a negative electrode material with a mass of m1 and soak it in a hydrofluoric acid solution with a mass fraction of 20% for 1 hour. Take out the soaked negative electrode material, wash and dry it, and measure the mass of m3;
[0139] (3) Calculate the residual carbon rate of the negative electrode material
[0140] 2. Gas production A test of negative electrode materials:
[0141] Place 50 g of negative electrode material in a 300 mL slurry stirring tank, add 50 g of 5% sodium carboxymethyl cellulose and 100 mL of pure water into the stirring tank, stir at a frequency of 50 Hz and for 1 h to obtain slurry, place the slurry in an aluminum-plastic film, and measure the 10-day gas production A of the slurry by the drainage method.
[0142] 3. Powder conductivity test of negative electrode material:
[0143] Place 3g of powdered negative electrode material in an 80℃ drying oven to fully dry, shake and mix the dried powdered negative electrode material, take 2g of the treated powdered negative electrode material and apply a force of 20kN for 30s to press it into a disc. Use a digital vernier caliper to measure the thickness of the sample and record it. Select the PRCD2110 powder resistivity of Yuanneng Technology Co., Ltd. and place the pressed disc-shaped sample on the test bench of the four-probe tester. Place the four probes of the four-probe tester at different positions on the surface of the sample. Start the test program according to the operating instructions of the four-probe tester. The tester will automatically apply a certain current to the current probe and measure the voltage response on the sample through the voltage probe. Then use physical formulas such as Ohm's law to calculate the resistivity or conductivity of the sample.
[0144] 4. ID / IG test of negative electrode material:
[0145] Take 100 mg of negative electrode material sample, which is dry, stable, non-volatile and non-toxic. Before testing, calibrate the Raman spectrometer to ensure the accuracy of the test results. Place the sample on the sample stage of the Raman spectrometer. Set appropriate test parameters, such as laser wavelength of 532 nm. Start the Raman spectrometer Anton Paar Cora 5X00 series and perform a spectral scan. Record the Raman spectrum obtained from the test, find the positions of the D peak and the G peak in the spectrum, and measure their intensities. Calculate the ID / IG value, which is the ratio of the D peak intensity to the G peak intensity. Judge the disorder of the negative electrode material according to the size of the ID / IG value.
[0146] 5. Particle size D10, D50, D90 test of negative electrode materials:
[0147] Take 1 g of the powdered negative electrode material and dissolve it in 30 mL of pure water. Ultrasonic oscillate for 2 minutes. Pour the mixed solution after ultrasonic oscillation into the measuring cylinder of the Malvern 3000 test instrument, start the test instrument, and obtain the particle size distribution data.
[0148] 6. Test of average particle size of active material and thickness of carbon coating layer of negative electrode material:
[0149] The JEM-2100F testing instrument of JEOL Ltd. was selected to test the TEM image of the material at high magnification. The particle size in the TEM image was statistically analyzed to obtain the average particle size. The carbon layer on the outer layer of the particles in the TEM image was statistically analyzed. There was a clear boundary between the outer layer of the particles in the TEM image. The outermost layer was the carbon coating layer. The thickness of the carbon coating layer was statistically analyzed. 10 mg of the material was properly processed and prepared, dissolved in alcohol, titrated, dried, fixed, and ultra-thinly sliced to ensure that the sample was suitable for TEM observation. A special sample fixture was used to load the processed sample onto the sample stage of the TEM, and the position and angle of the sample were adjusted to make it suitable for electron beam irradiation. Start the TEM system and vacuum it after initialization. Adjust the brightness, focus, magnification and other parameters of the electron gun. Calibrate the operating voltage and current of the instrument to ensure that the equipment is in the best working condition. Use the focusing device of the TEM system to adjust the focus of the sample to obtain a clear TEM image.
[0150] 7. Pore volume, proportion and specific surface area test of negative electrode material and matrix:
[0151] Using the ASAP 2425 Microbead tester, 0.5 g of the material was degassed. After degassing, it was placed in the test instrument and the test instrument was started. After the program was completed, the analysis of the adsorption and desorption isotherms made it possible to determine the pore volume and pore size distribution, as well as the proportion of the pore volume of micropores, mesopores and macropores in the total pore volume and the specific surface area.
[0152] 8. Test method for mass content of carbon: Using the G4 ICARUS HF infrared carbon-sulfur analyzer from Bruker, Germany, the sample is burned under high temperature and oxygen-rich conditions, and the carbon element it contains is oxidized into carbon dioxide. The generated gas enters the infrared detector with the carrier gas, and the carbon content can be calculated by quantitatively analyzing the changes in the carbon dioxide signal.
[0153] 9. Test method for mass content of silicon element: Use Nanyang Xinyu's SA2-9-17TP box-type atmosphere furnace to burn in an oxygen atmosphere, so that the silicon in the sample reacts into silicon dioxide, and the carbon burns into carbon dioxide and is discharged. The silicon content is calculated by weighing.
[0154] 10. Electrochemical related performance test:
[0155] (1) Assembling lithium-ion button cells:
[0156] Mix polyacrylic acid and sodium carboxymethyl cellulose in a mass ratio of 1:1, add a certain amount of pure water, and stir magnetically for 6-12 hours to obtain a binder;
[0157] According to the mass ratio of silicon composite material, conductive agent and binder of 70:15:15, the silicon composite material and conductive agent are added to the binder, and magnetic stirring is performed for 6-12 hours to obtain a slurry;
[0158] The slurry is evenly coated on the copper foil, and after drying, it is sliced and dried to obtain a silicon composite material electrode sheet;
[0159] Assemble button cells, using CR2032 battery shells, lithium metal sheets as counter electrodes, and 1M LiPF6 as electrolyte.
[0160] (2) Capacity and first coulombic efficiency test: The button cell was placed in the mold clamp of the high-precision battery testing system and allowed to stand for 12 hours. The discharge test conditions were a discharge current of 0.1C, a rated capacity of 1000mAh, and a discharge cut-off voltage of 5mV. The charge test conditions were a discharge current of 0.1C, a rated capacity of 1000mAh, and a discharge cut-off voltage of 1.5V. The capacity and first coulombic efficiency of the button cell were tested using a high-precision battery testing system.
[0161] (3) Cycle retention rate: The button cells with the above-mentioned test capacity and initial coulombic efficiency are subjected to a 1 C charge-discharge cycle stability test. The capacity ratio at the 50th week and the 1st week is the cycle retention rate.
[0162] (4) Expansion rate: For button cells with the above-mentioned test capacity and initial coulombic efficiency, a 1 C charge-discharge cycle stability test is performed, and the ratio of the thickness of the electrode at the 50th week to the original electrode thickness is the expansion rate.
[0163] Please refer to Table 1 for some of the preparation conditions of the above Examples 1-11 and Comparative Examples 1-3, and see Table 2 for the above test results.
[0164] Table 1. Partial preparation conditions in step S3 of Examples 1-11 and Comparative Examples 1-3 of the present application
[0165] Example Speed frequency(Hz) The reactor temperature reached (℃) Acetylene concentration (%) Time (h) Example 1 15 550 30 6 Example 2 15 600 30 6 Example 3 15 650 30 6 Example 4 15 700 30 6 Example 5 15 650 10 18 Example 6 15 650 50 3.6 Example 7 15 650 70 2.6 Example 8 5 650 30 6 Example 9 25 650 30 6 Example 10 40 650 30 6 Embodiment 11 15 610 30 6 Comparative Example 1 15 480 30 6 Comparative Example 2 15 650 90 2 Comparative Example 3 50 650 30 6
[0166] Table 2. Performance test results of Examples 1-11 and Comparative Examples 1-3 of the present application
[0167]
[0168] Under the improved preparation process conditions, the residual carbon rate γ of the negative electrode materials of Examples 1-11 of the present application is in line with the preset range, and the carbon coating layer of these negative electrode materials has a better protective effect on the core body, so that the slurry gas production of these negative electrode materials is effectively reduced. Among them, Example 11 increases the microwave frequency and power, which is conducive to reducing the cracking temperature of silane and acetylene. Therefore, the sample prepared by adjusting the temperature to 610°C in Example 11 is basically consistent with the performance of the sample prepared by the cracking temperature of 650°C in Example 3. Therefore, the expansion effect of the negative electrode materials of Examples 1-11 after being made into negative electrode sheets is alleviated, and the secondary batteries prepared have better cycle stability. At the same time, the carbon coating layers of these negative electrode materials have good compactness, which enables electrons to maintain good carbon layer permeability, so that these negative electrode materials have higher capacity and first coulomb efficiency after being made into secondary batteries.
[0169] Compared with Example 1, Comparative Example 1 lowers the temperature of the coating treatment. Too low a temperature leads to reduced efficiency of carbon source cracking, affecting the growth of the coating layer, affecting the coating amount in the negative electrode material, and not conducive to forming a uniform and dense coating layer. The residual carbon rate of the negative electrode material does not meet the preset range, resulting in increased gas production, higher expansion rate, and reduced cycle stability of the obtained negative electrode material.
[0170] Compared with Example 7, Comparative Example 2 increases the concentration of the carbon source. Excessive carbon source leads to intensified and concentrated cracking of the carbon source, which is not conducive to forming a uniform and dense coating layer, resulting in the residual carbon rate not meeting the preset range, and the gas production of the obtained negative electrode material increases, the expansion rate is higher, and the cycle stability performance is reduced.
[0171] Compared with Example 10, Comparative Example 3 increases the rotation speed frequency in the coating treatment. Excessively high rotation speed frequency leads to intensified collisions between particles and is not conducive to the formation of a uniform and dense coating layer, resulting in a residual carbon rate that does not meet the preset range. The gas production of the obtained negative electrode material increases, the expansion rate is higher, and the cycle stability performance decreases.
[0172] The above implementation modes are only used to illustrate the technical solutions of the present application and are not intended to limit the present application. Although the present application has been described in detail with reference to the above preferred implementation modes, a person skilled in the art should understand that the technical solutions of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present application.
Claims
1. A negative electrode material, comprising a core body and a carbon coating layer covering at least a portion of the surface of the core body, wherein the core body comprises a matrix and an active substance, It is characterized in that The gas production A of the negative electrode material in 10 days is less than or equal to 100 mL / kg; Define the residual carbon rate of the negative electrode material The residual carbon rate γ is less than or equal to 20%; The test method of the 10-day gas production A comprises: placing 50 g of the negative electrode material in a 300 mL slurry stirring tank, adding 50 g of 5% sodium carboxymethyl cellulose and 100 mL of pure water into the stirring tank, stirring at a frequency of 50 Hz and a stirring time of 1 hour to obtain a slurry, placing the slurry in an aluminum-plastic film, and measuring the 10-day gas production A of the slurry by a drainage method; m 2 The testing method includes: placing the negative electrode material in a slurry stirring tank and stirring, the stirring frequency is 50 Hz, the stirring time is 1 hour, and the mass taken out is m 1 The stirred negative electrode material is placed in a hydrofluoric acid solution with a mass fraction of 20% and immersed for 1 hour. The immersed negative electrode material is taken out, washed and dried, and the mass is measured to be m 2 ; m 3 The test method includes: taking the mass m 1 The negative electrode material is placed in a hydrofluoric acid solution with a mass fraction of 20% and immersed for 1 hour. The negative electrode material after immersion is taken out, washed and dried, and the mass is measured to be m 3 .
2. The negative electrode material according to claim 1, It is characterized in that The powder conductivity of the negative electrode material at 20 kN is 0.5 S / cm to 9.5 S / cm.
3. The negative electrode material according to claim 1, It is characterized in that The ID / IG of the negative electrode material is 0.5 to 5.
0.
4. The negative electrode material according to claim 1, It is characterized in that The negative electrode material satisfies at least one of the following conditions: (1) The specific surface area of the negative electrode material is less than or equal to 5 m 2 / g; (2) The total pore volume of the negative electrode material is 0.001 cm 3 / g to 0.1cm 3 / g; (3) The compaction density of the negative electrode material is 0.8 g / cm 3 Up to 1.2g / cm 3 ; (4) The negative electrode material includes micropores, mesopores and macropores. Based on the total pore volume of the negative electrode material, the volume proportion of the micropores is less than or equal to 5%, the volume proportion of the mesopores is 87% to 97%, and the volume proportion of the macropores is less than or equal to 13%; (5) The particle size D10 of the negative electrode material is 1 μm to 5 μm, the particle size D50 of the negative electrode material is 6 μm to 16 μm, and the particle size D90 of the negative electrode material is 16 μm to 24 μm.
5. The negative electrode material according to claim 1, It is characterized in that The carbon coating layer has a thickness of 10 nm to 1000 nm.
6. The negative electrode material according to claim 1, It is characterized in that The active substance meets at least one of the following conditions: (1) The active material includes one or more of Si, Sn, Ge, Pb, Ag, Mg, Zn, Ga, In, Sb, Bi and their alloys; (2) The active material includes silicon material, the silicon material includes silicon particles, and the silicon particles include one of amorphous silicon, crystalline silicon, and a composite of crystalline silicon and amorphous silicon; (3) The active material includes a silicon material, and the silicon material includes at least one of silicon oxide and a silicon alloy; (4) The active material includes a silicon material, the silicon material includes silicon particles and a silicon oxide layer located on the surface of the silicon particles, and the silicon oxide layer includes silicon oxide; (5) The average particle size of the active substance is 0.1 nm to 500 nm.
7. The negative electrode material according to claim 1, It is characterized in that The substrate satisfies at least one of the following conditions: (1) The total pore volume of the matrix is 0.5 cm 3 / g to 2.0cm 3 / g; (2) The specific surface area of the substrate is 600 m 2 / g to 3000m 2 / g; (3) The matrix includes a carbon matrix, and the carbon matrix includes one or more of amorphous carbon, graphitized carbon, mesophase carbon microspheres and carbon gel; (4) The matrix includes a non-carbon matrix, and the non-carbon matrix includes one or more of metal oxides, silicides, silicates, phosphates, titanates and aluminum borates.
8. The negative electrode material according to claim 1, It is characterized in that The matrix of the negative electrode material includes a carbon matrix, the active material of the negative electrode material includes a silicon material, and the negative electrode material further satisfies at least one of the following conditions: (1) Based on the mass of the negative electrode material, the mass proportion of carbon element in the negative electrode material is 40% to 60%; (2) Based on the mass of the negative electrode material, the mass of silicon element in the negative electrode material accounts for 35% to 55%.
9. A negative electrode sheet comprising a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, It is characterized in that The negative electrode active material layer comprises the negative electrode material according to any one of claims 1 to 8.
10. A secondary battery, It is characterized in that Comprising the negative electrode sheet as claimed in claim 9.
Citation Information
Patent Citations
Preparation method and application of amorphous silicon-based negative electrode material
CN116281943A
High-rate artificial graphite negative electrode material and preparation method thereof, lithium ion battery and power-related equipment
CN118306982A
Livestock growth status monitoring method and system for each individual
KR102615495B1
Silicon-based composite material, preparation method therefor and application thereof
WO2022204979A1
Cited By
Negative electrode material and battery
WO2025236650A1
Negative electrode material and battery
WO2026157366A1