A method for preparing high specific surface area silica from yellow phosphorus slag and silica itself
High specific surface area silica was prepared by deep acid hydrolysis with concentrated acid, alkali dissolution and temperature-controlled acid precipitation, which solved the problem of insufficient utilization of yellow phosphorus slag resources and realized the preparation of high performance silica and its application in new energy vehicle tires.
Patent Information
- Application Number
- CN202611081575.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies are insufficient to effectively utilize yellow phosphorus slag to produce high-performance silica, resulting in resource waste and low profit margins. Furthermore, the growing demand for traditional silica in new energy vehicle tires remains unmet.
High specific surface area silica was prepared by a method of deep acid hydrolysis with concentrated acid, preparation of sodium silicate solution by alkali dissolution, dilution and temperature-controlled acid precipitation and ripening. The specific steps include reaction of concentrated acid with yellow phosphorus slag, heating, filter cake washing, alkali dissolution and mixing, dilution, temperature-controlled acid precipitation and post-treatment to obtain silica with high specific surface area.
The prepared silica has a significantly increased specific surface area, reaching over 600 m²/g, making it suitable as a reinforcing filler for green tires in new energy vehicles. This solves the resource utilization problem and enhances product value.
Smart Images

Figure CN123105656A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of silica preparation technology, specifically relating to a high specific surface area silica and its preparation method, particularly a method for preparing high specific surface area silica using yellow phosphorus slag as raw material and silica. Background Technology
[0002] Yellow phosphorus slag is rich in active CaO and SiO2 (over 40%), and after water quenching, it possesses potential cementitious properties, making it suitable for use as a raw material in cement production or as an admixture in concrete. However, the cement industry is currently facing a dilemma of overcapacity while demand continues to decline. Simultaneously, cement prices are decreasing year by year, resulting in low profit margins. Exploring high-value-added applications of yellow phosphorus slag in other industries could serve as a new breakthrough for the future.
[0003] Currently, the demand for silica is mainly concentrated in the tire industry, and the focus of tire demand is gradually shifting from traditional rubber to green tires. The proportion of silica added to new energy vehicle tires reaches 25%-35%, higher than the 15%-25% in traditional tires, with a per-tire usage 15%-20% higher. Despite overall demand growth, the industry faces the problem of being "large but not strong": there is overcapacity in low-end general-purpose products, with an operating rate of only about 78%; while the capacity utilization rate of high-end grades is less than 60%, and some high-performance products still rely on imports.
[0004] In conclusion, using yellow phosphorus slag as raw material to prepare high-performance silica may be a better choice. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing high specific surface area silica from yellow phosphorus slag.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: a method for preparing high specific surface area silica from yellow phosphorus slag, characterized by comprising the following steps in sequence: S1, Deep acid hydrolysis: Concentrated acid is added to the reaction vessel, and yellow phosphorus slag is added under stirring. The mass ratio of yellow phosphorus slag to concentrated acid is 1:4 to 4.5. The mixture is heated to 100 to 110°C and kept at that temperature for 4 to 5 hours. After the reaction is completed, the mixture is filtered. The filter cake is washed and dried at 105 to 125°C to obtain the acid hydrolysis residue. The concentrated acid is 36% to 38% hydrochloric acid or 65% to 69% nitric acid. S2, Preparation of sodium silicate solution by alkaline dissolution: Deionized water is added to the reaction vessel, and the dried acid hydrolysis residue obtained in step S1 is mixed with sodium hydroxide at a mass ratio of 5:6-11. The mixture is stirred and heated to 80-98℃ and kept at that temperature for 30-60 min. After filtration, a sodium silicate solution is obtained. The sodium hydroxide is caustic soda flakes with a purity ≥96% or liquid caustic soda with a mass fraction ≥30%. S3, Sodium silicate dilution: Dilute the sodium silicate solution obtained in step S2 with deionized water, with the volume ratio of sodium silicate solution to water being 1:1 to 2, to obtain a sodium silicate diluted solution. S4, temperature-controlled acid precipitation and maturation: The sodium silicate dilution solution is pre-stirred at 50-80℃; while maintaining the system temperature at 50-80℃, acid is added to neutralize the system to pH=4-7; and the system is kept at 50-80℃ for 30-60 min to obtain silicate slurry. The neutralizing acid is sulfuric acid with a concentration ≥38%. S5, Post-processed precipitated silica: The silica slurry is vacuum filtered, pulped, washed with water, dried under normal pressure, and pulverized to obtain the finished precipitated silica; the drying temperature is controlled at 105-150℃.
[0007] Furthermore, the stirring speed is controlled at 350-500 rpm.
[0008] Furthermore, in step S1, the concentrated acid is concentrated hydrochloric acid with a mass fraction of 36% to 38%.
[0009] Furthermore, the sodium hydroxide mentioned in step S2 is caustic soda flakes with a purity of ≥96%.
[0010] Furthermore, in step S3, the volume ratio of sodium silicate solution to water is 1:1.
[0011] Furthermore, in step S4, the neutralizing acid is 98% concentrated sulfuric acid; the dropping rate of the neutralizing acid is controlled at 10-15 drops / minute.
[0012] Furthermore, the temperature for drying at normal pressure in step S5 is 120–130°C.
[0013] A high specific surface area silica product, prepared by the above method, has a BET specific surface area ≥530 m² / g.
[0014] The application of the silica is as a reinforcing filler for green tires in new energy vehicles.
[0015] The beneficial effects of this invention are as follows: First, the yellow phosphorus slag is acid-hydrolyzed with concentrated hydrochloric acid or concentrated nitric acid. After alkali dissolution of the acid-hydrolyzed slag, sulfuric acid is used as the precipitating acid to prepare silica. The resulting silica has a higher specific surface area than that obtained by other precipitation methods. Specifically, when concentrated sulfuric acid is used as the precipitating acid, the specific surface area can reach 600 μm². 2 / g or more; the preparation process is simple, requiring no additional seed crystals, and can convert yellow phosphorus slag into high-performance, high-value silica.
[0016] When adjusting the liquid alkali, dilution volume ratio of 1:1.5~2, neutralization pH of 5.5~6, aging for 30~40 min, and drying at 105-130℃ within the entire parameter range of this invention, the BET specific surface area of the obtained silica is stably maintained at 530~580 m² / g, which is still significantly higher than that of traditional precipitated silica, and it has the performance of a high-end reinforcing filler. Attached Figure Description
[0017] Figure 1 is a flowchart of the present invention; Figure 2 This is a test chart of the specific surface area of the product in Embodiment 1 of the present invention; Detailed Implementation
[0018] Example 1: The principles and features of the present invention are described below with reference to the accompanying drawings. The examples given are only for explaining the present invention and are not intended to limit the scope of the present invention.
[0019] General raw material specifications:
[0020] Solid waste generated during the production of yellow phosphorus contains 44.8% SiO2, 36.9% CaO, 4.0% Al2O3, 1.0% Fe2O3, and 3.7% P2O5. Concentrated hydrochloric acid: mass fraction 36%–38%; Concentrated nitric acid: 65%–69%; Caustic soda flakes: purity ≥ 96%; Detection index: BET specific surface area m² / g, sample degassed at 200℃ for 5h.
[0021] Example 1: A method for preparing high specific surface area silica from yellow phosphorus slag, characterized by comprising the following steps in sequence:
[0022] S1 concentrated acid deep acid hydrolysis: Take yellow phosphorus slag and 37% concentrated hydrochloric acid at a mass ratio of 1:4, add to the reactor and stir continuously, heat to 100℃ and keep warm for 5 hours, stirring speed is 450 rpm; after the reaction is completed, filter, wash the filter cake with water until neutral, and dry at 125℃ to obtain acid hydrolysis residue.
[0023] S2 Alkali Dissolution for Sodium Silicate: Dry the acid hydrolysis residue and mix it with 96% caustic soda flakes at a mass ratio of 5:11. Add deionized water and stir. Heat the mixture to 80℃ and keep it at that temperature for 60 minutes. Filter the mixture to remove insoluble impurities and obtain a sodium silicate solution.
[0024] S3 dilution: Sodium silicate solution and deionized water are mixed at a volume ratio of 1:1 and stirred until homogeneous to obtain a diluted sodium silicate solution.
[0025] S4 temperature-controlled acid precipitation and maturation: Sodium silicate dilution solution is pre-stirred at 50℃ for 10 min; the temperature is raised to 80℃, and 98% concentrated sulfuric acid is added dropwise under stirring to neutralize it at a rate of 10 drops / min, with an endpoint pH of 4; the temperature is maintained at 50℃ and stirred for 60 min to obtain silicate slurry. S5 post-processing: Vacuum filtration of slurry, pulping and washing to remove impurity ions such as Na, Al, Fe, K, and Mn, eliminating their influence on the color and properties of silica, drying at 125℃ under normal pressure, pulverizing and sieving to obtain high specific surface area silica.
[0026] Test results: BET specific surface area 664 m² / g, see Figure 2 .
[0027] Example 2: A method for preparing high specific surface area silica from yellow phosphorus slag, characterized by comprising the following steps in sequence: S1 concentrated acid deep acid hydrolysis: yellow phosphorus slag and 37% concentrated hydrochloric acid at a mass ratio of 1:4.5, stirred and heated to 104℃ and held for 5 hours at a stirring speed of 420 rpm; filtered and washed, and the acid hydrolysis residue was dried at 120℃.
[0028] S2 Sodium silicate preparation by alkaline dissolution: The mass ratio of acid hydrolysis residue to caustic soda flakes is 5:9. Deionized water is added and heated to 90℃ and kept at that temperature for 60 min. The sodium silicate solution is obtained by filtration.
[0029] S3 dilution: The volume ratio of sodium silicate solution to deionized water is 1:1.
[0030] S4 temperature-controlled acid precipitation and maturation: Sodium silicate dilution solution is pre-stirred at 80℃, and 98% concentrated sulfuric acid is added dropwise at 80℃ to neutralize to pH=4 at a rate of 12 drops / minute; then it is kept at 80℃ for 60 minutes.
[0031] S5 post-processing: filtration, water washing, drying and pulverizing at 120℃ and normal pressure, sieving to obtain the finished silica.
[0032] Test results: BET specific surface area 602 m² / g.
[0033] Example 3: A method for preparing high specific surface area silica from yellow phosphorus slag, characterized by comprising the following steps in sequence: S1 concentrated acid deep acid hydrolysis: yellow phosphorus slag and 37% concentrated hydrochloric acid at a mass ratio of 1:4.5, kept at 104℃ for 5 hours, stirred at 420 rpm, and the filter cake was dried at 120℃.
[0034] S2 Sodium silicate preparation by alkaline dissolution: The acid hydrolysis residue is mixed with caustic soda flakes at a ratio of 5:9, kept at 100℃ for 60 min for alkaline dissolution, and filtered to obtain a sodium silicate solution.
[0035] S3 dilution: The volume ratio of sodium silicate solution to deionized water is 1:1.2.
[0036] S4 temperature-controlled acid precipitation and maturation: Sodium silicate dilution solution is pre-stirred at 80℃, 98% concentrated sulfuric acid is added dropwise at 80℃ to neutralize to pH=5, the dropwise addition rate is 13 drops / minute, and maturation is carried out at 80℃ for 60 minutes.
[0037] S5 post-processing: water washing, drying and pulverizing at 120℃ to obtain finished silica.
[0038] Test results: The specific surface area of BET is 612 m² / g.
[0039] Example 4: A method for preparing high specific surface area silica from yellow phosphorus slag, characterized by comprising the following steps in sequence: S1 concentrated acid deep acid hydrolysis: yellow phosphorus slag and 68% concentrated nitric acid at a mass ratio of 1:4.5, kept at 104℃ for 5 hours, stirred at 450 rpm; filtered and washed, and the acid hydrolysis residue was dried at 125℃.
[0040] S2 Sodium silicate preparation by alkaline dissolution: Acid hydrolysis residue is mixed with caustic soda flakes at a ratio of 5:11, kept at 80℃ for 60 min for alkaline dissolution, and filtered to obtain sodium silicate solution.
[0041] S3 dilution: The volume ratio of sodium silicate solution to deionized water is 1:1.
[0042] S4 temperature-controlled acid precipitation and maturation: Sodium silicate dilution solution is pre-stirred at 80℃, and 38% sulfuric acid is added dropwise at 80℃ to neutralize to pH=4.5 at a rate of 15 drops / minute; maturation is carried out at 80℃ for 60 minutes. S5 post-processing: filtration, water washing, drying and pulverizing at 125℃ to obtain the finished silica.
[0043] Test results: The specific surface area of BET is 559 m² / g.
[0044] In addition to the original experimental examples 1-4 mentioned above, this invention conducted multiple sets of extended verification experiments within the parameter range defined in the claims. By adjusting process parameters such as the type of alkali agent, dilution ratio, neutralization pH, aging time, and drying temperature, multiple extended examples were obtained. Their BET specific surface area was obtained by actual fitting based on the performance change law of multi-gradient variable experiments. The performance change trend was completely consistent with the original examples, which proves that high specific surface area white carbon black can be stably prepared within the process parameter range of this invention.
[0045] Comparative Example 1: The acid hydrolysis parameters were the same as in Example 4. The sodium silicate solution obtained by alkali dissolution was not diluted with water and was directly precipitated with hydrochloric acid of the same concentration. The other experimental conditions were the same. The BET specific surface area of the obtained product was 92 m² / g, which was difficult to crush and the particles were severely agglomerated. Comparative Example 2:
[0046] The acid hydrolysis and alkali dissolution steps are the same as in Example 1. The temperature-controlled acid precipitation, ripening, neutralization, and precipitation steps are as follows: 4.8% dilute sulfuric acid is used, the acid precipitation and ripening temperature is 80°C, the ripening time remains unchanged, the endpoint pH is 7, and the remaining steps are the same as in Example 1. The BET specific surface area of the obtained product is 183 m² / g, which is too low and has no practical reinforcing value.
[0047] Comparative Example 3: Referring to Example 1, the subsequent alkali dissolution and acid precipitation steps were omitted, and the finished product, silica, was obtained directly by concentrated acid hydrolysis. The silica was grayish-white in color, and the BET specific surface area of the obtained product was 75 m² / g. It also contained a small amount of impurities such as Ca, P, and Cl.
[0048] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing high specific surface area silica from yellow phosphorus slag, characterized in that, The steps are as follows: S1, Deep acid hydrolysis: Concentrated acid is added to the reaction vessel, and yellow phosphorus slag is added under stirring. The mass ratio of yellow phosphorus slag to concentrated acid is 1:4 to 4.
5. The mixture is heated to 100 to 110°C and kept at that temperature for 4 to 5 hours. After the reaction is completed, the mixture is filtered. The filter cake is washed and dried at 105 to 125°C to obtain the acid hydrolysis residue. The concentrated acid is 36% to 38% hydrochloric acid or 65% to 69% nitric acid. S2, Preparation of sodium silicate solution by alkaline dissolution: Deionized water is added to the reaction vessel, and the dried acid hydrolysis residue obtained in step S1 is mixed with sodium hydroxide at a mass ratio of 5:6-11. The mixture is stirred and heated to 80-98℃ and kept at that temperature for 30-60 min. After filtration, a sodium silicate solution is obtained. The sodium hydroxide is caustic soda flakes with a purity ≥96% or liquid caustic soda with a mass fraction ≥30%. S3, Sodium silicate dilution: Dilute the sodium silicate solution obtained in step S2 with deionized water, with the volume ratio of sodium silicate solution to water being 1:1 to 2, to obtain a sodium silicate diluted solution. S4, temperature-controlled acid precipitation and maturation: The sodium silicate dilution solution is pre-stirred at 50-80℃; while maintaining the system temperature at 50-80℃, acid is added to neutralize the system to pH=4-7; and the system is kept at 50-80℃ for 30-60 min to obtain silicate slurry. The neutralizing acid is sulfuric acid with a concentration ≥38%. S5, Post-processed precipitated silica: The silica slurry is vacuum filtered, pulped, washed with water, dried under normal pressure, and pulverized to obtain the finished precipitated silica; the drying temperature is controlled at 105-150℃.
2. The method for preparing high specific gravity silica from yellow phosphorus slag according to claim 1, characterized in that, The stirring speed is controlled at 350-500 rpm.
3. The method for preparing high specific surface area silica from yellow phosphorus slag according to claim 1, characterized in that, In step S1, the concentrated acid is concentrated hydrochloric acid with a mass fraction of 36% to 38%.
4. The method for preparing high specific surface area silica from yellow phosphorus slag according to claim 1, characterized in that, The sodium hydroxide mentioned in step S2 is caustic soda flakes with a purity of ≥96%.
5. The method for preparing high specific surface area silica from yellow phosphorus slag according to claim 1, characterized in that, In step S3, the volume ratio of sodium silicate solution to water is 1:
1.
6. A method for preparing high specific surface area silica from yellow phosphorus slag according to claim 1, characterized in that, In step S4, the neutralizing acid is 98% concentrated sulfuric acid; the dropping rate of the neutralizing acid is controlled at 10-15 drops / minute.
7. The method for preparing high specific surface area silica from yellow phosphorus slag according to claim 1, characterized in that, The temperature for drying in step S5 at atmospheric pressure is 120–130°C.
8. A high specific surface area silica product, characterized in that, The silica is prepared by the preparation method according to any one of claims 1 to 7, and the BET specific surface area is ≥530 m² / g.
9. The high specific gravity carbon black product according to claim 8, characterized in that, The silica is used as a reinforcing filler for green tires in new energy vehicles.