A red mud dealkalization and filtration aid method based on phosphogypsum-acidic biochar synergy

By combining the synergistic effect of phosphogypsum and acidic biochar with chemical filter aids, the dealkali removal and filtration of red mud are integrated, solving the problems of high dealkali removal cost and poor filtration performance of red mud and improving the resource utilization efficiency of red mud.

CN123105940APending Publication Date: 2026-11-17SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611305460.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing red mud dealkali removal technology is costly, has a complex process, and is difficult to solve the alkalinity problem and improve filtration performance at the same time. Existing filter aid technology is also difficult to avoid filter cake clogging under pressure.

Method used

The synergistic use of phosphogypsum and acidic biochar generates slightly soluble calcium sulfate and ettringite gels through their combined action. These gels, along with chemical filter aids, facilitate flocculation and sedimentation, achieving integrated treatment of red mud for dealkalization and filtration.

Benefits of technology

It achieves a high alkali removal rate (≥90%) and a low filter cake moisture content (≤32%) for red mud, reducing treatment costs, simplifying the process, reducing the risk of secondary pollution, and improving the resource utilization potential of red mud.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105940A_ABST
    Figure CN123105940A_ABST
Patent Text Reader

Abstract

This invention relates to the field of red mud solid waste treatment technology, and particularly to a red mud dealkalization and filtration method based on phosphogypsum-acidic biochar synergy. The method includes the following steps: phosphogypsum is crushed, ground, and dried to obtain pretreated phosphogypsum; agricultural and forestry waste is pulverized, calcined under inert gas protection, cooled, activated by acid immersion, washed, dried, and ground to obtain acidic biochar; red mud is mixed with water and stirred to form a red mud slurry; the pretreated phosphogypsum, acidic biochar, and chemical filter aid are sequentially added to the red mud slurry, and the mixture is stirred at a constant temperature under stirring conditions to obtain a conditioned red mud slurry; the conditioned red mud slurry is then pressure filtered to collect the filtrate and filter cake. This method achieves waste-to-waste treatment, simultaneously improving the red mud dealkalization efficiency and filtration performance, reducing treatment costs, and laying the foundation for the subsequent resource utilization of red mud.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of red mud solid waste treatment technology, and in particular to a red mud dealkalization and filtration method based on the synergistic effect of phosphogypsum and acidic biochar. Background Technology

[0002] Red mud is an alkaline solid waste produced during the production of alumina. Its strong alkalinity (pH value is usually 10-13), fine particle size, and strong compressibility make dewatering and filtration difficult. The moisture content of the filter cake is generally higher than 50%, which restricts its subsequent resource utilization.

[0003] Existing red mud dealkali removal technologies, such as acid leaching, offer high dealkali removal rates but are costly and prone to introducing impurities. Calcium ion exchange methods require large amounts of reagents and have relatively low dealkali removal rates. Filter aid technologies, such as using single inorganic or chemical filter aids, can improve filtration performance but struggle to simultaneously address alkalinity issues, and the filter cake is easily compressed and clogged under pressure. While some existing methods utilize phosphogypsum for dealkali removal, these require high-temperature decomposition and gas conveying equipment, resulting in complex processes and lacking a dedicated filter aid function. Summary of the Invention

[0004] To address the shortcomings of existing technologies, the purpose of this invention is to provide a red mud dealkalization and filtration method based on the synergistic effect of phosphogypsum and acidic biochar, thereby achieving waste-to-waste treatment, simultaneously improving the red mud dealkalization efficiency and filtration performance, reducing treatment costs, and laying the foundation for the subsequent resource utilization of red mud.

[0005] To achieve the above objectives, the embodiments of the present invention provide the following technical solutions: A red mud dealkalization and filtration aid method based on phosphogypsum-acidic biochar synergy includes the following steps: Pretreated phosphogypsum is obtained by crushing, grinding and drying phosphogypsum. Agricultural and forestry waste is crushed, roasted under inert gas protection, cooled, activated by soaking in acid solution, washed, dried and ground to obtain acidic biochar. Mix red mud with water and stir to make red mud slurry; The pretreated phosphogypsum, the acidic biochar, and the chemical filter aid are added sequentially to the red mud slurry, and the mixture is stirred at a constant temperature under stirring conditions to obtain the conditioned red mud slurry. The conditioned red mud slurry was filtered by pressure, and the filtrate and filter cake were collected.

[0006] Furthermore, in the phosphogypsum pretreatment step, the phosphogypsum is ground and passed through a 100-200 mesh sieve, and then dried in an oven at 45-60℃ until the moisture content is ≤5%.

[0007] Furthermore, in the preparation step of acidic biochar, the agricultural and forestry waste is one or more mixtures of corn stalks, rice husks, and sawdust.

[0008] Furthermore, in the preparation steps of acidic biochar, the calcination temperature is 300-600℃ and the calcination time is 3-5h.

[0009] Furthermore, in the preparation step of acidic biochar, the acid solution is sulfuric acid or hydrochloric acid with a concentration of 0.5-1.0 mol / L, the liquid-solid ratio of the acid solution to the biochar is 5:1-10:1, and the soaking and activation time is 2-4 hours.

[0010] Furthermore, in the red mud slurry preparation step, the liquid-to-solid ratio is 3:1-6:1.

[0011] Furthermore, based on the dry weight of red mud: pretreated phosphogypsum 5%-15%, acidic biochar 3%-8%, and chemical filter aid 0.1%-0.5%.

[0012] Furthermore, the chemical filter aid is a compound system of PL50 polymeric filter aid, cationic polyacrylamide and ferric sulfate, with a mass ratio of 2:1:1 to 3:1:1.

[0013] Furthermore, during the synergistic conditioning process, the stirring speed is 200-400 r / min, the reaction temperature is 60-90℃, and the constant temperature stirring reaction time is 20-40 min.

[0014] Furthermore, in the filter press step, the filter press pressure is 0.8-1.5 MPa, the resulting filter cake has a moisture content of ≤32% and a dealkali removal rate of ≥90%.

[0015] One or more technical solutions provided in the embodiments of the present invention have at least the following technical effects or advantages: The red mud dealkali removal and filtration aid method of the present invention includes five steps: phosphogypsum pretreatment, acidic biochar preparation, red mud slurry preparation, synergistic conditioning and treatment, and pressure filtration separation. By synergistically using phosphogypsum, acidic biochar, and chemical filter aids, the dual functions of dealkali removal and filtration are achieved simultaneously in the same treatment process. Specifically, phosphogypsum is crushed, ground, and dried to obtain pretreated phosphogypsum, which removes free water and impurities, allowing it to be better dispersed in the red mud slurry. Agricultural and forestry waste is crushed and roasted under inert gas protection to carbonize the biomass and form a porous structure. It is then activated by soaking in acid solution, which grafts acidic functional groups such as carboxyl and hydroxyl groups onto the surface of the biochar. After washing, drying, and grinding, acidic biochar is obtained. Red mud is mixed with water to prepare a slurry, providing a liquid-phase contact environment for subsequent reactions. Pretreated phosphogypsum, acidic biochar, and chemical filter aids are added to the slurry in sequence, and the reaction is carried out at a constant temperature under stirring conditions to ensure sufficient contact between the components and the occurrence of physicochemical reactions. Finally, solid-liquid separation is achieved through pressure filtration to obtain filter cake and filtrate. This method completes the two objectives of dealkali removal and filtration aid in the same process, solving the problem of independent dealkali removal and filtration aid processes in existing technologies, which are complex. From the perspective of synergistic effects, the acidic functional groups on the surface of acidic biochar neutralize the free alkali in red mud, while its porous structure provides skeletal support for the subsequent filter cake; the sulfate ions in phosphogypsum react with calcium ions in red mud to generate calcium sulfate, releasing hydrogen ions to further neutralize the alkali, and at the same time react with the active components in red mud to generate gel substances such as ettringite and hydrated calcium silicate; the chemical filter aid causes red mud particles to flocculate into large flocs through charge neutralization and adsorption bridging. These three substances play a role from three dimensions: chemical dealkali removal, skeletal support, and flocculation sedimentation, respectively, and work together to form a composite conditioning system, realizing waste-to-waste treatment, simultaneously improving the dealkali removal efficiency and filtration performance of red mud, reducing treatment costs, and laying the foundation for the subsequent resource utilization of red mud.

[0016] Advantages of additional aspects of the invention will be set forth in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. The drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. In addition, the dimensions or spacing between the components are exaggerated to show the position of each component, and the schematic diagrams are for illustrative purposes only.

[0018] Figure 1 This is a schematic diagram of a red mud dealkalization and filtration method based on the synergistic effect of phosphogypsum and acidic biochar provided in an embodiment of the present invention; Detailed Implementation It should be noted that the following detailed description is illustrative and intended to provide further explanation of the invention. Unless otherwise specified, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. Furthermore, it should be understood that when the terms include and / or encompass are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0019] Terminology Explanation: PL50: Refers to PL50 type polymer filter aid, which is a polymer filter aid used in solid-liquid separation processes. It has the functions of adsorption bridging, improving filter cake structure, and improving filtration and dewatering efficiency. It is widely used in the field of industrial solid waste slurry filtration treatment.

[0020] PAM: Polyacrylamide is a linear water-soluble polymer. Cationic PAM can cause suspended particles to flocculate and aggregate through charge neutralization. It is often used as a flocculant and filter aid in solid-liquid separation processes.

[0021] Red mud is an alkaline solid waste generated during alumina production, producing approximately 1-1.5 tons of red mud for every ton of alumina produced. With the continuous increase in alumina production, the accumulated amount of red mud has exceeded 1.5 billion tons, with nearly 90 million tons added annually. The long-term accumulation of large quantities of red mud not only occupies valuable land resources, but its strong alkalinity (pH value typically between 10 and 13) also pollutes surrounding soil and groundwater through leaching, posing serious ecological and environmental risks. Simultaneously, the high alkalinity, fine particle size, and strong compressibility of red mud result in extremely poor dewatering and filtration performance, with filter cake moisture content generally exceeding 50%, further restricting its subsequent resource utilization. Therefore, developing treatment methods that can effectively reduce the alkalinity of red mud and improve its filtration performance is of great significance for its harmless disposal and resource utilization.

[0022] Currently, in terms of dealkali removal technology, acid leaching uses inorganic acids to neutralize the alkali in red mud, achieving a dealkali removal rate of over 90%. However, this method consumes a large amount of acid reagents, resulting in high processing costs and the introduction of harmful impurities, leading to a heavy burden on subsequent neutralization treatments. Calcium ion replacement removes alkali from red mud by adding calcium salts to precipitate it, but requires large amounts of reagents, and the dealkali removal rate is typically below 80%. Existing technologies also disclose the use of sulfur dioxide tail gas generated from the high-temperature decomposition of phosphogypsum to neutralize and remove alkali from red mud slurry. This method utilizes the acidic gas generated from the pyrolysis of phosphogypsum for dealkali removal, but it requires additional pyrolysis equipment and a gas delivery system, resulting in a long process flow, high energy consumption, and no improvement in the filtration performance of red mud.

[0023] In terms of filter aid technology, single inorganic filter aids such as lime and gypsum can improve the filter cake structure to a certain extent, but their dealkali removal effect is limited. Single chemical filter aids such as polyacrylamide can improve filtration efficiency through charge neutralization or adsorption bridging, but they are difficult to solve the problem of strong alkalinity of red mud. Moreover, the filter cake is easily compressed and deformed under pressure, which leads to blockage of the filtration channel and the dewatering efficiency is still not ideal.

[0024] Existing red mud dealkali removal technology and filtration technology are mostly independent of each other, and each has problems such as complex processing procedures, high costs, risk of secondary pollution, or poor performance.

[0025] Phosphogypsum, an industrial waste product from phosphate fertilizer production, is emitted in huge quantities annually. It contains a certain amount of sulfate and calcium ions, possessing the potential to neutralize alkaline substances. However, when used alone for red mud treatment, it actually increases the moisture content of the filter cake, resulting in poor filtration. Acidic biochar, made from biomass through high-temperature roasting and activation, is rich in acidic functional groups on its surface, which can neutralize the alkalinity of red mud. Its porous structure is expected to improve the air permeability of the filter cake. However, when used alone, it has a slow dealkali removal rate and insufficient support for the filter's skeletal structure.

[0026] This invention achieves integrated red mud dealkalization and filtration through the synergistic effect of phosphogypsum, acidic biochar, and chemical filter aids. The specific mechanism is as follows: Synergistic dealkali removal: The acidic functional groups such as carboxyl and hydroxyl groups on the surface of acidic biochar can neutralize the free alkali in red mud; the sulfate ions in phosphogypsum react with the calcium ions in red mud to generate slightly soluble calcium sulfate, while releasing hydrogen ions to further enhance dealkali removal, and can also remove some structural alkali in red mud, thereby increasing the depth of dealkali removal. Synergistic filtration: The porous structure of acidic biochar provides basic skeletal support for the filter cake, reducing its compressibility and preventing filtration channel blockage; phosphogypsum reacts with the active ingredients in red mud to generate gel substances with stable skeletal structures, such as ettringite and hydrated calcium silicate, which can further strengthen the filter cake skeleton and optimize its pore structure and permeability, thereby improving the filtration rate; chemical filter aids, through charge neutralization and adsorption bridging, cause red mud particles to flocculate into large flocs, which work together with the gel skeleton and the porous structure of biochar to further improve overall filtration performance.

[0027] Specifically, such as Figure 1 As shown, a red mud dealkali removal and filtration method based on phosphogypsum-acidic biochar synergy, wherein the red mud is Bayer process red mud, includes the following steps: S100 processes phosphogypsum through crushing, grinding, and drying to obtain pretreated phosphogypsum; S200 pulverizes agricultural and forestry waste, roasts it under inert gas protection, cools it, activates it by soaking in acid solution, washes it, dries it, and grinds it to obtain acidic biochar. S300 mixes red mud with water and stirs it to make red mud slurry; S400 adds the pretreated phosphogypsum, the acidic biochar, and the chemical filter aid to the red mud slurry in sequence, and stirs and reacts at a constant temperature under stirring conditions to obtain the conditioned red mud slurry; S500 performs pressure filtration on the conditioned red mud slurry and collects the filtrate and filter cake.

[0028] This method involves pretreating phosphogypsum before its reaction, which removes impurities and free water, improving its reaction efficiency with red mud. Acidic biochar prepared from agricultural and forestry waste forms acidic functional groups on its surface and possesses a porous structure, enabling it to neutralize the alkalinity of red mud and provide skeletal support for the filter cake. The preparation of the red mud slurry ensures it is in a homogeneous state, allowing subsequent additions of various conditioning agents to fully contact and react with the red mud. Pretreated phosphogypsum, acidic biochar, and chemical filter aids are added sequentially to the red mud slurry, and the reaction is carried out under constant temperature and stirring, achieving a synergistic effect of the three substances. The sulfate ions in the pretreated phosphogypsum react with calcium ions in the red mud, releasing hydrogen ions to enhance dealkalization and simultaneously generating slightly soluble calcium sulfate. The acidic functional groups on the surface of the acidic biochar neutralize the free alkali in the red mud, and its porous structure provides a basic framework for the filter cake. The chemical filter aid, through charge neutralization and adsorption bridging, causes the red mud particles to flocculate into large flocs. The three components work together to optimize the pore structure and air permeability of the filter cake, improving dealkali removal and filtration efficiency. Pressure filtration of the conditioned red mud slurry achieves solid-liquid separation, completing the integrated treatment of red mud dealkali removal and filtration, changing the existing technology's separate dealkali removal and filtration process, and simplifying the process.

[0029] This method achieves both dealkali removal and filtration in the same process. It uses acidic biochar prepared from industrial waste phosphogypsum and agricultural and forestry waste as the main conditioning agent, thereby reducing the treatment cost by treating waste with waste. At the same time, it avoids the problem of introducing harmful substances in the single acid leaching method and the easy blockage of the filter channel caused by a single chemical filter aid, thus reducing the risk of secondary pollution from the source.

[0030] Furthermore, in the phosphogypsum pretreatment step, the phosphogypsum is ground and passed through a 100-200 mesh sieve, and then dried in an oven at 45-60℃ until the moisture content is ≤5%.

[0031] After grinding, the phosphogypsum is passed through a 100-200 mesh sieve. This particle size range ensures that the phosphogypsum particles have a suitable specific surface area; if the particles are too coarse, the reaction contact area will be insufficient, and if they are too fine, filtration may be difficult. It is then dried until the moisture content does not exceed 5%, and the drying temperature is controlled between 45-60℃. This temperature range effectively removes moisture without causing decomposition or phase change of the phosphogypsum. Controlling the moisture content ensures the fluidity of the phosphogypsum during storage and addition, preventing clumping that could affect the uniformity of dispersion.

[0032] Furthermore, in the preparation steps of acidic biochar, the agricultural and forestry waste is one or more mixtures of corn stalks, rice husks, and sawdust. These agricultural and forestry wastes are widely available and inexpensive, aligning with the environmental protection concept of treating waste with waste. Mixing multiple raw materials can leverage the advantages of different materials, resulting in a more balanced performance of the biochar.

[0033] Furthermore, in the preparation steps of acidic biochar, the calcination temperature is 300-600℃ and the calcination time is 3-5h.

[0034] The roasting temperature range of 300-600℃ covers the typical temperature range for biomass carbonization. Within this range, cellulose, hemicellulose, and lignin in biomass undergo pyrolysis, forming carbon materials with a porous structure. Too low a temperature may lead to incomplete carbonization and insufficient pore development, while too high a temperature may cause the pore structure to collapse or become excessively graphitized, reducing the adhesion ability of surface functional groups. A roasting time of 3-5 hours ensures that the pyrolysis reaction proceeds fully, allowing the pore structure to stabilize.

[0035] Furthermore, in the preparation step of acidic biochar, the acid solution is sulfuric acid or hydrochloric acid with a concentration of 0.5-1.0 mol / L, the liquid-solid ratio of the acid solution to the biochar is 5:1-10:1, and the soaking and activation time is 2-4 hours.

[0036] Activation is performed using sulfuric acid or hydrochloric acid with a concentration of 0.5-1.0 mol / L. This effectively etches the surface of the biochar and introduces acidic functional groups without excessively damaging the carbon framework structure. A liquid-to-solid ratio of 5:1-10:1 ensures sufficient contact between the acid and the biochar, allowing the activation reaction to proceed uniformly. The immersion activation time is 2-4 hours, allowing ample time for the acid to react with the carbon surface and form acidic functional groups such as carboxyl and hydroxyl groups.

[0037] Furthermore, in the red mud slurry preparation step, the liquid-to-solid ratio is 3:1-6:1. This range ensures the slurry has appropriate fluidity, guaranteeing uniform dispersion of additives without diluting reactant concentrations or increasing subsequent filtration load due to excessive water. A liquid-to-solid ratio that is too low leads to excessive slurry viscosity, difficulty in stirring, and uneven additive dispersion; a ratio that is too high prolongs filtration time and increases energy consumption.

[0038] Furthermore, the addition amounts of each raw material, based on the dry red mud mass, are as follows: 5%-15% pretreated phosphogypsum, 3%-8% acidic biochar, and 0.1%-0.5% chemical filter aid.

[0039] The addition of 5%-15% pretreated phosphogypsum ensures sufficient calcium and sulfate ions to participate in the reaction and form a gel skeleton, while avoiding excessive addition that could lead to filter cake thickening and increased filtration resistance. The addition of 3%-8% acidic biochar provides sufficient acidic functional groups to neutralize the alkali and forms an effective porous skeleton support; too low a dosage results in incomplete alkali removal and insufficient skeleton support, while too high a dosage may occupy excessive volume and affect filter cake density. The addition of 0.1%-0.5% chemical filter aid promotes flocculation through charge neutralization and adsorption bridging; excessive dosage may lead to over-flocculation or increased reagent costs. The proportions of the three additives are matched to create a synergistic effect.

[0040] Furthermore, the chemical filter aid is a compound system of PL50 polymeric filter aid, cationic polyacrylamide, and ferric sulfate, with a mass ratio of 2:1:1 to 3:1:1. The cationic polyacrylamide carries a positive charge, which can neutralize the negative charge on the surface of red mud particles, causing the particles to destabilize and aggregate through charge neutralization. Ferric sulfate, as an inorganic flocculant, also plays a role in charge neutralization through the iron ions produced by hydrolysis, and may also form ferric hydroxide flocs. The combined use of these three components promotes flocculation through both charge neutralization and adsorption bridging, forming dense and high-strength flocs. Compared to a single filter aid, this compound system is better suited to the complex composition of red mud slurry, working in conjunction with the gel skeleton formed by phosphogypsum and the porous skeleton of acidic biochar to optimize the filter cake structure.

[0041] Furthermore, in the synergistic conditioning process, the stirring speed is 200-400 r / min, the reaction temperature is 60-90℃, and the constant temperature stirring reaction time is 20-40 min.

[0042] A stirring speed of 200-400 rpm ensures uniform dispersion of all additives in the slurry. Too low a speed will result in uneven dispersion, while too high a speed may damage the existing flocs. A reaction temperature of 60-90℃ accelerates the chemical reaction rate, promoting the reaction between phosphogypsum and the active components of red mud to form a gel, while also increasing the reaction rate between the functional groups on the surface of acidic biochar and the alkali. A reaction time of 20-40 minutes ensures a complete reaction; too short a time will result in incomplete reaction, while too long a time will reduce processing efficiency.

[0043] Furthermore, in the filter press step, the filter pressure is 0.8-1.5 MPa, the resulting filter cake has a moisture content ≤32%, and the dealkali removal rate ≥90%. At 0.8-1.5 MPa, the conditioned red mud slurry can achieve effective solid-liquid separation. The filter cake moisture content ≤32% provides a prerequisite for subsequent resource utilization. The dealkali removal rate ≥90% reduces environmental risks.

[0044] Existing red mud treatment methods mostly focus on a single objective: for example, using phosphogypsum to decompose gases at high temperatures to remove alkali, although it has a certain dealkali removal effect, it requires a complex pyrolysis device and does not involve improving filtration performance; or it improves filtration efficiency by adding chemical filter aids, but it is difficult to solve the alkalinity problem at the same time; some studies have also mixed biochar with red mud and phosphogypsum to prepare cementitious materials, but the biochar is not acid activated, and slag and activators need to be introduced into the system, and its goal is the strength of building materials rather than the dealkali removal and filtration of red mud slurry.

[0045] This method, for the first time, proposes a synergistic effect of acid-activated biochar, pretreated phosphogypsum, and chemical filter aids in a liquid-phase slurry, achieving the dual functions of dealkali removal and filtration of red mud in the same process. The acidic biochar not only provides acidic functional groups to neutralize alkali but also supports the filter cake framework through its porous structure. The phosphogypsum reacts with the red mud in the aqueous phase to form gel structures such as ettringite, further enhancing the air permeability and filtration performance of the filter cake. The chemical filter aid promotes particle aggregation through flocculation. The synergistic effect of these three components achieves a significant effect of dealkali removal rate ≥90% and filter cake moisture content ≤32%, far exceeding single or binary compound solutions. This technical solution is not a simple combination of D1–D3, but a systematic solution addressing the dual technical challenges of "difficult dealkali removal and difficult filtration" in red mud slurry treatment, possessing outstanding substantive characteristics and significant progress.

[0046] Specifically, the red mud dealkalization and filtration method based on the synergistic effect of phosphogypsum and acidic biochar includes the following steps: 1. Raw material pretreatment: Pretreatment of phosphogypsum: After crushing and grinding, phosphogypsum is passed through a 100-200 mesh sieve and dried in an oven at 45-60℃ until the moisture content is ≤5% to remove impurities and free water, thus obtaining pretreated phosphogypsum. Preparation of acidic biochar: Agricultural and forestry waste is used as raw material. After being crushed, it is calcined at 300-600℃ for 3-5 hours under inert gas protection. After cooling, it is activated by soaking in acid solution for 2-4 hours, washed until neutral, dried and ground through a 100-200 mesh sieve to obtain acidic biochar with a pH value of 3.5-5.5 and a specific surface area ≥200m² / g. Preferably, the agricultural and forestry waste is one or more mixtures of corn stalks, rice husks, and sawdust. The acid solution is sulfuric acid or hydrochloric acid with a concentration of 0.5-1.0 mol / L, and the liquid-to-solid ratio of the acid solution to biochar is 5:1-10:1 (mL / g).

[0047] Preparation of red mud slurry: Mix red mud with water and stir to prepare red mud slurry with a liquid-to-solid ratio of 3:1-6:1 (mL / g).

[0048] 2. Co-conditioning treatment: Pretreated phosphogypsum, acidic biochar, and chemical filter aid are added sequentially to the red mud slurry. The mixture is stirred at a constant temperature for 20-40 minutes at a stirring speed of 200-400 r / min and a temperature of 60-90℃ to obtain the conditioned red mud slurry. The amount of each raw material added is based on the dry red mud mass as follows: pretreated phosphogypsum 5%-15%, acidic biochar 3%-8%, and chemical filter aid 0.1%-0.5%.

[0049] Preferably, the chemical filter aid is a compound system of PL50 polymeric filter aid, cationic PAM and ferric sulfate, with a mass ratio of 2:1:1 to 3:1:1.

[0050] Preferably, the stirring reaction temperature is 75-85℃ and the stirring time is 25-35min, at which point the synergistic effect of dealkali removal and filtration is optimal.

[0051] 3. Solid-liquid separation: The conditioned red mud slurry is placed in a filter press and filtered under a pressure of 0.8-1.5 MPa. The filtrate and filter cake are collected to complete the integrated treatment of red mud dealkali removal and filtration.

[0052] 4. Product post-processing: The filtrate, after neutralization treatment to meet the standards, can be recycled for the preparation of red mud slurry; the filter cake has a moisture content ≤32% and a dealkali removal rate ≥90%, and can be used as a raw material for building materials or roadbed filler. This red mud dealkalization and filtration method has the following advantages: Significant synergistic effect: It realizes integrated treatment of dealkali removal and filtration, with a dealkali removal rate of ≥90% and a filter cake moisture content of ≤30%. Compared with single material treatment, the dealkali removal rate is increased by more than 15%, the filter cake moisture content is reduced by more than 20%, and the treatment efficiency is greatly improved. Waste-to-waste treatment: Both phosphogypsum and acidic biochar originate from industrial waste or agricultural and forestry waste, resulting in low resource utilization costs and reducing the pollution from the stockpiling of these two types of solid waste, thus yielding significant environmental benefits. The process is simple: no complex equipment is required, the conditioning and separation process is compact, it can be adapted to existing red mud treatment production lines, and it is easy to achieve industrialization. Product resource utilization: The treated filter cake has optimized performance and can be used in building materials, roadbed fillers, etc. The filtrate can be recycled, realizing a closed-loop resource system.

[0053] Example 1 1. Raw material pretreatment: Phosphogypsum was crushed and ground through a 150-mesh sieve and dried at 55℃ to a moisture content of 4%; corn stalks were used as raw material, calcined at 500℃ for 4 hours under nitrogen protection, cooled and then soaked in 0.8mol / L sulfuric acid solution for 3 hours to activate, washed until neutral, dried and ground through a 150-mesh sieve at 80℃ to obtain acidic biochar (pH=4.2, specific surface area 230m² / g); red mud was mixed with water to prepare a red mud slurry with a liquid-to-solid ratio of 5:1.

[0054] 2. Co-conditioning and treatment: Add 8g of pretreated phosphogypsum, 5g of acidic biochar, and 0.2g of chemical filter aid (PL50:PAM:ferric sulfate=2:1:1) to 100g of dry red mud slurry. Stir at a constant temperature for 30min at a stirring speed of 300r / min and a temperature of 80℃.

[0055] 3. Solid-liquid separation: The conditioned slurry is placed in a filter press and filtered under a pressure of 1.5 MPa to collect the filtrate and filter cake.

[0056] 4. Results: The filter cake moisture content was 26.2%, the red mud dealkalization rate was 92.5%, and the filtrate pH was 7.8.

[0057] Example 2 1. Raw material pretreatment: Phosphogypsum was crushed and ground through a 200-mesh sieve, and dried at 60℃ to a moisture content of 3.5%; rice husks were used as raw material, calcined at 450℃ for 5 hours under nitrogen protection, cooled, and then activated by soaking in 1.0 mol / L hydrochloric acid solution for 2.5 hours, washed until neutral, dried at 70℃, and ground through a 200-mesh sieve to obtain acidic biochar (pH=3.8, specific surface area 250 m² / g); red mud was mixed with water to prepare a slurry with a liquid-to-solid ratio of 5:1.

[0058] 2. Co-conditioning and treatment: Add 12g of pretreated phosphogypsum, 6g of acidic biochar, and 0.3g of chemical filter aid (PL50:PAM:ferric sulfate=3:1:1) to 100g of dry red mud slurry. Stir at a constant temperature of 350r / min and 85℃ for 35min.

[0059] 3. Solid-liquid separation: Pressure filtration at 0.8 MPa, collecting the filtrate and filter cake.

[0060] 4. Results: The filter cake moisture content was 29.8%, the red mud dealkalization rate was 93.1%, and the filtrate pH was 7.6.

[0061] Example 3 1. Raw material pretreatment: Phosphogypsum was crushed and ground through a 200-mesh sieve and dried at 45℃ to a moisture content of 5%; sawdust was used as raw material, calcined at 600℃ for 3 hours under nitrogen protection, cooled and then activated by soaking in 0.5mol / L sulfuric acid solution for 4 hours, washed until neutral, dried at 60℃ and ground through a 200-mesh sieve to obtain acidic biochar (pH=5.3, specific surface area 205m² / g); red mud was mixed with water to prepare a red mud slurry with a liquid-to-solid ratio of 6:1.

[0062] 2. Co-conditioning and treatment: Add 5g of pretreated phosphogypsum, 3g of acidic biochar, and 0.1g of chemical filter aid (PL50:PAM:ferric sulfate=2:1:1) to 100g of dry red mud slurry. Stir at a constant temperature for 25min at a stirring speed of 200r / min and a temperature of 75℃.

[0063] 3. Solid-liquid separation: The conditioned slurry is placed in a filter press and filtered under a pressure of 1.2 MPa to collect the filtrate and filter cake.

[0064] 4. Results: The filter cake moisture content was 28.8%, the red mud dealkalization rate was 90.2%, and the filtrate pH was 8.0.

[0065] Example 4 1. Raw material pretreatment: Phosphogypsum was crushed and ground through a 200-mesh sieve, and dried at 50℃ to a moisture content of 4.2%; a mixture of corn stalks and rice husks (mass ratio 1:1) was used as raw material, calcined at 400℃ for 4.5h under nitrogen protection, cooled, and activated by soaking in 0.7mol / L hydrochloric acid solution for 3.5h, washed until neutral, dried at 75℃, and ground through a 200-mesh sieve to obtain acidic biochar (pH=4.5, specific surface area 240m² / g); red mud was mixed with water to prepare a slurry with a liquid-to-solid ratio of 5.5:1.

[0066] 2. Co-conditioning and treatment: Add 10g of pretreated phosphogypsum, 4g of acidic biochar, and 0.4g of chemical filter aid (PL50:PAM:ferric sulfate=2.5:1:1) to 100g of dry red mud slurry. Stir at a constant temperature of 380r / min and 82℃ for 32min.

[0067] 3. Solid-liquid separation: Pressure filtration at 1.0 MPa, collecting the filtrate and filter cake.

[0068] 4. Results: The filter cake moisture content was 29.5%, the red mud dealkalization rate was 94.3%, and the filtrate pH was 7.5.

[0069] Example 5 1. Raw material pretreatment: Phosphogypsum was crushed and ground through a 200-mesh sieve, and dried at 55℃ to a moisture content of 3.8%; a mixture of rice husks and sawdust (mass ratio 2:1) was used as raw material, calcined at 550℃ for 3.5h under nitrogen protection, cooled, and then activated by soaking in 1.0mol / L sulfuric acid solution for 2h, washed until neutral, dried at 80℃, and ground through a 200-mesh sieve to obtain acidic biochar (pH=4.0, specific surface area 260m² / g); red mud was mixed with water to prepare a slurry with a liquid-to-solid ratio of 6:1.

[0070] 2. Co-conditioning and treatment: Add 15g of pretreated phosphogypsum, 8g of acidic biochar, and 0.5g of chemical filter aid (PL50:PAM:ferric sulfate=3:1:1) to 100g of dry red mud slurry. Stir at a constant temperature of 400r / min and 90℃ for 40min.

[0071] 3. Solid-liquid separation: Pressure filtration at 1.5 MPa, collecting the filtrate and filter cake.

[0072] 4. Results: The filter cake moisture content was 25.9%, the red mud dealkalization rate was 95.1%, and the filtrate pH was 7.4.

[0073] Example 6 1. Raw material pretreatment: Phosphogypsum was crushed and ground through a 200-mesh sieve, and dried at 45℃ to a moisture content of 4.8%; a mixture of corn stalks and sawdust (mass ratio 3:1) was used as raw material, calcined at 350℃ for 5 hours under argon protection, cooled, and then activated by soaking in 0.6mol / L sulfuric acid solution for 3.8 hours. After washing until neutral, it was dried at 65℃ and ground through a 200-mesh sieve to obtain acidic biochar (pH=5.0, specific surface area 210m² / g); red mud was mixed with water to prepare a slurry with a liquid-to-solid ratio of 5.5:1.

[0074] 2. Co-conditioning and treatment: Add 7g of pretreated phosphogypsum, 6g of acidic biochar, and 0.25g of chemical filter aid (PL50:PAM:ferric sulfate=2:1:1) to 100g of dry red mud slurry. Stir at a constant temperature of 250r / min and 78℃ for 28min.

[0075] 3. Solid-liquid separation: Pressure filtration at 0.9 MPa, collecting the filtrate and filter cake.

[0076] 4. Results: The filter cake moisture content was 30.2%, the red mud dealkalization rate was 91.8%, and the filtrate pH was 7.9.

[0077] Example 7 1. Raw material pretreatment: Phosphogypsum was crushed and ground through a 200-mesh sieve, and dried at 50℃ to a moisture content of 4.1%; rice husks were used as raw material, calcined at 520℃ for 3.2h under nitrogen protection, cooled, and then activated by soaking in 0.9mol / L hydrochloric acid solution for 2.2h, washed until neutral, dried at 72℃, and ground through a 200-mesh sieve to obtain acidic biochar (pH=4.1, specific surface area 245m² / g); red mud was mixed with water to prepare a slurry with a liquid-to-solid ratio of 4.2:1 (initial pH of red mud = 12.5, moisture content 66%).

[0078] 2. Co-conditioning and treatment: Add 13g of pretreated phosphogypsum, 5g of acidic biochar, and 0.35g of chemical filter aid (PL50:PAM:ferric sulfate=2.8:1:1) to 100g of dry red mud slurry. Stir at a constant temperature of 320r / min and 88℃ for 36min.

[0079] 3. Solid-liquid separation: Pressure filtration at 1.3 MPa, collecting the filtrate and filter cake.

[0080] 4. Results: The filter cake moisture content was 29.1%, the red mud dealkalization rate was 94.7%, and the filtrate pH was 7.5.

[0081] Example 8 1. Raw material pretreatment: Phosphogypsum was crushed and ground through a 190-mesh sieve, and dried at 50℃ to a moisture content of 3.9%; a mixture of corn stalks, rice husks, and sawdust (mass ratio 1:1:1) was used as raw material, calcined at 480℃ for 4.2h under nitrogen protection, cooled, and then activated by soaking in 0.8mol / L sulfuric acid solution for 3.0h. After washing until neutral, it was dried at 78℃ and ground through a 190-mesh sieve to obtain acidic biochar (pH=4.3, specific surface area 255m² / g); red mud was mixed with water to prepare a slurry with a liquid-to-solid ratio of 6:1.

[0082] 2. Co-conditioning and treatment: Add 9g of pretreated phosphogypsum, 7g of acidic biochar, and 0.45g of chemical filter aid (PL50:PAM:ferric sulfate=3:1:1) to 100g of dry red mud slurry. Stir at a constant temperature of 360r / min and 84℃ for 34min.

[0083] 3. Solid-liquid separation: Pressure filtration at 1.4 MPa, collecting the filtrate and filter cake.

[0084] 4. Results: The filter cake moisture content was 28.7%, the red mud dealkalization rate was 95.3%, and the filtrate pH was 7.3.

[0085] Comparative Example 1 100g of dry-based red mud slurry was treated with only 13g of pretreated phosphogypsum (same as in Example 1), and other conditions were the same as in Example 1. The results showed that the filter cake moisture content was 41.5% and the dealkali removal rate was 72.3%.

[0086] Comparative Example 2 100g of dry red mud slurry was treated with only 13g of acidic biochar (same as in Example 1), and other conditions were the same as in Example 1. The results showed that the filter cake moisture content was 36.8% and the dealkali removal rate was 78.5%.

[0087] Comparative Example 3 A compound of phosphogypsum and chemical filter aid (acid-free biochar) was used. 13g of pretreated phosphogypsum (same as in Example 1) and 0.2g of chemical filter aid (same as in Example 1) were added to 100g of dry red mud slurry. Other conditions were the same as in Example 1. The results showed that the filter cake moisture content was 37.2% and the dealkali removal rate was 81.6%. Compared with Example 1, the filter cake moisture content increased by 7% and the dealkali removal rate decreased by 10.9%.

[0088] Comparative Example 4 A mixture of acidic biochar and chemical filter aid (phospho-free gypsum) was used. 13g of acidic biochar (same as in Example 1) and 0.2g of chemical filter aid (same as in Example 1) were added to 100g of dry red mud slurry. Other conditions were the same as in Example 1. The results showed that the filter cake moisture content was 35.4% and the dealkali removal rate was 83.2%.

[0089] In summary, this invention constructs an integrated red mud dealkalization and filtration system through the synergistic effect of phosphogypsum, acidic biochar, and compounded chemical filter aids. Its core advantage lies in the ettringite and hydrated calcium silicate gel generated from the reaction of phosphogypsum and red mud, which complement the porous framework of acidic biochar. Combined with the flocculation effect of the chemical filter aids, this significantly optimizes the filter cake structure and filtration performance. Compared to single-raw-material or binary compound treatment schemes, the red mud dealkalization rate after treatment by this invention remains stable at over 90%, and the filter cake moisture content can be as low as 25.9%. Furthermore, using industrial waste phosphogypsum and agricultural and forestry waste-based acidic biochar as core conditioning agents, it realizes the environmentally friendly concept of treating waste with waste. The process is simple, the system is highly stable, and it is easily adaptable to existing red mud treatment production lines, possessing significant environmental, economic, and industrialization promotion value.

[0090] While the specific embodiments of the present invention have been described above, they are not intended to limit the scope of protection of the present invention. Those skilled in the art should understand that various modifications or variations that can be made by those skilled in the art without creative effort based on the technical solutions of the present invention are still within the scope of protection of the present invention.

Claims

1. A red mud dealkalization and filtration aid method based on phosphogypsum-acidic biochar synergy, characterized in that, Includes the following steps: Pretreated phosphogypsum is obtained by crushing, grinding and drying phosphogypsum. Agricultural and forestry waste is crushed, roasted under inert gas protection, cooled, activated by soaking in acid solution, washed, dried and ground to obtain acidic biochar. Mix red mud with water and stir to make red mud slurry; The pretreated phosphogypsum, the acidic biochar, and the chemical filter aid are added sequentially to the red mud slurry, and the mixture is stirred at a constant temperature under stirring conditions to obtain the conditioned red mud slurry. The conditioned red mud slurry was filtered by pressure, and the filtrate and filter cake were collected.

2. The red mud dealkalization and filtration method based on phosphogypsum-acidic biochar synergy as described in claim 1, characterized in that, In the pretreatment step of phosphogypsum, the phosphogypsum is ground and passed through a 100-200 mesh sieve, and then dried in an oven at 45-60℃ until the moisture content is ≤5%.

3. The red mud dealkalization and filtration method based on phosphogypsum-acidic biochar synergy as described in claim 1, characterized in that, In the preparation steps of acidic biochar, the agricultural and forestry waste is one or more mixtures of corn stalks, rice husks, and sawdust.

4. The red mud dealkalization and filtration method based on phosphogypsum-acidic biochar synergy as described in claim 1, characterized in that, In the preparation of acidic biochar, the calcination temperature is 300-600℃ and the calcination time is 3-5h.

5. The red mud dealkalization and filtration method based on phosphogypsum-acidic biochar synergy as described in claim 1, characterized in that, In the preparation steps of acidic biochar, the acid solution is sulfuric acid or hydrochloric acid with a concentration of 0.5-1.0 mol / L, the liquid-solid ratio of the acid solution to the biochar is 5:1-10:1, and the soaking and activation time is 2-4 hours.

6. The red mud dealkalization and filtration method based on phosphogypsum-acidic biochar synergy as described in claim 1, characterized in that, In the preparation of red mud slurry, the liquid-to-solid ratio is 3:1-6:

1.

7. The red mud dealkalization and filtration method based on phosphogypsum-acidic biochar synergy as described in claim 1, characterized in that, Based on dry red mud mass: 5%-15% pretreated phosphogypsum, 3%-8% acidic biochar, and 0.1%-0.5% chemical filter aid.

8. The red mud dealkalization and filtration method based on phosphogypsum-acidic biochar synergy as described in claim 1, characterized in that, The chemical filter aid is a compound system of PL50 polymer filter aid, cationic polyacrylamide and ferric sulfate, with a mass ratio of 2:1:1 to 3:1:

1.

9. The red mud dealkalization and filtration method based on phosphogypsum-acidic biochar synergy as described in claim 1, characterized in that, During the synergistic conditioning process, the stirring speed is 200-400 r / min, the reaction temperature is 60-90℃, and the constant temperature stirring reaction time is 20-40 min.

10. The red mud dealkalization and filtration method based on phosphogypsum-acidic biochar synergy as described in claim 1, characterized in that, In the filter press step, the filter press pressure is 0.8-1.5 MPa, the moisture content of the resulting filter cake is ≤32%, and the alkali removal rate is ≥90%.