A 45S5 bio-glass ceramic powder and its radio frequency plasma-assisted preparation method

By combining wet ball milling and radio frequency plasma treatment, the problems of high energy consumption and difficulty in structural control in the traditional preparation of 45S5 bioactive glass powder were solved, realizing the preparation of bio-glass ceramic powder with low cost and simplified process, and improving the mixing uniformity and spheroidization effect of powder.

CN123105982APending Publication Date: 2026-11-17KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611407868.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional preparation of 45S5 bioactive glass powder suffers from high energy consumption, complex processes, high costs, and difficulty in controlling powder structure. The price of commercial powder also limits its large-scale application.

Method used

A synergistic process of wet ball milling, pre-calcination decarburization, and radio frequency plasma treatment was adopted to prepare 45S5 bio-glass ceramic powder through pre-calcination decarburization and radio frequency plasma treatment, avoiding the traditional high-temperature melting and water quenching, and achieving microscopic mixing uniformity and structural rearrangement of the powder.

Benefits of technology

It reduces preparation costs, simplifies the process, improves the mixing uniformity and structural control of powders, forms a suitable microstructure, and promotes the spheroidization of glass-ceramic powders and the formation of amorphous phases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105982A_ABST
    Figure CN123105982A_ABST
Patent Text Reader

Abstract

This invention discloses a 45S5 bioactive glass ceramic powder and its radio frequency plasma-assisted preparation method, belonging to the field of bioactive glass ceramic powder preparation technology. The specific preparation method of the 45S5 bioactive glass ceramic powder of this invention is as follows: raw materials are weighed according to the target composition of 45S5 bioactive glass, and then a dispersion medium is added to the raw materials to obtain a solid-liquid mixture. The solid-liquid mixture is ball-milled to obtain a mixed slurry. The mixed slurry is then subjected to drying, pre-calcination decarburization, sieving, radio frequency plasma spheroidization, and cooling treatment to obtain 45S5 bioactive glass ceramic powder. This invention achieves the preparation of 45S5 bioactive glass ceramic powder through the synergistic effect of raw materials and preparation process. The process route of this invention is simple, the raw material cost is low, and it also has the value of solid waste resource utilization, and can be used in the fields of bone repair, bioactive coatings, tissue engineering scaffold fillers, and biomedical ceramic composite materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a 45S5 bio-glass ceramic powder and its radio frequency plasma-assisted preparation method, belonging to the field of bioactive glass ceramic powder preparation technology. Background Technology

[0002] 45S5 bioactive glass is a typical bioactive material based on the SiO2-Na2O-CaO-P2O5 system. Its common oxide composition, by mass percentage, includes 45% SiO2, 24.5% Na2O, 24.5% CaO, and 6% P2O5. This type of material has significant application value in bone repair, bio-coatings, dental restorations, and tissue engineering scaffold fillers.

[0003] Traditional 45S5 bioactive glass is typically prepared using a high-temperature melting-water quenching-pulverization process. While this method yields glass materials with relatively uniform composition, it suffers from drawbacks such as high melting temperature, high energy consumption, demanding equipment, a lengthy process flow, and complex subsequent pulverization and sieving. Furthermore, the high price of commercially available 45S5 bioactive glass powder limits its widespread adoption in large-scale basic research and engineering applications.

[0004] The preparation of 45S5 bioglass ceramic powder using inexpensive oxide, carbonate, and phosphate precursors offers significant cost advantages. Furthermore, using resource-recovered phosphogypsum as the calcium carbonate source not only yields 45S5 bioglass ceramic powder with performance comparable to that prepared from pure calcium carbonate but also achieves the goal of resource recovery and utilization of phosphogypsum. In the preparation of 45S5 bioglass ceramic powder, if only ordinary mixing and pre-firing are used, crystalline silicate, phosphate, and sodium-calcium silicate phases easily remain in the powder, while significant particle agglomeration and irregular morphology make it difficult to simultaneously achieve compositional uniformity, melt spheroidization, and structural control. This invention employs radio frequency plasma processing technology, achieving further melting, spheroidization, and structural rearrangement of the precursors after wet ball milling and pre-firing / pre-activation through the synergistic effect of the preparation processes.

[0005] This invention combines low-cost precursor preparation of 45S5 bioglass ceramic powder, pre-calcination decarburization, and radio frequency plasma post-treatment. For carbonate / phosphate system precursors, 45S5-based bioglass ceramic powder is prepared through the synergistic effect of pre-calcination decarburization and radio frequency plasma treatment without traditional whole-body melting and water quenching. The process is simple, the parameters are clear, the cost is low, and it is easy to prepare in the laboratory and for subsequent scale-up. Summary of the Invention

[0006] To address the shortcomings of related technologies, this invention provides a 45S5 bioglass ceramic powder and its radio frequency plasma-assisted preparation method. This invention, through a synergistic process of pre-calcination decarburization and radio frequency plasma post-treatment, provides a new approach for preparing 45S5-based bioglass ceramic powders for carbonate / phosphate system precursors. This approach is simple, low-cost, and easy to scale up, eliminating the need for traditional melt water quenching. It solves the problems of high raw material costs, high energy consumption of traditional melting processes, complex process flow, and difficulty in controlling powder structure in the preparation of 45S5 bioglass powder.

[0007] One objective of this invention is to provide a radio frequency plasma-assisted preparation method for 45S5 bio-glass ceramic powder, specifically comprising the following steps: (1) Weigh SiO2, Na2CO3, CaCO3 and anhydrous CaHPO4 raw materials according to the target composition of 45S5 bioactive glass and mix them to obtain mixed raw materials.

[0008] (2) Add the mixed raw materials to the dispersion medium to obtain a solid-liquid mixture, and then perform wet ball milling to obtain a mixed slurry.

[0009] (3) The mixed slurry is dried to obtain a dry mixed powder.

[0010] (4) The dried mixed powder is pre-calcined and decarbonized to obtain pre-calcined powder.

[0011] (5) The pre-burned powder is sieved to obtain precursor powder.

[0012] (6) The precursor powder was subjected to radio frequency plasma spheroidization treatment and then rapidly cooled to obtain 45S5 bioglass ceramic powder.

[0013] Preferably, the target composition of the bioactive glass in step (1) 45S5 includes, by mass percentage: 44-46% SiO2, 23-26% Na2O, 23-26% CaO, and 5-7% P2O5.

[0014] More preferably, the target composition of the 45S5 bioactive glass in step (1) includes, by mass percentage: 45% SiO2, 24.5% Na2O, 24.5% CaO, and 6% P2O5.

[0015] In the radio frequency plasma treatment process of this invention, Na and / or P are burned off, which is compensated by increasing the amount of Na2CO3 and / or anhydrous CaHPO4 fed.

[0016] More preferably, the CaCO3 raw material in step (1) is commercially available CaCO3 or CaCO3 obtained by resource utilization of phosphogypsum.

[0017] More preferably, the method of resource utilization treatment of phosphogypsum in step (1) is as follows: phosphogypsum is washed with water to remove impurities, then added to deionized water at a solid-liquid ratio of 1:5. After stirring at room temperature for 30 minutes, solid-liquid separation is performed to remove soluble impurities. The resulting calcium-containing solid is mixed with a Na2CO3 aqueous solution with a mass concentration of 1.2 mol / L, at a liquid-solid ratio of 5:1. The mixture is prepared with a CaSO4 to Na2CO3 molar ratio of approximately 1:1.05, and stirred at 60°C for 2 hours to convert CaSO4 to CaCO3. The reaction formula is as follows: After the reaction, solid-liquid separation was performed, and the solid was washed 2-3 times with deionized water to reduce residual sulfate and soluble impurities. The resulting solid was dried at 100℃ to constant weight, pulverized, and sieved to obtain phosphogypsum resource-based CaCO3. When using this calcium source in the formulation of 45S5, the amount added should be calculated based on its actual CaCO3 content to ensure that the CaO equivalent provided is consistent with the target 45S5 formulation.

[0018] More preferably, in step (1), the phosphogypsum is mainly composed of CaSO4·2H2O and contains a small amount of impurities such as SiO2, P2O5, F, Al2O3 and Fe2O3; the composition of the phosphogypsum by mass percentage includes 80~95% CaSO4·2H2O, 1~8% SiO2, 0.5~3% P2O5, 0.1~1% F, 0.1~1% Al2O3 and 0.1~1% Fe2O3.

[0019] Preferably, in step (2), the ball-to-material ratio of wet ball milling is 3~10:1, the ball milling time is 10~30h, the ball milling temperature is 20~25℃, and the ball milling speed is 300rpm.

[0020] More preferably, the grinding balls used in step (2) are agate balls with a diameter of 8 to 15 mm.

[0021] Preferably, the amount of raw material added to the solid-liquid mixture in step (2) is 1 g / mL.

[0022] More preferably, in step (2), the ball-to-material ratio of wet ball milling is 5:1, and the ball milling time is 20h.

[0023] More preferably, the dispersion medium in step (2) is anhydrous ethanol.

[0024] Preferably, the drying temperature in step (3) is 80~120℃.

[0025] More preferably, the drying temperature in step (3) is 100°C.

[0026] Preferably, the conditions for the pre-calcination decarburization treatment in step (4) are as follows: heat up to 120°C at a heating rate of 1°C / min and hold for 1 hour, then heat up to 500°C at a heating rate of 0.5~1°C / min and hold for 2 hours, then heat up to 800°C at a heating rate of 1~2°C / min and hold for 3 hours, and then cool.

[0027] The pre-calcination decarbonization treatment in step (4) of this invention is used to remove adsorbed water, promote the decomposition or pre-reaction of CaCO3 and Na2CO3, and cause silicates and phosphates to undergo preliminary solid-phase reactions.

[0028] More preferably, the pre-calcination decarburization treatment in step (4) is carried out in an air atmosphere.

[0029] Preferably, the particle size of the precursor powder in step (5) is 10~100μm.

[0030] More preferably, the particle size of the precursor powder in step (5) is 20~45μm.

[0031] Preferably, in step (6), the radio frequency plasma spheroidizing treatment uses argon as a protective gas, and the flow rate of argon is 3~15L / min; the power of the radio frequency plasma spheroidizing treatment is 1.0~3.0kW, and the feeding speed is 40g / min.

[0032] Preferably, the rapid cooling rate in step (6) is 10. 4 ℃ / s.

[0033] More preferably, the flow rate of argon gas in step (6) for radio frequency plasma spheroidization is 7 L / min.

[0034] More preferably, the cooling method in step (6) is direct water cooling, in which the radio frequency treated powder is directly injected into the water.

[0035] The radio frequency plasma spheroidizing treatment in step (6) of the present invention can cause the precursor powder to undergo melting, semi-melting, structural rearrangement, partial vitrification, or spheroidization.

[0036] The second objective of this invention is to provide a 45S5 bio-glass ceramic powder prepared using the method of this invention.

[0037] Mechanism of the invention: This invention achieves the preparation of 45S5 bio-glass ceramic powder through a sequential coupling of wet ball milling, pre-calcination decarburization, and radio frequency plasma spheroidization. The preparation process and raw materials of this invention produce a synergistic effect, realizing the rearrangement and reaction of silicate / phosphate structures in the glass powder, improving the microscopic mixing uniformity of the multi-component precursor, promoting the initial solid-phase reaction, and placing the precursor in a pre-activated state more suitable for radio frequency instantaneous melting, providing a raw material basis for subsequent radio frequency plasma treatment. Radio frequency plasma performs overall high-temperature melting and spheroidization of the pre-activated precursor, and rapid cooling inhibits crystallization; thus, the preparation of 45S5 bio-glass ceramic powder is achieved. This continuous process relationship ensures that the preceding treatments directly serve the subsequent radio frequency melting and spheroidization, rather than being independent process steps.

[0038] The beneficial effects of this invention are: (1) The present invention uses SiO2, Na2CO3, CaCO3 and anhydrous CaHPO4 as the main raw materials to replace the direct purchase of high-priced commercial 45S5 bioglass powder; among which the CaCO3 calcium source can be further adopted from phosphogypsum CaCO3 that has been resource-processed, thereby reducing the cost of raw materials and realizing the resource utilization of solid waste.

[0039] (2) The present invention prepares 45S5 bioglass ceramic powder by combining wet ball milling, pre-calcination decarburization and radio frequency plasma treatment. It does not require all raw materials to be melted and quenched into glass blocks by traditional high temperature and then crushed and ground, which can shorten the process flow. At the same time, the pre-activated precursor formed by wet ball milling and pre-calcination decarburization provides a basis for subsequent RF integral melting and spheroidization, so that each process step forms a continuous preparation relationship.

[0040] (3) The present invention removes adsorbed water by segmented heating and pre-calcination to remove carbon, promotes the decomposition or pre-reaction of Na2CO3 and CaCO3, and causes silicates and phosphates to undergo preliminary solid-phase reaction, thereby reducing the risk of pores, hollow particles and explosion caused by gas release during radio frequency processing.

[0041] (4) This invention achieves a suitable micro-mixing and pre-activation state for subsequent radio frequency (RF) treatment by sequentially coupling wet ball milling, pre-calcination decarburization, and radio frequency plasma spheroidization. The specific preparation method process flow diagram is shown below. Figure 1 As shown, the preparation method of this invention improves the mixing uniformity of the multi-component precursor, effectively reduces the gas generated by carbonate decomposition and promotes the initial solid-phase reaction. Subsequently, the instantaneous high temperature of RF promotes the overall melting and spheroidization of the pre-activated particles, and rapid cooling further inhibits crystallization. Thus, the three processes form an interconnected and synergistic relationship, rather than a simple process superposition, which can simultaneously improve the agglomeration state, sphericity, and amorphous / crystalline phase ratio of the powder. Attached Figure Description

[0042] Figure 1 This is a schematic diagram of the process flow of the preparation method of the present invention.

[0043] Figure 2 The images show the SEM morphology, EDS elemental distribution, and elemental composition analysis of the powder materials prepared in Example 1 and Comparative Example 2 of this invention; wherein... Figure 2 Image (a) shows the SEM morphology, EDS elemental surface distribution, and elemental composition analysis of the powder material in Example 1. Figure 2 Figure (b) shows the SEM morphology, EDS elemental distribution, and elemental composition analysis of the powder material in Comparative Example 2.

[0044] Figure 3 The images show the XRD patterns of the powder materials prepared in Example 1 and Comparative Examples 1-2 of this invention.

[0045] Figure 4 The images show the FTIR spectra of the powder materials prepared in Example 1 and Comparative Example 2 of this invention. Detailed Implementation

[0046] To better illustrate the purpose, technical solution, and advantages of this invention, the invention will be further described below with reference to specific embodiments. In the embodiments and comparative examples of this invention, unless otherwise specified, all chemical reagents used were commercially available analytical grade reagents.

[0047] Example 1 A radio frequency plasma-assisted preparation method for 45S5 bio-glass ceramic powder specifically includes the following steps: (1) The raw materials SiO2, Na2CO3, CaCO3 and anhydrous CaHPO4 (45.00g SiO2, 45.54g Na2CO3, 34.82g CaCO3 and 12.11g anhydrous CaHPO4 were weighed according to the target composition of 45S5 bioactive glass by mass percentage, which includes 45% SiO2, 24.5% Na2O, 24.5% CaO and 6% P2O5, respectively, and were mixed to obtain the mixed raw materials.

[0048] (2) Add the mixed raw materials to anhydrous ethanol to obtain a solid-liquid mixture. The amount of mixed raw materials added to the solid-liquid mixture is 1 g / mL. The solid-liquid mixture is wet-milled at 20°C for 20 h at a ball speed of 300 rpm under the condition of a ball-to-material ratio of 5:1. Agate balls with a diameter of 8 mm are used as grinding balls to obtain a mixed slurry.

[0049] (3) Dry the mixed slurry at 100°C to constant weight to obtain dry mixed powder.

[0050] (4) The dry mixed powder is spread in a thin layer in an alumina boat and pre-calcined for decarburization in an air atmosphere. The pre-calcination and decarburization conditions are as follows: the temperature is increased from room temperature to 120°C at a heating rate of 1°C / min and held for 1 hour, then increased to 500°C at a heating rate of 1°C / min and held for 2 hours, then increased to 800°C at a heating rate of 1°C / min and held for 3 hours, then cooled to 200°C in the furnace and placed in a desiccator to cool to room temperature to obtain pre-calcined powder. This step removes adsorbed water and promotes the initial reaction of carbonates, silicates and phosphates.

[0051] (5) Grind the pre-calcined powder into powder and sieve it to obtain precursor powder with a particle size of 20~45µm.

[0052] (6) The precursor powder was placed in an RF plasma device for RF plasma spheroidization treatment, using argon as the protective gas with a flow rate of 7 L / min, an RF power of 2 kW, and a feed rate of 40 g / min. The powder was then directly injected into water for rapid cooling at a rate of approximately 10 g / min. 4 ℃ / s, to obtain 45S5 bio-glass ceramic powder.

[0053] The powder obtained in this embodiment was characterized by XRD, SEM-EDS, and FTIR. SEM-EDS analysis showed that the powder prepared in this embodiment contains the main elements Si, Na, Ca, P, and O. (See [link to relevant documentation]). Figure 2 (a) XRD shows the coexistence of amorphous dispersed background and crystalline phase diffraction peaks, indicating that radio frequency treatment promoted partial melting and vitrification of the crystalline phase. This suggests that the 45S5-based bio-glass ceramic powder exhibits a coexistence of crystalline and amorphous phases. (See also...) Figure 3 FTIR is used to analyze Si-O-Si, Si-O-Ca, and PO4. 3- Structural features, in the range of 1000-1100cm -1 The range contains Si-O-Si, Si-O-Ca and / or PO4 3- Relevant characteristic absorption peaks; at 925 cm⁻¹ -1 Nearby, there are peaks related to Si-O-Ca or non-bridged oxygen structures; at 620 cm⁻¹ -1 and 530cm -1 PO4 is present nearby 3- The bending vibration-related peaks indicate that radio frequency treatment promoted silicate / phosphate structural rearrangement and reactions. (See [reference needed]) Figure 4 .

[0054] Example 2 A radio frequency plasma-assisted preparation method for 45S5 bio-glass ceramic powder specifically includes the following steps: (1) The raw materials SiO2, Na2CO3, CaCO3 and anhydrous CaHPO4 (45.00g SiO2, 45.54g Na2CO3, 34.82g CaCO3 and 12.11g anhydrous CaHPO4 were weighed according to the target composition of 45S5 bioactive glass by mass percentage, which includes 45% SiO2, 24.5% Na2O, 24.5% CaO and 6% P2O5, respectively, and were mixed to obtain the mixed raw materials.

[0055] (2) Add the mixed raw materials to anhydrous ethanol to obtain a solid-liquid mixture. The amount of mixed raw materials added to the solid-liquid mixture is 1 g / mL. The solid-liquid mixture is wet-milled at 25°C for 20 h at a ball speed of 300 rpm under the condition of a ball-to-material ratio of 5:1. Agate balls with a diameter of 15 mm are used as grinding balls to obtain a mixed slurry.

[0056] (3) Dry the mixed slurry at 100°C to constant weight to obtain dry mixed powder.

[0057] (4) The dry mixed powder is spread in a thin layer in an alumina boat and pre-calcined for decarburization in an air atmosphere. The pre-calcination and decarburization conditions are as follows: the temperature is increased from room temperature to 120°C at a heating rate of 1°C / min and held for 1 hour, then increased to 500°C at a heating rate of 0.5°C / min and held for 2 hours, then increased to 800°C at a heating rate of 1.5°C / min and held for 3 hours, then cooled to 200°C in the furnace and placed in a desiccator to cool to room temperature to obtain pre-calcined powder. This step removes adsorbed water and promotes the initial reaction of carbonates, silicates and phosphates.

[0058] (5) Grind the pre-calcined powder into powder and sieve it to obtain precursor powder with a particle size of 20~45µm.

[0059] (6) The precursor powder was placed in an RF plasma device for RF plasma spheroidization treatment, using argon as the protective gas with a flow rate of 7 L / min, an RF power of 1.5 kW, and a feed rate of 40 g / min. The powder was then directly injected into water for rapid cooling at a rate of approximately 10 g / min. 4 ℃ / s, to obtain 45S5 bio-glass ceramic powder.

[0060] The ceramic powder prepared in this embodiment can detect the main elements of the 45S5 system, namely O, Na, Si, P, and Ca. In typical regions, the contents of O, Na, Si, P, and Ca by mass percentage are 39.91%, 16.68%, 20.56%, 2.20%, and 18.58%, respectively, indicating that the main elements of the sample are consistent with the 45S5 system.

[0061] The SEM morphology of this embodiment is basically similar to that of Example 1. XRD analysis shows that the amorphous dispersed background is obvious in Example 2, and the diffraction peaks of some crystalline phases are relatively weakened, indicating that this embodiment achieves powder melting and structural rearrangement, thereby increasing the amorphous phase content and inhibiting the formation of crystalline phases.

[0062] Example 3 A radio frequency plasma-assisted preparation method for 45S5 bio-glass ceramic powder, wherein the CaCO3 raw material used in this embodiment is derived from the resource-based treatment of phosphogypsum, specifically includes the following steps: (1) Phosphogypsum was added to deionized water and mixed to obtain a mixture. The amount of phosphogypsum added to the mixture was 0.2 g / mL. After stirring at room temperature for 30 min, solid-liquid separation was performed to obtain calcium-containing solid to remove soluble impurities. The obtained calcium-containing solid was mixed with sodium carbonate aqueous solution and a conversion reaction was carried out at a ratio of approximately 1:1.05 between CaSO4 and Na2CO3 in the calcium-containing solid (the content of CaSO4 in the calcium-containing solid can be determined by taking a small amount of calcium-containing solid and testing it by EDTA). During the conversion reaction, the liquid-solid ratio of the calcium-containing solid to the 1.2 mol / L sodium carbonate aqueous solution was 5:1. The reaction was stirred at 60 °C for 2 h to convert CaSO4 to CaCO3. After the reaction, solid-liquid separation was performed and the mixture was washed twice with deionized water to reduce residual sulfate and soluble impurities. Then it was dried at 100 °C until constant temperature. The material was crushed and sieved to obtain CaCO3 raw material from phosphogypsum. The amount of CaCO3 raw material from phosphogypsum was calculated based on the actual CaCO3 content to ensure that the CaO equivalent provided was consistent with the target 45S5 formulation. SiO2, Na2CO3, CaCO3 and anhydrous CaHPO4 raw materials were weighed according to the target composition of 45S5 bioactive glass, which includes 45% SiO2, 24.5% Na2O, 24.5% CaO and 6% P2O5 by mass percentage (45.00g SiO2, 45.54g Na2CO3, 34.82g CaCO3 and 12.11g anhydrous CaHPO4 per 100g of target oxide system, this ratio compensates for the burn-off of Na and P components during radio frequency processing) and mixed to obtain mixed raw material.

[0063] (2) Add the mixed raw materials to anhydrous ethanol to obtain a solid-liquid mixture. The amount of mixed raw materials added to the solid-liquid mixture is 1 g / mL. The solid-liquid mixture is wet-milled at 22℃ for 20 h at a ball speed of 300 rpm under the condition of ball-to-material ratio of 5:1. Agate balls with a diameter of 10 mm are used as grinding balls to obtain a mixed slurry.

[0064] (3) Dry the mixed slurry at 100°C to constant weight to obtain dry mixed powder.

[0065] (4) The dry mixed powder is spread in a thin layer in an alumina boat and pre-calcined for decarburization in an air atmosphere. The pre-calcination and decarburization conditions are as follows: the temperature is increased from room temperature to 120°C at a heating rate of 1°C / min and held for 1 hour, then increased to 500°C at a heating rate of 0.8°C / min and held for 2 hours, then increased to 800°C at a heating rate of 2°C / min and held for 3 hours, then cooled to 200°C in the furnace and placed in a desiccator to cool to room temperature to obtain pre-calcined powder. This step removes adsorbed water and promotes the initial reaction of carbonates, silicates and phosphates.

[0066] (5) Grind the pre-calcined powder into powder and sieve it to obtain precursor powder with a particle size of 20~45µm.

[0067] (6) The precursor powder was placed in an RF plasma device for RF plasma spheroidization treatment, using argon as the protective gas with a flow rate of 7 L / min, an RF power of 3 kW, and a feeding speed of 40 g / min. The powder was then directly injected into water for rapid cooling at a rate of approximately 10 g / min. 4 ℃ / s, to obtain 45S5 bio-glass ceramic powder.

[0068] The powder obtained in this embodiment was characterized by XRD, SEM-EDS, and FTIR. SEM-EDS analysis showed that the powder prepared in this embodiment contains the main elements Si, Na, Ca, P, and O. XRD showed that an amorphous dispersed background coexists with crystalline phase diffraction peaks, indicating that this embodiment prepared 45S5-based bioglass ceramic powder containing both crystalline and amorphous phases. FTIR analysis showed that the ceramic powder material prepared in this embodiment has a wavelength range of 1000-1100 cm⁻¹. -1 The range contains Si-O-Si, Si-O-Ca and / or PO4 3- Relevant characteristic absorption peaks; at 925 cm⁻¹ -1 Nearby, there are peaks related to Si-O-Ca or non-bridged oxygen structures; at 620 cm⁻¹ -1 and 530cm -1 PO4 is present nearby 3- The bending vibration-related peaks indicate that the ceramic powder in this embodiment underwent silicate / phosphate structural rearrangement and reaction.

[0069] Comparative Example 1 This comparative example uses the same method as Example 1 to prepare 45S5 bio-glass ceramic powder, the only difference being that this comparative example uses water-cooled wall cooling to cool the powder after radio frequency plasma spheroidization treatment, specifically including the following steps: (1) The raw materials SiO2, Na2CO3, CaCO3 and anhydrous CaHPO4 (45.00g SiO2, 45.54g Na2CO3, 34.82g CaCO3 and 12.11g anhydrous CaHPO4 were weighed according to the target composition of 45S5 bioactive glass by mass percentage, which includes 45% SiO2, 24.5% Na2O, 24.5% CaO and 6% P2O5, respectively, and were mixed to obtain the mixed raw materials.

[0070] (2) Add the mixed raw materials to anhydrous ethanol to obtain a solid-liquid mixture. The amount of mixed raw materials added to the solid-liquid mixture is 1 g / mL. The solid-liquid mixture is wet-milled at 20°C for 20 h at a ball speed of 300 rpm under the condition of a ball-to-material ratio of 5:1. Agate balls with a diameter of 8 mm are used as grinding balls to obtain a mixed slurry.

[0071] (3) Dry the mixed slurry at 100°C to constant weight to obtain dry mixed powder.

[0072] (4) The dry mixed powder is spread in a thin layer in an alumina boat and pre-calcined for decarburization in an air atmosphere. The pre-calcination and decarburization conditions are as follows: the temperature is increased from room temperature to 120°C at a heating rate of 1°C / min and held for 1 hour, then increased to 500°C at a heating rate of 1°C / min and held for 2 hours, then increased to 800°C at a heating rate of 1°C / min and held for 3 hours, then cooled to 200°C in the furnace and placed in a desiccator to cool to room temperature to obtain pre-calcined powder. This step removes adsorbed water and promotes the initial reaction of carbonates, silicates and phosphates.

[0073] (5) Grind the pre-calcined powder into powder and sieve it to obtain precursor powder with a particle size of 20~45μm.

[0074] (6) The precursor powder is placed in an RF plasma device for RF plasma spheroidization treatment. Argon is used as the protective gas, with an argon flow rate of 7 L / min, an RF power of 2 kW, and a feeding speed of 40 g / min. After RF plasma treatment, the powder enters a collection chamber with a water-cooled wall. The water-cooled wall lowers the temperature of the collection chamber, cooling the powder within the chamber at a rate of approximately 10. 3 ℃ / s, to obtain 45S5 bio-glass ceramic powder.

[0075] This comparative example uses water-cooled walls for indirect cooling of the powder after radio frequency plasma treatment. The cooling rate of this comparative example powder is relatively low, resulting in a longer residence time in the high-temperature and crystallization temperature ranges, thus making crystallization more likely. XRD results show (see...) Figure 3The diffraction peaks of the crystalline phase in this comparative example are more obvious, and the amorphous diffuse background is relatively weakened, indicating that the lower cooling rate is not conducive to the preservation of the amorphous structure and promotes the formation of the crystalline phase.

[0076] Comparative Example 2 This comparative example uses the same method as Example 1 to prepare powder materials, the only difference being that the precursor powder is not subjected to radio frequency plasma treatment in this comparative example. Specifically, the following steps are included: (1) The raw materials SiO2, Na2CO3, CaCO3 and anhydrous CaHPO4 (45.00g SiO2, 45.54g Na2CO3, 34.82g CaCO3 and 12.11g anhydrous CaHPO4 were weighed according to the target composition of 45S5 bioactive glass by mass percentage, which includes 45% SiO2, 24.5% Na2O, 24.5% CaO and 6% P2O5, respectively, and were mixed to obtain the mixed raw materials.

[0077] (2) Add the mixed raw materials to anhydrous ethanol to obtain a solid-liquid mixture. The amount of mixed raw materials added to the solid-liquid mixture is 1 g / mL. The solid-liquid mixture is wet-milled at 20°C for 20 h at a ball speed of 300 rpm under the condition of a ball-to-material ratio of 5:1. Agate balls with a diameter of 8 mm are used as grinding balls to obtain a mixed slurry.

[0078] (3) Dry the mixed slurry at 100°C to constant weight to obtain dry mixed powder.

[0079] (4) The dry mixed powder is spread in a thin layer in an alumina boat and pre-calcined for decarburization in an air atmosphere. The pre-calcination and decarburization conditions are as follows: the temperature is increased from room temperature to 120°C at a heating rate of 1°C / min and held for 1 hour, then increased to 500°C at a heating rate of 1°C / min and held for 2 hours, then increased to 800°C at a heating rate of 1°C / min and held for 3 hours, then cooled to 200°C in the furnace and placed in a desiccator to cool to room temperature to obtain pre-calcined powder. This step removes adsorbed water and promotes the initial reaction of carbonates, silicates and phosphates.

[0080] (5) Grind the pre-calcined powder into powder and sieve it to obtain precursor powder with a particle size of 20~45μm.

[0081] XRD analysis was performed on the precursor powder prepared in this comparative example (see [reference]). Figure 3 Analysis revealed that the precursor powder exhibited sharp diffraction peaks at approximately 23°, 26°, 33°-35°, and 49°, indicating that the pre-calcined powder still contained a significant amount of crystalline silicates, phosphates, or sodium-calcium silicates, and had not yet formed a fully vitrified structure.

[0082] SEM observation revealed that the pre-calcined precursor powder in this comparative example exhibited significant agglomeration, with particles adhering to each other, resulting in poor overall dispersibility. The particles had irregular outlines with sharp edges and low sphericity. Figure 2 As shown in (b); EDS elemental distribution results show that Si, Na, Ca, and P are distributed throughout the overall region, but there are certain differences in brightness in local areas. Among them, the distribution of P is relatively uneven, indicating that although the powder has undergone preliminary solid-phase reaction after pre-calcination, there is still a certain degree of inhomogeneity in its microstructure and composition. XRD analysis shows that the pre-calcined precursor of this comparative example has obvious sharp diffraction peaks around 23°, 26°, 33°-35°, and 49°, indicating that it still contains a lot of crystalline silicates, phosphates, and sodium-calcium silicate phases. FTIR analysis results are as follows. Figure 4 As shown, at 3450cm -1 1630cm -1 1450cm -1 1080-1030cm -1 925cm -1 620cm -1 and 530cm -1 Corresponding absorption peaks appeared in the vicinity, especially at 1000-1100 cm⁻¹. -1 and 925cm -1 The nearby peak is mainly related to the silicate structure, 620 cm⁻¹ -1 and 530cm -1 Nearby peaks and PO4 3- Vibration is relevant; the relatively broad and gentle structural peaks in this comparative example indicate that the precursor has not undergone further high-temperature melting and structural rearrangement without radio frequency plasma treatment.

[0083] Comparative Example 3 This comparative example uses the same method as Example 1 to prepare 45S5 bio-glass ceramic powder, the only difference being that this comparative example does not perform pre-calcination decarburization treatment on the dried mixed powder. Specifically, it includes the following steps: (1) The raw materials SiO2, Na2CO3, CaCO3 and anhydrous CaHPO4 (45.00g SiO2, 45.54g Na2CO3, 34.82g CaCO3 and 12.11g anhydrous CaHPO4 were weighed according to the target composition of 45S5 bioactive glass by mass percentage, which includes 45% SiO2, 24.5% Na2O, 24.5% CaO and 6% P2O5, respectively, and were mixed to obtain the mixed raw materials.

[0084] (2) Add the mixed raw materials to anhydrous ethanol to obtain a solid-liquid mixture. The amount of mixed raw materials added to the solid-liquid mixture is 1 g / mL. The solid-liquid mixture is wet-milled at 20°C for 20 h at a ball speed of 300 rpm under the condition of a ball-to-material ratio of 5:1. Agate balls with a diameter of 8 mm are used as grinding balls to obtain a mixed slurry.

[0085] (3) Dry the mixed slurry at 100°C to constant weight to obtain dry mixed powder.

[0086] (4) Grind the dry mixed powder and sieve it to obtain precursor powder with a particle size of 20~45μm.

[0087] (5) The precursor powder was placed in an RF plasma device for RF plasma spheroidization treatment. Argon was used as the protective gas, with an argon flow rate of 7 L / min, an RF power of 2 kW, and a feeding speed of 40 g / min. The powder was then directly injected into water for rapid cooling at a rate of approximately 10 g / min. 4 ℃ / s, to obtain 45S5 bio-glass ceramic powder.

[0088] Because this comparative example did not undergo pre-calcination, the residual adsorbed water and carbonates in the precursor decomposed in the high-temperature zone of the radio frequency (RF) circuit, easily releasing more gas. This increased the likelihood of pores and hollow structures forming inside the particles, as well as the volatilization of Na and P, leading to localized compositional inhomogeneity. The lack of pre-calcination decarburization treatment also hindered the formation of a stable pre-activated state, reducing the uniformity of particle melting, spheroidization, and structural rearrangement during the RF process.

[0089] Comparative Example 4 This comparative example uses the same method as Example 1 to prepare 45S5 bio-glass ceramic powder, the only difference being that the raw materials in this comparative example are not ball-milled. The specific steps include: (1) The raw materials SiO2, Na2CO3, CaCO3 and anhydrous CaHPO4 (45.00g SiO2, 45.54g Na2CO3, 34.82g CaCO3 and 12.11g anhydrous CaHPO4 were weighed according to the target composition of 45S5 bioactive glass by mass percentage, which includes 45% SiO2, 24.5% Na2O, 24.5% CaO and 6% P2O5, respectively. This ratio compensates for the burn-off of Na and P components during radio frequency processing) and stirred and mixed evenly to obtain the mixed raw materials.

[0090] (2) The mixed raw materials are spread in a thin layer in an alumina boat and pre-calcined for decarburization in an air atmosphere. The conditions for pre-calcination for decarburization are as follows: the temperature is increased from room temperature to 120°C at a heating rate of 1°C / min and held for 1 hour, then the temperature is increased to 500°C at a heating rate of 1°C / min and held for 2 hours, then the temperature is increased to 800°C at a heating rate of 1°C / min and held for 3 hours, then the furnace is cooled to 200°C and taken out and placed in a desiccator to cool to room temperature to obtain pre-calcined powder. This step removes adsorbed water and promotes the initial reaction of carbonates, silicates and phosphates.

[0091] (3) Grind the pre-calcined powder into powder and sieve it to obtain precursor powder with a particle size of 20~45μm.

[0092] (4) The precursor powder was placed in an RF plasma device for RF plasma spheroidization treatment. Argon was used as the protective gas, with an argon flow rate of 7 L / min, an RF power of 2 kW, and a feeding speed of 40 g / min. The powder was then directly injected into water for rapid cooling at a cooling rate of approximately 10 g / min. 4 ℃ / s, to obtain 45S5 bio-glass ceramic powder.

[0093] Because this comparative example did not undergo wet ball milling, the raw materials were in a macroscopically mixed state. At the microscopic scale, SiO2, Na2CO3, CaCO3, and CaHPO4 were prone to localized enrichment and depletion. During pre-calcination, the degree of solid-phase reaction varied in different regions, resulting in uneven distribution of the formed silicate, phosphate, and sodium-calcium silicate phases. After radio frequency treatment, although the particles could melt and spheroidize, localized compositional differences led to uneven EDS element distribution and variations in the degree of melting and spheroidization between particles.

[0094] In summary, this invention achieves the preparation of 45S5 bio-glass ceramic powder through the synergistic effect of the preparation process and raw materials. The wet ball milling, pre-calcination decarburization, and radio frequency plasma treatment of this invention form a continuous sequential synergistic relationship: improving the precursor state from the perspective of microscopic mixing uniformity and pre-activation, creating conditions for subsequent RF instantaneous melting, spheroidization, and rapid cooling, thereby achieving synergistic effects of raw material resource utilization, powder spheroidization, and structural control. Under the instantaneous high temperature of RF plasma, the particle surface can preferentially undergo instantaneous melting and tend to spheroidize under the action of surface tension; subsequent direct quenching in water causes rapid solidification of the molten surface and inhibits crystallization, thus facilitating the formation of a core-shell structure with a 45S5 matrix as the core and an amorphous surface rich in amorphous structures. This structure can provide high reactivity to the surface while maintaining the composition of the particle matrix.

[0095] This invention uses inexpensive and readily available SiO2, Na2CO3, CaCO3, and anhydrous CaHPO4 as main raw materials. Wet ball milling improves the uniformity of raw material mixing, and radio frequency plasma is used to replace the traditional high-temperature melting process, shortening the material preparation process and reducing dependence on traditional high-temperature melting equipment. Simultaneously, CaCO3 is obtained through the resource utilization of phosphogypsum, further reducing calcium source costs and realizing the resource utilization of solid waste. The resulting powder, detected by SEM-EDS, contains the main elements of the 45S5 system, including Si, Na, Ca, P, and O. FTIR reveals a silicate-phosphate network structure, and XRD shows a structure with coexisting amorphous and crystalline phases. Furthermore, radio frequency treatment improves the powder's agglomeration state and sphericity, indicating that this invention can obtain 45S5-based bio-glass ceramic powder with good compositional characteristics, tunable structure, and improved particle morphology. Therefore, this invention provides a method for preparing 45S5 bioglass ceramic powder with low raw material cost, relatively simple process flow, adjustable radio frequency power and cooling method, and the ability to simultaneously control the degree of material crystallization and powder particle morphology. This provides a new technical route for the low-cost preparation of 45S5 bioglass ceramic powder and its application in bone repair, bioactive coatings, tissue engineering scaffolds and biomedical composite materials.

[0096] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments. The terminology used herein is chosen to best explain the principles, practical application, or improvement of the technology in the market, or to enable others skilled in the art to understand the embodiments disclosed herein.

Claims

1. A method for the radio frequency plasma assisted preparation of 45S5 bioglass ceramic powder, characterized in that, Specifically, the following steps are included: (1) Weigh out SiO2, Na2CO3, CaCO3 and anhydrous CaHPO4 raw materials according to the target composition of 45S5 bioactive glass and mix them to obtain mixed raw materials; (2) Add the mixed raw materials to the dispersion medium to obtain a solid-liquid mixture, and then perform wet ball milling to obtain a mixed slurry; (3) The mixed slurry is dried to obtain a dried mixed powder; (4) The dried mixed powder is subjected to pre-calcination and decarburization treatment to obtain pre-calcined powder; (5) The pre-calcined powder is sieved to obtain precursor powder; (6) The precursor powder was subjected to radio frequency plasma spheroidization treatment and then rapidly cooled to obtain 45S5 bioglass ceramic powder.

2. The method of radio frequency plasma assisted production of 45S5 bioglass ceramic powder according to claim 1, characterized in that, The target composition of the bioactive glass in step (1) includes, by mass percentage: 44-46% SiO2, 23-26% Na2O, 23-26% CaO, and 5-7% P2O5.

3. The method of claim 1, wherein the radio frequency plasma assisted preparation of 45S5 bioglass ceramic powder is characterized by, In step (2), the ball-to-material ratio of wet ball milling is 3~10:1, the ball milling time is 10~30h, the ball milling temperature is 20~25℃, and the ball milling speed is 300rpm.

4. A method for the radio frequency plasma assisted production of 45S5 bioglass ceramic powder according to claim 1, characterized by, The amount of mixed raw materials added in the solid-liquid mixture in step (2) is 1 g / mL.

5. A method of radio frequency plasma assisted production of 45S5 bioglass ceramic powder according to claim 1, characterized in that, The drying temperature in step (3) is 80~120℃.

6. The method of claim 1, wherein the radio frequency plasma assisted production of 45S5 bioglass ceramic powder is characterized by, The conditions for the pre-calcination decarburization treatment in step (4) are as follows: heat up to 120°C at a heating rate of 1°C / min and hold for 1 hour, then heat up to 500°C at a heating rate of 0.5~1°C / min and hold for 2 hours, then heat up to 800°C at a heating rate of 1~2°C / min and hold for 3 hours, and then cool.

7. The radio frequency plasma-assisted preparation method of 45S5 bio-glass ceramic powder according to claim 1, characterized in that, The particle size of the precursor powder in step (5) is 10~100μm.

8. The radio frequency plasma-assisted preparation method of 45S5 bio-glass ceramic powder according to claim 1, characterized in that, In step (6), the radio frequency plasma spheroidizing treatment uses argon as a protective gas with an argon flow rate of 3~15L / min, a power of 1.0~3.0kW, and a feeding speed of 40g / min.

9. The radio frequency plasma-assisted preparation method of 45S5 bio-glass ceramic powder according to claim 1, characterized in that, The cooling rate of the step (6) rapid cooling is 10 4 °C / s.

10. 45S5 bioglass ceramic powder prepared by the method according to any one of claims 1 to 9.