A corrosion-resistant, high-humidity withstand voltage porcelain insulator and its preparation method

By preparing yttrium-doped aluminum-titanium composite oxide particles and fluorination treatment, combined with specific minerals, the performance problems of porcelain insulators in humid and corrosive environments were solved, improving high humidity withstand voltage and corrosion resistance, and enhancing the durability and safety of porcelain insulators.

CN123106162APending Publication Date: 2026-11-17JIANGXI HUAYI ELECTRIC PORCELAIN CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611543349.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-08
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Porcelain insulators are prone to forming a continuous water film under humid or polluted conditions, which leads to an increase in leakage current along the surface, local arcing, and in turn, flashover accidents. At the same time, they are also affected by environmental corrosion, which reduces their electrical strength and mechanical properties.

Method used

By preparing yttrium-doped aluminum-titanium composite oxide particles and subjecting them to fluorination treatment, combined with kaolin, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder, a corrosion-resistant, high-humidity, voltage-resistant porcelain insulator is formed. The yttrium ion stabilizes the crystal structure and the fluorination treatment improves the corrosion resistance and density of the material.

Benefits of technology

It improves the corrosion resistance and power frequency wet resistance of porcelain insulators, enhances the durability and safety of insulators, and reduces maintenance and replacement costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure REF-OBJ-1791344842218-000001
    Figure REF-OBJ-1791344842218-000001
Patent Text Reader

Abstract

This invention discloses a method for preparing a corrosion-resistant, high-humidity withstand voltage porcelain insulator. The steps include: (1) preparing yttrium-doped aluminum-titanium composite oxide particles to obtain composite oxide particles; (2) coating zirconium oxide and simultaneously fluorinating it to obtain loaded particles; (3) mixing kaolin, the loaded particles, potassium feldspar, sodium feldspar, quartz powder, and calcium oxide powder evenly to form a mixture, adding water to the mixture, mixing well, pouring into a mold for die casting, drying, demolding, and firing to obtain the corrosion-resistant, high-humidity withstand voltage porcelain insulator. The porcelain insulator prepared by the method of this invention has good corrosion resistance and high high-humidity withstand voltage, improving the durability and safety of the insulator and reducing maintenance and replacement costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of ceramic insulator materials technology, and in particular to a corrosion-resistant, high-humidity, voltage-resistant ceramic insulator and its preparation method. Background Technology

[0002] Porcelain insulators, as the most widely used and oldest external insulation equipment in power systems, operate under long-term exposure to the atmospheric environment, enduring the combined effects of multiple factors such as electric fields, mechanical stress, temperature changes, and environmental corrosion. With the large-scale construction of ultra-high voltage transmission projects and the increasingly severe air pollution situation, the power frequency wet withstand voltage level and corrosion resistance of porcelain insulators have become key bottlenecks restricting the safe and reliable operation of external insulation in power grids.

[0003] Under humid or polluted conditions, a continuous water film easily forms on the surface of porcelain insulators. This water film bridges the air gaps between the skirts, leading to a sharp increase in surface leakage current. When the Joule heating generated by the leakage current causes localized water film vaporization, forming a dry area, electric field distortion triggers a localized electric arc. If the arc continues to develop and penetrates both poles, it evolves into a flashover accident. Flashover accidents often cause large-area, prolonged power outages. Therefore, improving the power frequency wet withstand voltage of porcelain insulators to fundamentally suppress surface discharge under wet and polluted conditions is an urgent engineering need. Meanwhile, the chemical corrosion of porcelain insulator bodies by environmental factors such as industrial emissions, sea fog salinity, and acid rain cannot be ignored. Acidic media erode the glassy phase in the porcelain body, leading to surface roughening and increased porosity, which in turn provides favorable conditions for dirt deposition and moisture retention, forming a "corrosion-dirt accumulation-wet flashover" cycle. Corrosion not only reduces the electrical strength of the insulator but also weakens its mechanical properties, accelerating aging and failure. Summary of the Invention

[0004] Therefore, the present invention provides a method for preparing a corrosion-resistant, high-humidity, voltage-resistant porcelain insulator, the steps of which include: (1) Prepare an ethanol solution of tetrabutyl titanate; mix glacial acetic acid, deionized water, propylene glycol and ethanol in a reaction vessel to form a mixture; add aluminum nitrate nonahydrate and yttrium nitrate hexahydrate to the mixture, stir and mix after the addition is complete, then add the ethanol solution of tetrabutyl titanate while stirring, heat and keep warm in a water bath after the addition is complete, add ammonia water, then keep warm and stir, separate solid and liquid, wash the solid phase, dry, calcine to obtain composite oxide particles; (2) Dissolve zirconium nitrate in deionized water to prepare a coating solution; add the composite oxide particles to an anhydrous ethanol solution of hydroxypropyl cellulose, stir under ultrasonic conditions to form a suspension, and then add the coating solution to the suspension under stirring. After the addition is completed, place the mixture under negative pressure and keep it under pressure, then heat it in a water bath for aging, separate the solid and liquid, dry the solid phase, soak the dried solid phase in ammonium fluoride solution, keep it under negative pressure, separate the solid and liquid after the pressure is kept, dry the solid phase, and calcine to obtain the loaded particles. (3) Mix kaolin, the loaded particles, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder evenly to form a mixture, add water to the mixture, mix well, pour into a mold for die casting, dry, demold, and fire to obtain the corrosion-resistant, high-humidity, voltage-resistant porcelain insulator.

[0005] Further, in step (1), the mass percentage of the ethanol solution of tetrabutyl titanate is 20% to 30%, and the solvent is ethanol; the mixing ratio of glacial acetic acid, deionized water, propylene glycol and ethanol is glacial acetic acid: deionized water: propylene glycol: ethanol = 10 mL: 5 to 8 mL: 1 to 3 mL: 20 to 25 mL; the ratio of aluminum nitrate nonahydrate, yttrium nitrate hexahydrate and ethanol solution of tetrabutyl titanate added to the mixture is mixture: aluminum nitrate nonahydrate: yttrium nitrate hexahydrate: ethanol solution of tetrabutyl titanate = 50 mL: 8 to 10 g: 1 to 5 g: 50 to 60 mL.

[0006] Further, in step (1), the water bath is heated to 50±5℃ and kept warm, and ammonia is added to adjust the pH to 10; then it is kept warm and stirred for more than 10 hours, and the calcination temperature is 400~450℃ and the calcination time is 2~3 hours.

[0007] Further, in step (2), the ratio of zirconium nitrate added to deionized water is zirconium nitrate:deionized water = 20-25g:200mL; the ratio of the composite oxide particles added to the anhydrous ethanol solution of hydroxypropyl cellulose is composite oxide particles:anhydrous ethanol solution of hydroxypropyl cellulose = 5g:150-200mL, wherein the mass percentage of hydroxypropyl cellulose in the anhydrous ethanol solution of hydroxypropyl cellulose is 1%-2%, and the solvent is ethanol; the ratio of the coating solution added to the suspension is suspension:coating solution = 10mL:3-5mL, and the suspension is heated in a water bath to 60±5℃ and aged for 2-4 hours.

[0008] Further, in step (2), the concentration of ammonium fluoride in the ammonium fluoride solution is 0.5-1g / 100mL, and the solvent is water; the ratio of the dried solid phase to the ammonium fluoride solution is 1g: 20-50mL, the calcination temperature is 450-480℃, and the calcination time is 1-2h.

[0009] Further, in step (3), the components are as follows by weight: 50 parts kaolin, 20-30 parts loaded particles, 5-10 parts potassium feldspar, 3-6 parts sodium feldspar, 15-20 parts quartz powder, and 1-2 parts calcium oxide powder; wherein the kaolin, potassium feldspar, sodium feldspar, quartz powder, and calcium oxide powder are all sieved powders that have passed through a 300-mesh sieve.

[0010] Further, in step (3), water is added to the mixture to prepare a mud with a water content of 6wt% to 7wt%. The calcination process is as follows: first, the temperature is raised to 600℃ at a rate of 3℃ / min and held for 30min, then the temperature is raised to 1250 to 1260℃ at a rate of 2℃ / min and held for 2h, and then cooled to room temperature with the furnace.

[0011] The beneficial effects of this invention are as follows: the porcelain insulator prepared by the method described in this invention has good corrosion resistance and high high-humidity withstand voltage, improving the durability and safety of the insulator and reducing maintenance and replacement costs. By adding yttrium doping and fluorinated loaded particles to the porcelain insulator described in this invention, the corrosion resistance and power frequency humidity withstand voltage of the porcelain insulator can be significantly improved. This may be because: firstly, this invention prepares yttrium-doped aluminum-titanium composite oxide particles, utilizing the high corrosion resistance of the aluminum-titanium composite oxide to improve the overall corrosion resistance of the porcelain insulator. Simultaneously, through yttrium doping, yttrium ions occupy cation sites in the crystal lattice to form a new phase with good chemical stability, stabilizing the crystal structure through a charge compensation mechanism, thereby improving the overall corrosion resistance and power frequency humidity withstand voltage of the material. Secondly, by coating zirconium oxide and simultaneously fluorinating to replace some oxygen, the density of the porcelain insulator is improved; since fluorination also reduces the wettability of the material surface to water, it improves the high-humidity withstand voltage. Furthermore, due to the large number of micropores and blind pores on the surface and inside the oxide particles, solutions are difficult to completely penetrate under normal pressure. The negative pressure environment draws out the gas from these pores, creating negative pressure, which then forces the solution deep into the pores, achieving deep impregnation. Detailed Implementation

[0012] The present invention will be further described below with reference to the embodiments.

[0013] Example 1

[0014] A method for preparing a corrosion-resistant, high-humidity, voltage-resistant porcelain insulator, comprising the following steps: (1) Prepare an ethanol solution of tetrabutyl titanate; the ethanol solution of tetrabutyl titanate contains 20% tetrabutyl titanate by mass and ethanol as the solvent; glacial acetic acid, deionized water, propylene glycol and ethanol are mixed in a reaction vessel to form a mixture; the mixing ratio of glacial acetic acid, deionized water, propylene glycol and ethanol is glacial acetic acid:deionized water:propylene glycol:ethanol = 10mL:5mL:1mL:20mL; aluminum nitrate nonahydrate and yttrium nitrate hexahydrate are added to the mixture, and after the addition is completed, the mixture is stirred for 30 minutes to mix evenly, and then the ethanol solution of tetrabutyl titanate is added while stirring. The mixture was then added to an ethanol solution of aluminum nitrate nonahydrate, yttrium nitrate hexahydrate, and n-butyl titanate in a ratio of 50 mL: 8 g: 1 g: 50 mL. After the addition was complete, the mixture was heated to 50°C in a water bath and kept at that temperature. Ammonia (25% by mass of solute) was added to adjust the pH to 10. The mixture was then stirred at 50°C for 10 hours, followed by solid-liquid separation. The solid phase was washed three times with ethanol and then three times with deionized water. It was dried at 100°C for 2 hours and then calcined at 400°C for 2 hours to obtain composite oxide particles. (2) Dissolve zirconium nitrate fully in deionized water to prepare a coating solution; the ratio of zirconium nitrate to deionized water is 20g:200mL; add the composite oxide particles to an anhydrous ethanol solution of hydroxypropyl cellulose, the ratio of composite oxide particles to anhydrous ethanol solution of hydroxypropyl cellulose is 5g:150mL, the mass percentage of hydroxypropyl cellulose in the anhydrous ethanol solution is 1%, and the solvent is ethanol; stir for 30 minutes under ultrasonic conditions to form a suspension, and then add the coating solution (prepared fresh) to the suspension while stirring. The coating solution has a volume ratio of suspension to coating solution of 10 mL to 3 mL. After addition, the mixture is held at 0.01 atm for 20 min, then removed and heated in a water bath to 60°C for 2 h. Solid-liquid separation is performed, and the solid phase is dried at 30°C for 3 h. The dried solid phase is then immersed in an ammonium fluoride solution with an ammonium fluoride concentration of 0.5 g / 100 mL and water as the solvent. The volume ratio of the dried solid phase to ammonium fluoride solution is 1 g to 20 mL. The mixture is held at 0.01 atm for 20 min. After holding, solid-liquid separation is performed, and the solid phase is dried at 100°C for 2 h and calcined at 450°C for 1 h to obtain loaded particles. (3) Weigh each raw material component, and each component is as follows by weight: 50 parts kaolin, 20 parts loaded particles, 5 parts potassium feldspar, 3 parts sodium feldspar, 15 parts quartz powder, and 1 part calcium oxide powder; wherein the kaolin, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder are all sieved powders that have passed through a 300-mesh sieve; mix the kaolin, the loaded particles, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder evenly to form a mixture, add water to the mixture to adjust it into a mud with a water content of 7wt%, mix evenly, pour into a mold for die casting (30MPa, holding pressure for 5min), air dry at room temperature for 5h, demold, and fire. The calcination process is as follows: first heat up to 600℃ at a rate of 3℃ / min, hold for 30min, then heat up to 1250℃ at a rate of 2℃ / min, hold for 2h, and then cool to room temperature with the furnace; obtain the corrosion-resistant, high-humidity, voltage-resistant porcelain insulator.

[0015] Example 2

[0016] A method for preparing a corrosion-resistant, high-humidity, voltage-resistant porcelain insulator, comprising the following steps: (1) Prepare an ethanol solution of tetrabutyl titanate; the ethanol solution of tetrabutyl titanate contains 20% tetrabutyl titanate by mass and ethanol as the solvent; glacial acetic acid, deionized water, propylene glycol and ethanol are mixed in a reaction vessel to form a mixture; the mixing ratio of glacial acetic acid, deionized water, propylene glycol and ethanol is glacial acetic acid:deionized water:propylene glycol:ethanol = 10mL:6mL:2mL:20mL; aluminum nitrate nonahydrate and yttrium nitrate hexahydrate are added to the mixture, and after the addition is completed, the mixture is stirred for 30 minutes to mix evenly, and then the ethanol solution of tetrabutyl titanate is added while stirring. The mixture was then added to an ethanol solution of aluminum nitrate nonahydrate, yttrium nitrate hexahydrate, and n-butyl titanate in a ratio of 50 mL: 9 g: 3 g: 55 mL. After the addition was complete, the mixture was heated to 50°C in a water bath and kept at that temperature. Ammonia (25% by mass of solute) was added to adjust the pH to 10. The mixture was then stirred at 50°C for 10 hours, followed by solid-liquid separation. The solid phase was washed three times with ethanol and then three times with deionized water. It was dried at 100°C for 2 hours and then calcined at 400°C for 2 hours to obtain composite oxide particles. (2) Dissolve zirconium nitrate fully in deionized water to prepare a coating solution; the ratio of zirconium nitrate to deionized water is 20g:200mL; add the composite oxide particles to an anhydrous ethanol solution of hydroxypropyl cellulose, the ratio of composite oxide particles to anhydrous ethanol solution of hydroxypropyl cellulose is 5g:150mL, the mass percentage of hydroxypropyl cellulose in the anhydrous ethanol solution is 1%, and the solvent is ethanol; stir for 30 minutes under ultrasonic conditions to form a suspension, and then add the coating solution (prepared fresh) to the suspension while stirring. The coating solution has a volume ratio of suspension to coating solution of 10 mL to 4 mL. After addition, the mixture is held at 0.01 atm for 20 min, then removed and aged in a water bath at 60°C for 2 h. Solid-liquid separation is performed, and the solid phase is dried at 30°C for 3 h. The dried solid phase is then immersed in an ammonium fluoride solution with an ammonium fluoride concentration of 0.5 g / 100 mL and water as the solvent. The volume ratio of the dried solid phase to ammonium fluoride solution is 1 g to 20 mL. The mixture is held at 0.01 atm for 20 min. After the pressure holding is completed, solid-liquid separation is performed, and the solid phase is dried at 100°C for 2 h and calcined at 460°C for 1 h to obtain loaded particles. (3) Weigh each raw material component, and each component is as follows by weight: 50 parts kaolin, 25 parts loaded particles, 5 parts potassium feldspar, 5 parts sodium feldspar, 15 parts quartz powder, and 1 part calcium oxide powder; wherein the kaolin, potassium feldspar, sodium feldspar, quartz powder, and calcium oxide powder are all sieved powders that have passed through a 300-mesh sieve; mix the kaolin, the loaded particles, potassium feldspar, sodium feldspar, quartz powder, and calcium oxide powder evenly to form a mixture, add water to the mixture to adjust it into a mud with a water content of 7wt%, mix evenly, pour into a mold for die casting (30MPa, holding pressure for 5min), air dry at room temperature for 5h, demold, and fire. The calcination process is as follows: first heat up to 600℃ at a rate of 3℃ / min, hold for 30min, then heat up to 1250℃ at a rate of 2℃ / min, hold for 2h, and then cool to room temperature with the furnace; obtain the corrosion-resistant, high-humidity, voltage-resistant porcelain insulator.

[0017] Example 3

[0018] A method for preparing a corrosion-resistant, high-humidity, voltage-resistant porcelain insulator, comprising the following steps: (1) Prepare an ethanol solution of tetrabutyl titanate; the ethanol solution of tetrabutyl titanate contains 30% tetrabutyl titanate by mass and ethanol as the solvent; glacial acetic acid, deionized water, propylene glycol and ethanol are mixed in a reaction vessel to form a mixture; the mixing ratio of glacial acetic acid, deionized water, propylene glycol and ethanol is glacial acetic acid:deionized water:propylene glycol:ethanol = 10mL:7mL:2mL:25mL; aluminum nitrate nonahydrate and yttrium nitrate hexahydrate are added to the mixture, and after the addition is completed, the mixture is stirred for 30 minutes to mix evenly, and then the ethanol solution of tetrabutyl titanate is added while stirring. The mixture was then added to an ethanol solution of aluminum nitrate nonahydrate, yttrium nitrate hexahydrate, and n-butyl titanate in a ratio of 50 mL: 9 g: 3 g: 55 mL. After the addition was complete, the mixture was heated to 50°C in a water bath and kept at that temperature. Ammonia (25% by mass of solute) was added to adjust the pH to 10. The mixture was then stirred at 50°C for 10 hours, followed by solid-liquid separation. The solid phase was washed three times with ethanol and then three times with deionized water. It was dried at 100°C for 2 hours and then calcined at 450°C for 2 hours to obtain composite oxide particles. (2) Dissolve zirconium nitrate fully in deionized water to prepare a coating solution; the ratio of zirconium nitrate to deionized water is 25g:200mL; add the composite oxide particles to an anhydrous ethanol solution of hydroxypropyl cellulose, the ratio of composite oxide particles to anhydrous ethanol solution of hydroxypropyl cellulose is 5g:150mL, wherein the mass percentage of hydroxypropyl cellulose in the anhydrous ethanol solution is 2%, and the solvent is ethanol; stir for 30 minutes under ultrasonic conditions to form a suspension, and then add the coating solution (prepared fresh) to the suspension while stirring. The ratio of the added suspension to the coating solution is 10 mL: 4 mL. After the addition is complete, the mixture is held at 0.01 atm for 20 min, then removed and heated in a water bath to 60°C for 2 h. Solid-liquid separation is performed, and the solid phase is dried at 30°C for 3 h. The dried solid phase is then immersed in an ammonium fluoride solution with an ammonium fluoride concentration of 1 g / 100 mL and water as the solvent. The ratio of the dried solid phase to the ammonium fluoride solution is 1 g: 20 mL. The mixture is held at 0.01 atm for 20 min. After the pressure holding is completed, solid-liquid separation is performed, and the solid phase is dried at 100°C for 2 h and then calcined at 470°C for 1 h to obtain the loaded particles. (3) Weigh each raw material component, and each component is as follows by weight: 50 parts kaolin, 25 parts loaded particles, 10 parts potassium feldspar, 5 parts sodium feldspar, 20 parts quartz powder, and 2 parts calcium oxide powder; wherein the kaolin, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder are all sieved powders that have passed through a 300-mesh sieve; mix the kaolin, the loaded particles, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder evenly to form a mixture, add water to the mixture to adjust it into a mud with a water content of 7wt%, mix evenly, pour into a mold for die casting (30MPa, holding pressure for 5min), air dry at room temperature for 5h, demold, and fire. The calcination process is as follows: first heat up to 600℃ at a rate of 3℃ / min, hold for 30min, then heat up to 1260℃ at a rate of 2℃ / min, hold for 2h, and then cool to room temperature with the furnace; obtain the corrosion-resistant, high-humidity, voltage-resistant porcelain insulator.

[0019] Example 4

[0020] A method for preparing a corrosion-resistant, high-humidity, voltage-resistant porcelain insulator, comprising the following steps: (1) Prepare an ethanol solution of tetrabutyl titanate; the ethanol solution of tetrabutyl titanate contains 30% tetrabutyl titanate by mass and ethanol as the solvent; glacial acetic acid, deionized water, propylene glycol and ethanol are mixed in a reaction vessel to form a mixture; the mixing ratio of glacial acetic acid, deionized water, propylene glycol and ethanol is glacial acetic acid:deionized water:propylene glycol:ethanol = 10mL:8mL:3mL:25mL; aluminum nitrate nonahydrate and yttrium nitrate hexahydrate are added to the mixture, and after the addition is completed, the mixture is stirred for 30 minutes to mix evenly, and then the ethanol solution of tetrabutyl titanate is added while stirring. The mixture was then added to an ethanol solution of aluminum nitrate nonahydrate, yttrium nitrate hexahydrate, and n-butyl titanate in a ratio of 50 mL: 10 g: 5 g: 60 mL. After the addition was complete, the mixture was heated to 50°C in a water bath and kept at that temperature. Ammonia (25% by mass of solute) was added to adjust the pH to 10. The mixture was then stirred at 50°C for 10 hours. The solid and liquid phases were separated. The solid phase was washed three times with ethanol and then three times with deionized water. The solid phase was dried at 100°C for 2 hours and then calcined at 450°C for 2 hours to obtain composite oxide particles. (2) Dissolve zirconium nitrate fully in deionized water to prepare a coating solution; the ratio of zirconium nitrate to deionized water is 25g:200mL; add the composite oxide particles to an anhydrous ethanol solution of hydroxypropyl cellulose, the ratio of composite oxide particles to anhydrous ethanol solution of hydroxypropyl cellulose is 5g:150mL, wherein the mass percentage of hydroxypropyl cellulose in the anhydrous ethanol solution is 2%, and the solvent is ethanol; stir for 30 minutes under ultrasonic conditions to form a suspension, and then add the coating solution (prepared fresh) to the suspension while stirring. The ratio of suspension to coating solution added is 10 mL: 5 mL. After addition, the mixture is held at 0.01 atm for 20 min, then removed and aged in a water bath at 60°C for 2 h. Solid-liquid separation is performed, and the solid phase is dried at 30°C for 3 h. The dried solid phase is then immersed in an ammonium fluoride solution with an ammonium fluoride concentration of 1 g / 100 mL and water as the solvent. The ratio of dried solid phase to ammonium fluoride solution is 1 g: 20 mL. The mixture is held at 0.01 atm for 20 min. After the pressure holding period, solid-liquid separation is performed, and the solid phase is dried at 100°C for 2 h and calcined at 480°C for 1 h to obtain loaded particles. (3) Weigh each raw material component, and each component is as follows by weight: 50 parts kaolin, 30 parts loaded particles, 10 parts potassium feldspar, 6 parts sodium feldspar, 20 parts quartz powder, and 2 parts calcium oxide powder; wherein the kaolin, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder are all sieved powders that have passed through a 300-mesh sieve; mix the kaolin, the loaded particles, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder evenly to form a mixture, add water to the mixture to adjust it into a mud with a water content of 7wt%, mix evenly, pour into a mold for die casting (30MPa, holding pressure for 5min), air dry at room temperature for 5h, demold, and fire. The calcination process is as follows: first heat up to 600℃ at a rate of 3℃ / min, hold for 30min, then heat up to 1260℃ at a rate of 2℃ / min, hold for 2h, and then cool to room temperature with the furnace; obtain the corrosion-resistant, high-humidity, voltage-resistant porcelain insulator.

[0021] Comparative Example 1 A comparative method for preparing a porcelain insulator includes the following steps: (1) Prepare an ethanol solution of tetrabutyl titanate; the ethanol solution of tetrabutyl titanate contains 20% tetrabutyl titanate by mass and ethanol as the solvent; glacial acetic acid, deionized water, propylene glycol and ethanol are mixed in a reaction vessel to form a mixture; the mixing ratio of glacial acetic acid, deionized water, propylene glycol and ethanol is glacial acetic acid:deionized water:propylene glycol:ethanol = 10mL:6mL:2mL:20mL; aluminum nitrate nonahydrate is added to the mixture, and after the addition is completed, the mixture is stirred for 30 minutes to mix evenly, and then the tetrabutyl titanate is added while stirring. An ethanol solution was prepared, and aluminum nitrate nonahydrate and ethanol solution of titanate n-butyl ester were added to the mixture in a ratio of ethanol solution of mixture: aluminum nitrate nonahydrate: ethanol solution of titanate n-butyl ester = 50 mL: 9 g: 55 mL. After the addition was completed, the mixture was heated to 50°C in a water bath and kept at that temperature. Ammonia water (mass percentage of solute was 25%) was added to adjust the pH to 10. Then, the mixture was stirred at 50°C for 10 h, and the solid and liquid phases were separated. The solid phase was washed three times with ethanol and then three times with deionized water. It was dried at 100°C for 2 h and then calcined at 400°C for 2 h to obtain composite oxide particles. (2) Dissolve zirconium nitrate fully in deionized water to prepare a coating solution; the ratio of zirconium nitrate to deionized water is 20g:200mL; add the composite oxide particles to an anhydrous ethanol solution of hydroxypropyl cellulose, the ratio of composite oxide particles to anhydrous ethanol solution of hydroxypropyl cellulose is 5g:150mL, the mass percentage of hydroxypropyl cellulose in the anhydrous ethanol solution is 1%, and the solvent is ethanol; stir for 30 minutes under ultrasonic conditions to form a suspension, and then add the coating solution (prepared fresh) to the suspension while stirring. The coating solution has a volume ratio of suspension to coating solution of 10 mL to 4 mL. After addition, the mixture is held at 0.01 atm for 20 min, then removed and aged in a water bath at 60°C for 2 h. Solid-liquid separation is performed, and the solid phase is dried at 30°C for 3 h. The dried solid phase is then immersed in an ammonium fluoride solution with an ammonium fluoride concentration of 0.5 g / 100 mL and water as the solvent. The volume ratio of the dried solid phase to ammonium fluoride solution is 1 g to 20 mL. The mixture is held at 0.01 atm for 20 min. After the pressure holding is completed, solid-liquid separation is performed, and the solid phase is dried at 100°C for 2 h and calcined at 460°C for 1 h to obtain loaded particles. (3) Weigh each raw material component, and each component is as follows by weight: 50 parts kaolin, 25 parts loaded particles, 5 parts potassium feldspar, 5 parts sodium feldspar, 15 parts quartz powder, and 1 part calcium oxide powder; wherein the kaolin, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder are all sieved powders that have passed through a 300-mesh sieve; mix the kaolin, the loaded particles, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder evenly to form a mixture, add water to the mixture to adjust it into a mud with a water content of 7wt%, mix evenly, pour into a mold for die casting (30MPa, holding pressure for 5min), air dry at room temperature for 5h, demold, and fire. The calcination process is as follows: first heat up to 600℃ at a rate of 3℃ / min, hold for 30min, then heat up to 1250℃ at a rate of 2℃ / min, hold for 2h, and then cool to room temperature with the furnace; obtain the porcelain insulator described in this comparative example.

[0022] Comparative Example 2 A comparative method for preparing a porcelain insulator includes the following steps: (1) Prepare an ethanol solution of tetrabutyl titanate; the ethanol solution of tetrabutyl titanate contains 20% tetrabutyl titanate by mass and ethanol as the solvent; glacial acetic acid, deionized water, propylene glycol and ethanol are mixed in a reaction vessel to form a mixture; the mixing ratio of glacial acetic acid, deionized water, propylene glycol and ethanol is glacial acetic acid:deionized water:propylene glycol:ethanol = 10mL:6mL:2mL:20mL; aluminum nitrate nonahydrate and yttrium nitrate hexahydrate are added to the mixture, and after the addition is completed, the mixture is stirred for 30 minutes to mix evenly, and then the ethanol solution of tetrabutyl titanate is added while stirring. The mixture was then added to an ethanol solution of aluminum nitrate nonahydrate, yttrium nitrate hexahydrate, and n-butyl titanate in a ratio of 50 mL: 9 g: 3 g: 55 mL. After the addition was complete, the mixture was heated to 50°C in a water bath and kept at that temperature. Ammonia (25% by mass of solute) was added to adjust the pH to 10. The mixture was then stirred at 50°C for 10 hours, followed by solid-liquid separation. The solid phase was washed three times with ethanol and then three times with deionized water. It was dried at 100°C for 2 hours and then calcined at 400°C for 2 hours to obtain composite oxide particles. (2) Dissolve zirconium nitrate fully in deionized water to prepare a coating solution; the ratio of zirconium nitrate to deionized water is 20g:200mL; add the composite oxide particles to an anhydrous ethanol solution of hydroxypropyl cellulose, the ratio of composite oxide particles to anhydrous ethanol solution of hydroxypropyl cellulose is 5g:150mL, and the mass percentage of hydroxypropyl cellulose in the anhydrous ethanol solution is... The fraction was 1%, and the solvent was ethanol. The mixture was stirred for 30 minutes under ultrasonic conditions to form a suspension. Then, the coating solution (prepared and used immediately) was added to the suspension while stirring. The ratio of the amount of coating solution added to the suspension was 10 mL: 4 mL. After the addition was completed, the mixture was placed under 0.01 standard atmospheres for 20 minutes. Then, it was taken out and heated to 60°C in a water bath for 2 hours. The solid and liquid phases were separated, the solid phase was dried at 30°C for 3 hours, and then calcined at 460°C for 1 hour to obtain the loaded particles. (3) Weigh each raw material component, and each component is as follows by weight: 50 parts kaolin, 25 parts loaded particles, 5 parts potassium feldspar, 5 parts sodium feldspar, 15 parts quartz powder, and 1 part calcium oxide powder; wherein the kaolin, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder are all sieved powders that have passed through a 300-mesh sieve; mix the kaolin, the loaded particles, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder evenly to form a mixture, add water to the mixture to adjust it into a mud with a water content of 7wt%, mix evenly, pour into a mold for die casting (30MPa, holding pressure for 5min), air dry at room temperature for 5h, demold, and fire. The calcination process is as follows: first heat up to 600℃ at a rate of 3℃ / min, hold for 30min, then heat up to 1250℃ at a rate of 2℃ / min, hold for 2h, and then cool to room temperature with the furnace; obtain the porcelain insulator described in this comparative example.

[0023] Example 5

[0024] Corrosion resistance test: Prepare a 3.5 wt% sodium chloride aqueous solution as the corrosive medium. Weigh the initial mass of the porcelain insulator to be tested obtained by the method described in the above examples and comparative examples, and then immerse it in the corrosive medium. The entire porcelain insulator should be completely submerged. Immerse at room temperature for 21 days. After immersion, clean it with ultrasonic cleaning, dry it, weigh the mass after corrosion, and calculate the mass loss of each porcelain insulator before and after corrosion.

[0025] Power frequency humidity withstand voltage test: The test environment was set as follows: ambient temperature 26℃, absolute humidity 17.2 g / m³. 3The arc distance was 0.29m, the simulated rainwater temperature was 22℃, and the measured resistivity of the simulated rainwater was 99.1Ω·m. The simulated rainfall was 1.3mm / min for both the horizontal and vertical components. The voltage correction coefficient was 0.99, the test voltage was 70.5kV, and the test time was 60s. The tolerance was observed, and the results are shown in Table 1.

[0026] Table 1

[0027] As shown in Table 1, the porcelain insulator prepared by the method described in this invention exhibits good corrosion resistance and high high-humidity withstand voltage, improving the durability and safety of the insulator and reducing maintenance and replacement costs. Comparing Example 2 and the comparative examples, it is evident that adding yttrium doping and fluorinated loaded particles to the porcelain insulator described in this invention significantly improves its corrosion resistance and power frequency humidity withstand performance. This may be because: this invention first prepares yttrium-doped aluminum-titanium composite oxide particles, utilizing the high corrosion resistance of the aluminum-titanium composite oxide to improve the overall corrosion resistance of the porcelain insulator. Simultaneously, yttrium doping utilizes yttrium ions occupying cation sites in the crystal lattice to form a new phase with good chemical stability, stabilizing the crystal structure through a charge compensation mechanism, thereby improving the overall corrosion resistance and power frequency humidity withstand performance of the material. Secondly, coating with zirconium oxide and simultaneously fluorinating to replace some oxygen improves the density of the porcelain insulator; since fluorination also reduces the wettability of the material surface to water, it further improves high-humidity withstand performance. Furthermore, due to the numerous micropores and blind pores on and inside the oxide particles, the solution cannot completely penetrate under normal pressure. A negative pressure environment draws out the gas from these pores, creating negative pressure, which then forces the solution deep into the pores, achieving deep impregnation.

[0028] The technical solutions provided by the present invention have been described in detail above. For those skilled in the art, there will be changes in specific implementation methods and application scope based on the ideas of the embodiments of the present invention. Therefore, the content of this specification should not be construed as a limitation of the present invention.

Claims

1. A method for preparing a corrosion-resistant, high-humidity, voltage-resistant porcelain insulator, characterized in that the steps include... include: (1) Prepare an ethanol solution of tetrabutyl titanate; mix glacial acetic acid, deionized water, propylene glycol and ethanol in a reaction vessel to form a mixture; add aluminum nitrate nonahydrate and yttrium nitrate hexahydrate to the mixture, stir and mix after the addition is complete, then add the ethanol solution of tetrabutyl titanate while stirring, heat and keep warm in a water bath after the addition is complete, add ammonia water, then keep warm and stir, separate solid and liquid, wash the solid phase, dry, calcine to obtain composite oxide particles; (2) Dissolve zirconium nitrate in deionized water to prepare a coating solution; add the composite oxide particles to an anhydrous ethanol solution of hydroxypropyl cellulose, stir under ultrasonic conditions to form a suspension, and then add the coating solution to the suspension under stirring. After the addition is completed, place the mixture under negative pressure and keep it under pressure, then heat it in a water bath for aging, separate the solid and liquid, dry the solid phase, soak the dried solid phase in ammonium fluoride solution, keep it under negative pressure, separate the solid and liquid after the pressure is kept, dry the solid phase, and calcine to obtain the loaded particles. (3) Mix kaolin, the loaded particles, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder evenly to form a mixture, add water to the mixture, mix well, pour into a mold for die casting, dry, demold, and fire to obtain the corrosion-resistant, high-humidity, voltage-resistant porcelain insulator.

2. The method for preparing a corrosion-resistant, high-humidity, voltage-resistant porcelain insulator according to claim 1, characterized in that, In step (1), the mass percentage of the ethanol solution of tetrabutyl titanate is 20%–30%, and the solvent is ethanol; the mixing ratio of glacial acetic acid, deionized water, propylene glycol, and ethanol is glacial acetic acid:deionized water:propylene glycol:ethanol = 10 mL: 5–8 mL: 1–3 mL: 20–25 mL; the ratio of aluminum nitrate nonahydrate, yttrium nitrate hexahydrate, and ethanol solution of tetrabutyl titanate added to the mixture is mixture: aluminum nitrate nonahydrate: yttrium nitrate hexahydrate: ethanol solution of tetrabutyl titanate = 50 mL: 8–10 g: 1–5 g: 50–60 mL.

3. The method for preparing a corrosion-resistant, high-humidity, voltage-resistant porcelain insulator according to claim 1, characterized in that, In step (1), the water bath is heated to 50±5℃ and kept warm, and ammonia is added to adjust the pH to 10; then it is kept warm and stirred for more than 10 hours. The calcination temperature is 400~450℃ and the calcination time is 2~3 hours.

4. The method for preparing a corrosion-resistant, high-humidity, voltage-resistant porcelain insulator according to claim 1, characterized in that, In step (2), the ratio of zirconium nitrate added to deionized water is zirconium nitrate:deionized water = 20-25g:200mL; the ratio of the composite oxide particles added to the anhydrous ethanol solution of hydroxypropyl cellulose is composite oxide particles:anhydrous ethanol solution of hydroxypropyl cellulose = 5g:150-200mL, wherein the mass percentage of hydroxypropyl cellulose in the anhydrous ethanol solution of hydroxypropyl cellulose is 1%-2%, and the solvent is ethanol; the ratio of the coating solution added to the suspension is suspension:coating solution = 10mL:3-5mL, and the suspension is heated in a water bath to 60±5℃ and aged for 2-4 hours.

5. The method for preparing a corrosion-resistant, high-humidity, voltage-resistant porcelain insulator according to claim 1, characterized in that, In step (2), the concentration of ammonium fluoride in the ammonium fluoride solution is 0.5-1g / 100mL, and the solvent is water; the ratio of the dried solid phase to the ammonium fluoride solution is 1g: 20-50mL, the calcination temperature is 450-480℃, and the calcination time is 1-2h.

6. The method for preparing a corrosion-resistant, high-humidity, voltage-resistant porcelain insulator according to claim 1, characterized in that, In step (3), the components are as follows by weight: 50 parts kaolin, 20-30 parts loaded particles, 5-10 parts potassium feldspar, 3-6 parts sodium feldspar, 15-20 parts quartz powder, and 1-2 parts calcium oxide powder; wherein the kaolin, potassium feldspar, sodium feldspar, quartz powder and calcium oxide powder are all sieved powders that have passed through a 300-mesh sieve.

7. The method for preparing a corrosion-resistant, high-humidity, voltage-resistant porcelain insulator according to claim 1, characterized in that, In step (3), water is added to the mixture to prepare mud with a water content of 6wt% to 7wt%. The calcination process is as follows: first, the temperature is raised to 600℃ at a rate of 3℃ / min and held for 30min, then the temperature is raised to 1250 to 1260℃ at a rate of 2℃ / min and held for 2h, and then cooled to room temperature with the furnace.