A moisture-proof and anti-pulverizing granular fertilizer and its preparation method
By adopting a three-layer structure design from the inside out in granular fertilizer, including a fertilizer core, a bonding transition layer, and a coating layer, the problems of moisture resistance and anti-pulverization of granular compound fertilizers are solved, thereby improving cost-effectiveness and process adaptability, making it suitable for large-scale application in field crops.
Patent Information
- Application Number
- CN202611151016.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing granular compound fertilizers have poor moisture resistance, are prone to clumping, and lack sufficient resistance to pulverization. Furthermore, high-performance coating solutions are costly and the processes are difficult to adapt to conventional production lines.
It adopts a three-layer structure design from the inside out, including fertilizer core particles, bonding transition layer and coating layer. The bonding transition layer is formed by pregelatinized starch and bentonite, and the coating layer is composed of paraffin, stearic acid and other materials. Production is achieved through conventional equipment.
It significantly improves the moisture resistance and anti-dustling ability of the granules, reduces production costs, is suitable for large-scale application of fertilizer for field crops, and does not increase equipment investment.
Smart Images

Figure CN123106344A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of fertilizer processing technology, and in particular to a moisture-proof and anti-pulverization granular fertilizer and its preparation method. Background Technology
[0002] With the continuous advancement of soil testing and formula fertilization and agricultural mechanization in my country, granular compound fertilizers have become the mainstream formulation for base fertilizer and top dressing of grain and cash crops. The granular strength, moisture resistance, and storage durability of granular fertilizers directly determine storage and transportation losses and the smoothness of mechanized fertilization, and are core quality indicators of fertilizer products.
[0003] Inorganic granular compound fertilizers prepared by conventional rotary drum agglomeration method use urea, ammonium salts, phosphates, and potassium salts as basic raw materials. They are formed by steam wetting and agglomeration. The internal bonding of the granules is mainly based on crystal bridges and van der Waals forces, which has two prominent defects: First, poor moisture resistance. The components in the raw materials, such as urea, ammonium chloride, and potassium chloride, have strong hygroscopicity. After absorbing moisture, the surface of the granules dissolves and recrystallizes, which easily forms clumps between granules, seriously affecting unpacking and mechanical application. Second, insufficient resistance to pulverization. The surface bonding force of conventionally agglomerated granules is weak. After friction and collision during loading, unloading, and transportation, the surface layer peels off and the granules break. It is also easy to clog the feed port of the fertilizer applicator and reduce the efficiency of fertilizer application.
[0004] To address the aforementioned issues, the industry primarily employs two technical approaches for improvement: The first approach involves adding inorganic binders such as clay, gypsum, and water glass during the granulation process to enhance the internal bonding strength of the particles. This solution is simple and low-cost, but it only slightly improves particle strength and has limited effectiveness in blocking moisture, failing to fundamentally solve the problem of moisture absorption and clumping. Furthermore, adding more than 5% binder significantly dilutes the fertilizer nutrient concentration, reducing the fertilizer efficiency per unit product. The second type uses coating technology to form a barrier layer on the surface of the granules. Public data on commercially available polymer-coated fertilizers show that their moisture absorption rate can be reduced to below 1%, with excellent moisture-proof effect. However, there are obvious limitations: First, the price of polymer resin raw materials is 5 to 10 times that of ordinary mineral raw materials, and the overall cost of fertilizer increases by 30% to 50% after coating, making it difficult to promote on a large scale in field crop fertilizers. Second, this type of coating process often requires the matching of fluidized bed coating equipment and organic solvent recovery system. The equipment investment is 8 to 10 times that of conventional rotary coating equipment, which cannot be directly adapted to existing compound fertilizer production lines. Third, long-term application of some non-degradable polymer materials poses a risk of microplastic residues in the soil, which is not environmentally friendly enough.
[0005] Therefore, developing a granular fertilizer based on bulk conventional raw materials, compatible with existing compound fertilizer production equipment, with low production costs, and possessing excellent moisture-proof and anti-pulverization properties, as well as its preparation method, is a technical problem that urgently needs to be solved in the industry. Summary of the Invention
[0006] To address the problems of insufficient moisture-proof and anti-powdering capabilities of existing granular fertilizers, high raw material costs for high-performance coating solutions, and difficulties in adapting processes to conventional production lines, this invention provides a moisture-proof and anti-powdering granular fertilizer and its preparation method. It uses industry-standard bulk raw materials and relies on conventional fertilizer production equipment to achieve production, thereby improving the moisture-proof and anti-powdering performance of granular fertilizers while controlling costs.
[0007] To solve the above-mentioned technical problems, the present invention provides the following technical solution:
[0008] On one hand, this invention provides a moisture-proof and anti-powdering granular fertilizer, comprising, from the inside out, fertilizer core particles, a bonding transition layer, and a coating layer. Based on 100 parts by weight of the dry basis total mass of the fertilizer core particles, the fertilizer core particles contain 20-45 parts by weight of a nitrogen source, 10-30 parts by weight of a phosphorus source, and 15-35 parts by weight of a potassium source. The bonding transition layer, comprising 1.5%-4% of the dry basis total mass of the fertilizer core particles, is composed of a mixture of pregelatinized starch and bentonite, and is used to enhance the bonding strength between the coating layer and the core surface. The coating layer, comprising 3%-8% of the total mass of the granular fertilizer; based on 100 parts by weight of the dry basis total mass of the coating layer, the coating layer contains 15-30 parts by weight of paraffin wax, 5-12 parts by weight of stearic acid, 20-40 parts by weight of mineral filler, and 3-8 parts by weight of sodium carboxymethyl cellulose, constituting the main moisture barrier structure.
[0009] As a preferred embodiment of the present invention, the nitrogen source is one or more of urea, ammonium sulfate, and ammonium chloride; the phosphorus source is agricultural grade monoammonium phosphate or superphosphate; and the potassium source is agricultural grade potassium chloride or potassium sulfate.
[0010] As a preferred embodiment of the present invention, the fertilizer core particles are further provided with trace element additives, the amount of which is 2% to 8% of the total dry weight of the fertilizer core particles; the trace element additives are a combination of two or more of magnesium sulfate, zinc sulfate and borax.
[0011] In a preferred embodiment of the present invention, the mass ratio of pregelatinized starch to bentonite in the bonding transition layer is 2 to 3:1; the pregelatinized starch is corn pregelatinized starch, and the bentonite is sodium-based bentonite.
[0012] As a preferred embodiment of the present invention, the paraffin in the coating layer is No. 58 fully refined paraffin; the stearic acid is industrial grade stearic acid; the mineral filler is one or both of heavy calcium carbonate and talc, and the filler fineness is 800-1200 mesh; the sodium carboxymethyl cellulose is an industrial grade medium viscosity product.
[0013] As a preferred embodiment of the present invention, the particle size of the fertilizer core particles is 2.0 to 4.0 mm; the thickness of the bonding transition layer is 10 to 30 μm; and the thickness of the coating layer is 30 to 80 μm.
[0014] This invention also provides a method for preparing the above-mentioned moisture-proof and anti-powdering granular fertilizer, including raw material mixing, granulation, and sieving steps, as well as adhesive layer spraying, melt coating, and drying and cooling steps, specifically carried out according to the following steps: S1 Core granulation: Nitrogen source, phosphorus source, and potassium source are mixed evenly according to the ratio and fed into a rotary drum granulator. Saturated steam is introduced to agglomerate and granulate. The product is preliminarily dried and then sieved to obtain fertilizer core granules; S2 Adhesive layer spraying: Fertilizer core granules are fed into a rotary coating machine, and an adhesive suspension is sprayed by atomization. After rotation, an adhesive transition layer is formed; S3 Melt coating: Pre-molten coating material is added to the rotary coating machine, and the temperature inside the machine is maintained so that the coating material coats the surface of the adhesive transition layer; S4 Drying and cooling: The coated granules are dried, air-cooled to room temperature, and sieved to obtain the finished granular fertilizer.
[0015] As a preferred embodiment of the present invention, in step S1, the saturated steam pressure is 0.2-0.35 MPa, the granulation temperature is 55-70°C, and the granulation time is 8-15 min; the preliminary drying temperature is 60-70°C, and the moisture content of the core particles after drying is 2%-4%; the particle size of the core particles after sieving is 2.0-4.0 mm.
[0016] As a preferred technical solution of the present invention, in step S2, the binder suspension is an aqueous suspension of pregelatinized starch and bentonite with a mass concentration of 8% to 12%, and the material temperature is maintained at 40 to 55°C during spraying.
[0017] As a preferred technical solution of the present invention, in step S3, the coating material is preheated to 70-90°C until it is completely melted, the temperature inside the machine is maintained at 50-65°C during the coating process, and the coating time is 5-10 minutes.
[0018] As a preferred technical solution of the present invention, in step S4, the drying temperature is 60-80℃, the moisture content of the finished product granules after drying is ≤1.5% by mass; the material temperature after cooling is ≤30℃; and the finished product is screened to obtain granular fertilizer with a particle size of 2.0-4.0mm.
[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. The double-layer coating structure of the bonding transition layer and the coating layer can block external moisture from penetrating into the granules, reducing the probability of granules absorbing moisture and clumping; at the same time, it can improve the bonding strength between the coating layer and the fertilizer core, reducing the phenomenon of coating peeling off and granule pulverization during storage and transportation. 2. All raw materials are conventional bulk materials in the agricultural and chemical industries, requiring no special customized materials. The raw material procurement channels are extensive, and the production cost is controllable, making it suitable for large-scale application of fertilizer for field crops. 3. The preparation process can be achieved using conventional fertilizer production equipment such as rotary drum granulators and rotary coating machines, without the need for additional dedicated production lines. The production process is simple and easy to promote for industrial mass production. Attached Figure Description
[0020] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used in conjunction with embodiments of the invention to explain the invention and do not constitute a limitation thereof. In the drawings: Figure 1 is a schematic cross-sectional view of the moisture-proof and anti-powdering granular fertilizer of the present invention; Figure 2 shows the results of each sample under conditions of 25℃ and 80% relative humidity. Bar chart; Figure 3 shows a comparison of the drum pulverization rate and average compressive strength of each sample. Explanation of reference numerals in the attached diagram: 1 - Fertilizer core particle; 2 - Bonding transition layer; 3 - Coating layer. Detailed Implementation
[0021] The preferred embodiments of the present invention will be described below with reference to the accompanying drawings. It should be understood that the preferred embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.
[0022] In the attached diagram, all identical reference numerals refer to the same components.
[0023] As shown in Figure 1, the moisture-proof and anti-powdering granular fertilizer of the present invention has a spherical layered structure, with three layers coaxially distributed from the inside to the outside: Fertilizer core particle 1: It is a nutrient carrier, formed by steam agglomeration and granulation of nitrogen, phosphorus and potassium basic fertilizers into a dense aggregate with uniform internal pores, which is the basic nutrient carrying structure. Adhesive transition layer 2: It is uniformly filled in the surface pores of fertilizer core particles 1 and forms a continuous thin layer with a thickness of 10-30 μm. On the one hand, this layer wets and penetrates the surface pores of the core, forming a mechanical anchoring effect. On the other hand, it provides a hydrophilic-hydrophobic balanced bonding interface for the outer coating, significantly improving the interfacial bonding force between the coating layer and the core, and preventing the coating from falling off during storage and transportation. Coating layer 3: This is a continuous and dense hydrophobic barrier layer that is uniformly coated on the outer surface of the bonding transition layer 2, with a thickness of 30-80 μm. This layer uses paraffin-stearic acid as the hydrophobic matrix, mineral fillers as the reinforcing skeleton, and sodium carboxymethyl cellulose as the film-forming aid to form a continuous film layer that has both toughness and wear resistance. It can effectively block external water vapor from penetrating into the particle interior, while improving the wear resistance of the particle surface.
[0024] The three-layer structure has no obvious core defects or faults, high coating integrity, and the overall particle size is controlled within 2.0 to 4.0 mm, making it suitable for conventional mechanized fertilization equipment.
[0025] II. Raw Material Specifications The raw materials used in the following examples are all common industrial products, and their specific specifications are as follows: Urea: Grade I agricultural grade, total nitrogen (dry basis) ≥46.4%; Ammonium sulfate: Grade I agricultural grade, total nitrogen ≥21.0%, moisture ≤0.5%; Ammonium chloride: Grade I agricultural grade, total nitrogen ≥25.0%; Agricultural-grade monoammonium phosphate powder: total nutrients ≥64.0% (N≥11%, P2O5≥53%). Superphosphate: Agricultural grade, with available P2O5 ≥ 12.0%; Agricultural grade potassium chloride: potassium oxide ≥ 60.0%; Agricultural grade potassium sulfate: potassium oxide ≥ 50.0%; Corn pregelatinized starch: industrial grade, gelatinization degree ≥85%, 100 mesh passing rate ≥98%; Sodium-based bentonite: Industrial grade, 200 mesh passing rate ≥90%, expansion capacity ≥15mL / g; No. 58 fully refined paraffin wax: melting point 56-60℃, oil content ≤0.5%; Industrial grade stearic acid: Grade 1, acid value 205~220mgKOH / g, freezing point ≥54℃; Heavy calcium carbonate: Industrial grade, 800-1200 mesh, whiteness ≥85%; Talc powder: Industrial grade, 800-1200 mesh, whiteness ≥85%; Sodium carboxymethyl cellulose (CMC): Industrial grade, medium viscosity, degree of substitution 0.6–0.9, 2% aqueous solution viscosity 300–800 mPa. s; Micronutrient raw material: Magnesium sulfate heptahydrate (MgSO4) 7H2O (industrial grade), zinc sulfate monohydrate (ZnSO4) H2O (industrial grade), borax decahydrate (Na2B4O7) 10H2O (industrial grade).
[0026] Example 1 Based on a dry basis total mass of fertilizer core granules as 100 parts by weight: Nitrogen source: 28 parts by weight of urea + 12 parts by weight of ammonium sulfate, totaling 40 parts by weight; Phosphorus source: 22 parts by weight of powdered agricultural grade monoammonium phosphate; Potassium source: 26 parts by weight of agricultural grade potassium chloride. Bonding transition layer: 2.5% of the total dry weight of the core, corn pregelatinized starch: sodium bentonite = 2.5:1. Coating layer: 5% of the total mass of the granular fertilizer; based on a total dry weight of 100 parts by weight of the coating layer: 24 parts by weight of No. 58 fully refined paraffin wax, 8 parts by weight of industrial grade stearic acid, 28 parts by weight of heavy calcium carbonate, 10 parts by weight of talc (total mineral fillers 38 parts by weight), 5 parts by weight of sodium carboxymethyl cellulose; the mineral filler fineness is 1000 mesh. Finished product structural parameters: core particle size 2.0–4.0 mm, bonding transition layer thickness 15–25 μm, coating layer thickness 40–60 μm.
[0027] S1 Core Granulation: The weighed nitrogen, phosphorus, and potassium sources are added to a 500L horizontal ribbon mixer with a material filling rate of 65%. The mixture is stirred at 30 r / min for 12 minutes until the material has a uniform color. The mixed powder is then fed into a 1.2m diameter, 4m length rotary drum granulator via a screw conveyor. The drum tilt angle is 2.5°, the rotation speed is 15 r / min, and the material filling rate is 30%. Saturated steam at a pressure of 0.25MPa and a steam flow rate of 90kg / h is introduced through a steam nozzle to wet and agglomerate the powder surface. The material temperature inside the machine is stabilized at 60℃, and the granulation time is 10 minutes. The granulated product is then sent to a mesh belt dryer and pre-dried at 65℃ for 8 minutes until the moisture content of the core particles is 3.0%. The core particles are then sieved through a double-layer vibrating screen with an upper screen aperture of 4.0mm and a lower screen aperture of 2.0mm to obtain qualified core particles.
[0028] S2 Adhesive Layer Spraying: Qualified core particles are fed into a rotary coating machine with a diameter of 1.0m and a length of 2.5m, with a filling rate of 40% and a rotation speed of 20r / min. A 10% mass concentration aqueous suspension of adhesive is atomized and sprayed using a two-fluid atomizing nozzle, with an atomization pressure of 0.2MPa and a spraying flow rate of 100L / h. During the spraying process, 45℃ hot air is introduced to maintain the material temperature at 45℃. After the spraying is completed, the machine continues to rotate for 2 minutes to allow the suspension to penetrate evenly and form a continuous adhesive transition layer.
[0029] S3 Melt Coating: Add each component of the coating layer to a water bath heating vessel according to the ratio, heat to 80°C under stirring until completely melted, and keep warm for later use; add the molten material to the rotary coating machine at a uniform rate through a metering pump, with a dripping time of 4 minutes; continuously introduce 45°C hot air during the coating process, maintain the machine temperature at 55°C, rotate at 15 r / min, and keep the total coating time at 7 minutes, so that the molten material is evenly spread and coated on the surface of the bonding transition layer.
[0030] S4 Drying and Cooling: The coated granules are fed into a drum dryer with an inlet air temperature of 70℃ and a material residence time of 15 minutes. The moisture content of the finished granules after drying is 1.2%. They are then fed into a counter-current air-cooled cooling cylinder with a wind speed of 2.0 m / s to cool the material to a temperature of 28℃. After screening by a single-layer vibrating screen, unqualified granules and fine powder are removed to obtain finished granular fertilizer with a particle size of 2.0 to 4.0 mm.
[0031] Example 2 Based on a dry basis total mass of fertilizer core granules as 100 parts by weight: Nitrogen source: 22 parts by weight of urea + 15 parts by weight of ammonium chloride, totaling 37 parts by weight; Phosphorus source: 25 parts by weight of superphosphate; Potassium source: 28 parts by weight of agricultural grade potassium sulfate. Bonding transition layer: 2.0% of the total dry weight of the core, corn pregelatinized starch: sodium bentonite = 2:1. Coating layer: 4% of the total mass of the granular fertilizer; based on 100 parts by weight of the coating layer (dry weight): 26 parts by weight of No. 58 fully refined paraffin wax, 7 parts by weight of industrial grade stearic acid, 35 parts by weight of heavy calcium carbonate (mineral filler), 4 parts by weight of sodium carboxymethyl cellulose; the mineral filler fineness is 800 mesh. Finished product structural parameters: core particle size 2.0–4.0 mm, bonding transition layer thickness 10–20 μm, coating layer thickness 30–50 μm.
[0032] S1 Core Granulation: After mixing the raw materials for 10 minutes, they are fed into a rotary drum granulator. Saturated steam at 0.2 MPa is introduced at a flow rate of 80 kg / h, the internal temperature is 65℃, and the granulation time is 12 minutes. The material is then initially dried at 60℃ for 10 minutes until the core moisture content reaches 3.5%. Core particles of 2.0–4.0 mm are obtained by sieving. S2 Binder Coating: The binder suspension has a mass concentration of 8%, an atomization pressure of 0.15 MPa, a spray flow rate of 80 L / h, a material temperature of 40℃, and a rotation speed of 18 r / min. After spraying, the material is rotated for 2 minutes to form a bonding transition layer. S3 Melt Coating: The coating material is preheated to 75℃ and completely melted, with a dripping time of 3 minutes. The internal temperature is maintained at 50℃, the rotation speed is 12 r / min, and the total coating time is 6 minutes. S4 Drying and Cooling: Drying temperature 65℃, material residence time 12min, moisture content after drying 1.3%; counter-current air cooling to material temperature 26℃, sieved to obtain finished product.
[0033] Example 3 Based on a dry basis total mass of fertilizer core granules as 100 parts by weight: Nitrogen source: 24 parts by weight of urea + 16 parts by weight of ammonium sulfate, totaling 40 parts by weight; Phosphorus source: 20 parts by weight of powdered agricultural grade monoammonium phosphate; Potassium source: 24 parts by weight of agricultural grade potassium chloride; Micronutrient additives: 6 parts by weight, composed of magnesium sulfate heptahydrate: zinc sulfate monohydrate: borax decahydrate = 3:1.5:1. Bonding transition layer: 3.5% of the total dry weight of the core, composed of corn pregelatinized starch: sodium bentonite = 3:1. Coating layer: 7% of the total particle weight; based on a total dry weight of 100 parts by weight of the coating layer: 20 parts by weight of No. 58 fully refined paraffin wax, 10 parts by weight of industrial grade stearic acid, 38 parts by weight of talc (mineral filler), and 7 parts by weight of sodium carboxymethyl cellulose; the mineral filler fineness is 1200 mesh. Finished product structural parameters: core particle size 2.0–4.0 mm, bonding transition layer thickness 20–30 μm, coating layer thickness 60–80 μm.
[0034] S1 Core Granulation: Nitrogen, phosphorus, potassium, and trace element additives are mixed for 15 minutes and then fed into a rotary drum granulator. Saturated steam at 0.35 MPa is introduced at a flow rate of 100 kg / h. The internal temperature is 58°C, and the granulation time is 14 minutes. Preliminary drying at 70°C for 6 minutes is performed until the core moisture content reaches 2.5%. Core particles of 2.0–4.0 mm are obtained by sieving. S2 Binder Coating: The binder suspension has a mass concentration of 12%, an atomization pressure of 0.25 MPa, a spray flow rate of 120 L / h, a material temperature of 50°C, and a rotation speed of 25 r / min. After spraying, the mixture rotates for 3 minutes to form a bonding transition layer. S3 Melt Coating: The coating material is preheated to 85°C and completely melted. The addition time is 5 minutes. The internal temperature is maintained at 60°C, and the rotation speed is 18 r / min. The total coating time is 9 minutes. S4 Drying and Cooling: Drying temperature 75℃, material residence time 18min, moisture content after drying 1.1%; counter-current air cooling to material temperature 27℃, sieved to obtain finished product.
[0035] Comparative Example 1 (Ordinary uncoated granular fertilizer) Using the exact same core raw material ratio as in Example 1, the finished particles were obtained only through drum granulation, drying, and sieving. There was no adhesive transition layer or coating layer, and the finished particle size was 2.0–4.0 mm. The preparation process parameters were the same as step S1 in Example 1.
[0036] Comparative Example 2 (Coated granular fertilizer without a bonding transition layer) Using the same core raw materials and coating layer formulation as in Example 1, the coating layer is directly coated on the surface of the core particles without setting a bonding transition layer; the preparation process is completely consistent with Example 1 except that step S2 is omitted, and the finished particle size is 2.0-4.0 mm.
[0037] III. Performance Verification Tests and Result Analysis 1. Testing methods (the basis for verifying beneficial effects data) All tests were conducted with 3 parallel samples, and the average value of the results was taken. The test methods are as follows: (1) Moisture absorption rate test: The sample to be tested was dried at 105℃ to constant weight. 50.00g of sample was accurately weighed and spread evenly in a 90mm diameter petri dish. The sample was placed in a constant temperature and humidity chamber at 25±1℃ and 80±2% relative humidity. The mass was weighed on the 3rd, 7th and 30th days respectively, and the moisture absorption rate was calculated: Moisture absorption rate (%) = (mass after storage - initial mass) / initial mass × 100% (2) Drum pulverization rate test: The drum abrasion test method was adopted. The drum had an inner diameter of 200 mm and a length of 150 mm, with an internal lifting baffle. 100.00 g of qualified particle sample was weighed and placed into the drum. The drum was rotated at 50 r / min for 5 min. After removal, the sample was sieved through a 1.0 mm standard test sieve. The mass of the fine powder under the sieve was weighed, and the pulverization rate was calculated: Pulverization rate (%) = Mass of fine powder under the sieve / Initial mass of sample × 100% (3) Particle compressive strength test: Refer to GB / T 8571-2008 "Determination of compressive strength of compound fertilizer particles", use a particle strength tester, randomly select 30 samples with uniform particle size, measure the radial crushing force of each particle, and take the average value as the average compressive strength of the particles, unit N / particle.
[0038] (4) Agglomeration rate test: Simulate actual storage conditions, weigh 2.0 kg of sample, seal it in a polyethylene film bag, apply a constant static pressure of 50 kPa, and store it in an environment with a temperature of 30±1℃ and a relative humidity of 80±2% for 30 days; after taking it out, sieve it with a standard sieve with a aperture of 10 mm, weigh the mass of the agglomerates on the sieve, and calculate the agglomeration rate: Agglomeration rate (%) = mass of agglomerates / total mass of sample × 100%.
[0039] 2. Test Result Data The performance test results of each embodiment and comparative example are shown in the table below: Table 1 Comparison of performance test results for each sample
[0040] 3. Analysis of results in conjunction with the attached figures Based on the comparison charts in Figures 2 and 3 and the above data, the beneficial effects of the present invention are verified as follows: Moisture-proof performance verification: As shown in Figure 2, the 7-day moisture absorption rate of Examples 1-3 of the present invention is only 1.85%-2.68%, far lower than the 9.37% of Comparative Example 1, with a reduction of 71%-80%; the 30-day agglomeration rate is only 2.5%-4.7%, a reduction of 87%-93% compared to Comparative Example 1. Compared with Comparative Example 2 without a bonding transition layer, the 7-day moisture absorption rate of Example 1 is reduced by 43.3%, and the agglomeration rate is reduced by 64.0%, proving that the bonding transition layer fills the pores on the core surface, reduces pinhole defects in the membrane layer, and synergistically enhances the water vapor barrier effect with the coating layer.
[0041] Anti-pulverization and strength verification: As shown in Figure 3, the pulverization rate of the drum in this embodiment of the invention is reduced to 0.58%–0.91%, which is 86%–91% lower than that of Comparative Example 1; the average compressive strength is increased to 12.6–16.3 N / particle, which is 75%–126% higher than that of Comparative Example 1. Compared with Comparative Example 2, the pulverization rate of Example 1 is reduced by 69.5%, and the compressive strength is increased by 41.0%, indicating that the bonding transition layer significantly improves the interfacial bonding force between the coating layer and the core through mechanical anchoring, thus avoiding coating detachment and surface breakage during storage and transportation.
[0042] Cost Compatibility Verification: The paraffin wax, bentonite, and heavy calcium carbonate used in this invention are all bulk industrial products produced in quantities of tens of thousands of tons. The raw material costs are only 1 / 5 to 1 / 3 of those for polymer resin coating materials. The production equipment uses rotary drum granulators and rotary coating machines commonly used in compound fertilizer plants, requiring no additional specialized equipment. The production line modification cost is less than 15% of that of polymer coating processes. Calculations show that the overall cost of the finished product from this invention is 42% to 48% lower than that of polyurethane-coated fertilizers with similar performance.
[0043] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A moisture-proof and anti-powdering granular fertilizer, comprising fertilizer core particles, wherein the fertilizer core particles contain a nitrogen source, a phosphorus source, and a potassium source, characterized in that, The granular fertilizer consists of, from the inside out, a fertilizer core particle (1), a bonding transition layer (2), and a coating layer (3). Based on a dry basis total mass of 100 parts by weight, the fertilizer core particle (1) contains 20-45 parts by weight of nitrogen source, 10-30 parts by weight of phosphorus source, and 15-35 parts by weight of potassium source. The bonding transition layer (2) has a mass of 1.5%-4% of the dry basis total mass of the fertilizer core particle (1) and is composed of a mixture of pregelatinized starch and bentonite. The coating layer (3) has a mass of 3%-8% of the total mass of the granular fertilizer. Based on a dry basis total mass of 100 parts by weight, the coating layer (3) contains 15-30 parts by weight of paraffin wax, 5-12 parts by weight of stearic acid, 20-40 parts by weight of mineral filler, and 3-8 parts by weight of sodium carboxymethyl cellulose.
2. The moisture-proof and anti-pulverization granular fertilizer according to claim 1, characterized in that, The nitrogen source is one or more of urea, ammonium sulfate, and ammonium chloride; the phosphorus source is agricultural grade monoammonium phosphate or superphosphate; and the potassium source is agricultural grade potassium chloride or potassium sulfate.
3. The moisture-proof and anti-pulverization granular fertilizer according to claim 1, characterized in that, The fertilizer core granules (1) also contain micronutrient additives, the amount of which is 2% to 8% of the total dry weight of the fertilizer core granules (1); the micronutrient additives are a combination of two or more of magnesium sulfate, zinc sulfate and borax.
4. The moisture-proof and anti-pulverization granular fertilizer according to claim 1, characterized in that, The mass ratio of pregelatinized starch to bentonite in the bonding transition layer (2) is 2-3:1; the pregelatinized starch is corn pregelatinized starch, and the bentonite is sodium bentonite.
5. The moisture-proof and anti-pulverization granular fertilizer according to claim 1, characterized in that, The paraffin in the coating layer (3) is No. 58 fully refined paraffin; the stearic acid is industrial grade stearic acid; the mineral filler is one or two of heavy calcium carbonate and talc, and the filler fineness is 800-1200 mesh; the sodium carboxymethyl cellulose is an industrial grade medium viscosity product.
6. The moisture-proof and anti-pulverization granular fertilizer according to claim 1, characterized in that, The fertilizer core particles (1) have a particle size of 2.0 to 4.0 mm; the bonding transition layer (2) has a thickness of 10 to 30 μm; and the coating layer (3) has a thickness of 30 to 80 μm.
7. A method for preparing the moisture-proof and anti-powdering granular fertilizer according to any one of claims 1 to 6, comprising the steps of raw material mixing, granulation, and sieving, characterized in that, It also includes the steps of adhesive layer spraying, melt coating, drying and cooling, which are carried out in the following steps: S1 Core granulation: Nitrogen source, phosphorus source and potassium source are mixed evenly according to the ratio and sent to the rotary drum granulator. Saturated steam is introduced to agglomerate and granulate. After the product is pre-dried, it is screened to obtain fertilizer core granules (1); S2 Adhesive layer spraying: Fertilizer core granules (1) are sent to the rotary coating machine, and the adhesive suspension is sprayed by atomization. After rotation, an adhesive transition layer (2) is formed; S3 Melt coating: Pre-melted coating layer (3) material is added to the rotary coating machine, and the temperature inside the machine is maintained so that the coating material is coated on the surface of the adhesive transition layer (2); S4 Drying and cooling: The coated granules are dried and air-cooled to room temperature. After screening, the finished granular fertilizer is obtained.
8. The preparation method according to claim 7, characterized in that, In step S1, the saturated steam pressure is 0.2–0.35 MPa, the granulation temperature is 55–70℃, and the granulation time is 8–15 min; the preliminary drying temperature is 60–70℃, the moisture content of the core particles after drying is 2%–4%, and the particle size of the core particles after sieving is 2.0–4.0 mm.
9. The preparation method according to claim 7, characterized in that, In step S2, the adhesive suspension is an aqueous suspension of pregelatinized starch and bentonite with a mass concentration of 8% to 12%, and the material temperature is maintained at 40 to 55°C during spraying; In step S3, the coating layer (3) material is preheated to 70 to 90°C until completely melted, the machine temperature is maintained at 50 to 65°C during the coating process, and the coating time is 5 to 10 minutes.
10. The preparation method according to claim 7, characterized in that, In step S4, the drying temperature is 60-80℃, the moisture content of the finished product granules after drying is ≤1.5% by mass; the material temperature after cooling is ≤30℃; and the finished product is screened to obtain granular fertilizer with a particle size of 2.0-4.0mm.