A copper-based complex and its preparation method and application; a humidity indicator material and its preparation method.
By preparing and applying copper-based complexes as color developers, the problems of limited cobalt content and high cost in traditional humidity indicator materials have been solved, providing a low-cost and environmentally friendly humidity indicator material solution and achieving efficient and reversible humidity indication effects.
Patent Information
- Application Number
- CN202611344274.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional cobalt-containing humidity indicators are restricted in their application because they contain cobalt chloride, which is classified as a Group 2 carcinogen under the EU REACH regulation. Meanwhile, cobalt-free silica gel color-changing indicators are more expensive.
Using copper-based complexes as color developers, copper-based complexes are prepared through complexation reactions and adsorbed onto a carrier. Color changes are achieved by utilizing the coordination equilibrium shift of water molecules, thus preparing a low-cost and environmentally friendly humidity indicator material.
This invention achieves a low-cost, environmentally friendly humidity indicator material that is reusable, meets EU environmental standards, has a simple manufacturing process, high production efficiency, and can replace traditional cobalt-containing humidity indicator materials.
Smart Images

Figure CN123106443A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of functional materials technology, and in particular to a copper-based complex and its preparation method and application, and a humidity indicator material and its preparation method. Background Technology
[0002] Humidity indicator materials are generally color-changing silica gel or humidity indicator cards. Color-changing silica gel uses microporous silica gel as a matrix, while humidity indicator cards use cellulose paper as a carrier and are usually loaded with cobalt chloride. They absorb moisture and undergo a reversible color change (blue-pink), achieving visual humidity indication. They are widely used in moisture-proof indication scenarios such as electronics, pharmaceuticals, precision instruments, lithium batteries, food packaging, and transformer respirators.
[0003] Traditional cobalt-containing humidity indicators are the mainstream products in the current market, but their application is restricted because they contain cobalt chloride, which is classified as a Group 2 carcinogen under the EU REACH regulation. Cobalt-free silica gel or humidity indicator cards primarily use methyl violet as the color-changing indicator, utilizing the change in pH value of the surface microenvironment after the silica gel absorbs water, thus causing a color change; however, methyl violet is relatively expensive to use. Summary of the Invention
[0004] In view of this, the purpose of this invention is to provide a copper-based complex and its preparation method and application, as well as a humidity indicator material and its preparation method. This invention uses a copper-based complex as a colorimetric agent, which is non-toxic and environmentally friendly, and has low raw material costs, and is expected to gradually replace traditional cobalt-containing humidity indicator materials.
[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a copper-based complex having the structure shown in Formula 1: X2[CuY4] Equation I; In Formula 1, X is an ammonium ion or an organic ammonium cation, wherein the organic ammonium cation is a primary amine ion, a secondary amine ion, or a tertiary amine ion; Y is a chloride ion or a bromide ion.
[0006] Preferably, the substituents in the primary amine ion are C1-C18 alkyl groups; the two substituents in the secondary amine ion are independently C1-C18 alkyl groups; and the three substituents in the tertiary amine ion are independently C1-C18 alkyl groups.
[0007] The present invention provides a method for preparing the copper-based complex described above, comprising the following steps: performing a complexation reaction between a salt containing X and a salt containing Y in an alcohol solvent, removing the solvent, and obtaining the copper-based complex; wherein the salt containing X is ammonium chloride, ammonium bromide, hydrochloride of an organic amine cation, or hydrobromide of an organic amine cation; and wherein the salt containing Y is copper chloride or copper bromide.
[0008] This invention provides the application of the copper-based complex described above as a colorimetric agent in humidity indicator materials.
[0009] The present invention provides a humidity indicating material, comprising a carrier and a copper-based complex adsorbed on the carrier; the copper-based complex is one or more of the copper-based complexes described in the above embodiments.
[0010] Preferably, the carrier comprises granular silica gel or cellulose filter paper.
[0011] This invention provides a method for preparing the humidity indicating material described above, comprising the following steps: dissolving a copper-based complex in a mixed solvent to obtain a complex solution; The carrier is immersed in the complex solution for adsorption, and then dried to obtain the humidity indicator material.
[0012] Preferably, the mixed solvent is a water-alcohol mixture or a water-alcohol ether mixture; the alcohol includes ethanol and / or isopropanol; the alcohol ether includes diethylene glycol butyl ether.
[0013] Preferably, the concentration of copper ions in the complex solution is 0.01 g / L to 5 g / L.
[0014] Preferably, the soaking time is 0.5 to 1 hour.
[0015] This invention provides a copper-based complex that utilizes the principle of water molecules participating in the coordination equilibrium shift, leading to a change in the environment of the central copper ion ligand. Upon contact with water, the copper ion complex containing specific ligands (chloride or bromide ions) dissociates into hydrated copper ions, achieving a color change from a dry to a hygroscopic state. Specifically, it transforms from a non-white state (which can appear yellow, purple, or blue depending on the types X and Y) to white (hydrated copper ions are very light in color at lower concentrations, appearing white on the carrier). This process is reversible; after drying or absorbing moisture, the color changes significantly. The copper-based complex provided by this invention is sensitive to humidity and can be reused.
[0016] The present invention also provides a method for preparing the above-mentioned copper-based complex. The preparation method of the present invention is simple to operate and easy to implement for industrial application.
[0017] This invention provides a humidity indicator material. After the carrier adsorbs a copper-based complex, it exhibits a color change in response to changes in moisture content. Furthermore, the preparation process of the copper-based complex-based humidity indicator material is simple, efficient, and cost-effective, thus effectively replacing existing cobalt-containing humidity indicator materials. The results of the embodiments show that the copper-based complex-based humidity indicator material prepared by this invention exhibits significant color change in response to moisture, extremely high stability, and can be recycled multiple times.
[0018] This invention uses copper-based complexes as color developers, requiring a low dosage, and is non-toxic and environmentally friendly, meeting EU environmental standards. The raw material cost is low, and it is expected to gradually replace traditional cobalt-containing humidity indicator materials. Attached Figure Description
[0019] Figure 1 The color change of the humidity indicator material prepared in Example 1 in dry and wet states; Figure 2 The color change of the humidity indicator material prepared in Example 2 in dry and wet states; Figure 3 The color change of the humidity indicator material prepared in Example 3 in dry and wet states; Figure 4 The color change of the humidity indicator material prepared in Example 4 in dry and wet states; Figure 5 The color change of the humidity indicator material prepared in Example 5 in dry and wet states. Detailed Implementation
[0020] This invention provides a copper-based complex having the structure shown in Formula 1: X2[CuY4] Equation I; In Formula 1, X represents the ammonium ion [NH4+]. + [Or an organic ammonium cation, wherein the organic ammonium cation is a primary amine ion [RNH3] + Secondary amine ions [(R)2NH2] + or tertiary amine ion [(R)3NH + ]; Y represents chloride or bromide ions.
[0021] In this invention, the substituent in the primary amine ion is a C1-C18 alkyl group; in specific embodiments, it can be methyl, ethyl, propyl, butyl, or pentyl.
[0022] In this invention, the two substituents in the secondary amine ion are independently C1-C18 alkyl groups; in specific embodiments, they can be independently methyl, ethyl, propyl, butyl, or pentyl. In this invention, "independently" means that the two substituents in the secondary amine ion can be the same or different, but both can be C1-C18 alkyl groups.
[0023] In this invention, the three substituents in the tertiary amine ion are independently C1-C18 alkyl groups; in specific embodiments, they can be independently methyl, ethyl, propyl, butyl, or pentyl.
[0024] In embodiments of the present invention, the copper-based complex may specifically be one or more of diammonium tetrabromocuinate, di(triethylammonium tetrabromocuinate), diammonium tetrachlorocuinate, and di(triethylammonium tetrachlorocuinate).
[0025] The present invention provides a method for preparing the copper-based complex described above, comprising the following steps: performing a complexation reaction between a salt containing X and a salt containing Y in an alcohol solvent, removing the solvent, and obtaining the copper-based complex.
[0026] In this invention, the salt containing X is ammonium chloride, ammonium bromide, hydrochloride of an organic amine cation, or hydrobromide of an organic amine cation; the salt containing Y is copper chloride or copper bromide. Both the salt containing X and the salt containing Y can be obtained by purchasing commercially available products.
[0027] In this invention, the molar ratio of the salt containing X to the salt containing Y is preferably 2:1; the alcohol solvent preferably includes methanol or ethanol; this invention does not impose a special limitation on the amount of the alcohol solvent used, as long as it is sufficient to completely dissolve the organic ammonium cation.
[0028] In this invention, the temperature of the complexation reaction is preferably room temperature (i.e., no additional heating or cooling is required), and the time is preferably 0.5 to 2 hours. This invention does not impose special requirements on the method of solvent removal; evaporation to dryness is acceptable.
[0029] This invention provides the application of the copper-based complex described above as a colorimetric agent in humidity indicator materials.
[0030] This invention utilizes the principle that water molecules participate in the shift of coordination equilibrium, thereby altering the environment of the central copper ion ligand. When a copper ion complex containing a specific ligand comes into contact with water, it dissociates into hydrated copper ions, achieving a color change from a dry state to a hygroscopic state.
[0031] The present invention provides a humidity indicating material, comprising a carrier and a copper-based complex adsorbed on the carrier; the copper-based complex is one or more of the aforementioned copper-based complexes.
[0032] In a specific embodiment, the copper-based complex can be diammonium tetrachlorocubic acid (i.e., X in Formula 1 is the ammonium ion NH4). + ), diorganoammonium tetrachlorocubic (i.e., X in formula 1 is an organic amine cation), diammonium tetrabromocubic (i.e., X in formula 1 is an ammonium ion NH4+). +It can be diammonium tetrabromocubinate or diorganoammonium tetrabromocubinate (i.e., X in Formula 1 is an organic amine cation), or it can be diammonium tetrabromocubinate and diorganoammonium tetrabromocubinate, or it can be diammonium tetrabromocubinate and diorganoammonium tetrabromocubinate. When it is diammonium tetrabromocubinate and diorganoammonium tetrabromocubinate, the molar ratio of diammonium tetrabromocubinate to diorganoammonium tetrabromocubinate is preferably 1:1.05 to 1:3, and in specific embodiments it can be 1:1.5, 1:2, 1:2.5 or 1:3. When it is diammonium tetrabromocubinate and diorganoammonium tetrabromocubinate, the molar ratio of diammonium tetrabromocubinate to diorganoammonium tetrabromocubinate is preferably 1:1.05 to 1:3, and in specific embodiments it can be 1:1.5, 1:2, 1:2.5 or 1:3.
[0033] In this invention, the carrier comprises granular silica gel or cellulose filter paper; the diameter of the granular silica gel is preferably 5-8 mm.
[0034] In this invention, in the dry state, the color of the humidity indicator material is related to the types of Y and X in the copper-based complex.
[0035] When Y in the copper-based complex is a chloride ion, the humidity indicator material is yellow in its dry state and turns white after absorbing moisture. When Y in the copper-based complex is a bromide ion and X is either a single ammonium ion or a single organic amine cation, it is blue in its dry state. When the copper-based complex is a mixture, i.e., X is both ammonium and organic amine cations, it is purple in its dry state and turns white after absorbing moisture.
[0036] When the humidity indicator material includes multiple copper-based complexes, the humidity indicator material is the color exhibited by the combination of each complex. It may not be limited to the aforementioned yellow, blue, or purple, but it is clearly not white, and it turns white after absorbing moisture, thereby achieving humidity indication.
[0037] This invention provides a method for preparing the humidity indicating material described above, comprising the following steps: dissolving a copper-based complex in a mixed solvent to obtain a complex solution; The carrier is immersed in the complex solution for adsorption, and then dried to obtain the humidity indicator material.
[0038] This invention dissolves a copper-based complex in a mixed solvent to obtain a complex solution.
[0039] In this invention, the mixed solvent is preferably a water-alcohol mixed solvent or a water-alcohol ether mixed solvent; the alcohol preferably includes ethanol and / or isopropanol; the alcohol ether preferably includes diethylene glycol butyl ether copper complex; the mass ratio of water to alcohol in the water-alcohol mixed solvent is preferably 17:1 to 18:1; the mass ratio of water to alcohol ether in the water-alcohol ether mixed solvent is preferably 17:1 to 18:1.
[0040] In this invention, the concentration of copper ions in the complex solution is preferably 0.01 g / L to 5 g / L, and in specific embodiments it can be 0.01, 0.03, 0.05, 0.1, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 or 5 g / L.
[0041] After obtaining the complex solution, the present invention immerses the carrier in the complex solution for adsorption, removes it and dries it to obtain the humidity indicator material.
[0042] In this invention, the impregnation is preferably carried out at room temperature, i.e., no additional heating or cooling is required; the impregnation time is preferably 0.5 to 1 hour. In this invention, the drying is preferably vacuum drying; the vacuum drying pressure is preferably -0.9 MPa, and the temperature is preferably 60 to 90°C.
[0043] The following detailed descriptions, in conjunction with embodiments, illustrate the copper-based complexes and their preparation methods and applications, as well as the humidity indicator materials and their preparation methods provided by the present invention. However, these descriptions should not be construed as limiting the scope of protection of the present invention.
[0044] The preparation process of the diammonium tetrabromocubic acid used in the following examples is as follows: Ammonium bromide and copper bromide are mixed in methanol at a molar ratio of 2:1 at room temperature for 1 hour. The solvent is then removed by evaporation to obtain diammonium tetrabromocopperate.
[0045] The preparation process of the tetrabromocubic di(triethylammonium cation) used is as follows: Triethylamine hydrobromide and copper bromide were mixed in methanol at a molar ratio of 2:1 and stirred for 1 hour at room temperature. The solvent was then removed by evaporation to obtain tetrabromocopper bis(triethylammonium cation).
[0046] The preparation process of the diammonium tetrachlorocubic acid used is as follows: Ammonium chloride and copper chloride are mixed in methanol at a molar ratio of 2:1 at room temperature for 1 hour. The solvent is then removed by evaporation to obtain diammonium tetrachlorocuprate.
[0047] The preparation process of the tetrachlorocubic acid di(triethylammonium cation) used is as follows: Triethylamine hydrochloride and copper chloride were mixed in methanol at a molar ratio of 2:1 for 1 hour at room temperature. The solvent was then removed by evaporation to obtain tetrachlorocubic acid di(triethylammonium cation).
[0048] Example 1 Diammonium tetrabromocubic acid and di(triethylammonium tetrabromocubic acid) were mixed in a molar ratio of 1:1.5 and dissolved in a mixed solvent containing water and isopropanol (water to isopropanol mass ratio of 90:5), with a copper ion concentration of 3 g / L. 10 g of porous silica gel with a diameter of 5-8 mm was soaked in 20 g of the above solution containing the copper-based complex for 1 hour. The solution was filtered off, the silica gel was removed, and dried in a vacuum drying oven at 90°C for 2 hours to obtain purple silica gel particles. This silica gel turned white after absorbing moisture at room temperature in an environment with humidity >65%. Figure 1 As shown, there is a clear difference in color.
[0049] Example 2 Diammonium tetrabromocubic acid was dissolved in a mixed solvent containing water and isopropanol (water to isopropanol mass ratio 90:5), with a copper ion concentration of 3 g / L. 10 g of porous silica gel with a diameter of 5-8 mm was immersed in 20 g of the above solution containing the copper-based complex for 1 hour. After adsorption, the solution was filtered off, and the silica gel was removed and dried in a vacuum drying oven at 90°C for 2 hours to obtain blue silica gel particles. This silica gel turned white after absorbing moisture at room temperature in an environment with humidity >65%. Figure 2 As shown, there is a clear difference in color.
[0050] Example 3 Tetrabromocopper bis(triethylammonium cation) was dissolved in a mixed solvent containing water and isopropanol (water to isopropanol mass ratio 90:5), with a copper ion concentration of 3 g / L. 10 g of porous silica gel with a diameter of 5-8 mm was soaked in 20 g of the above solution containing the copper-based complex for 1 hour. The solution was filtered off, the silica gel was removed, and dried in a vacuum drying oven at 90°C for 2 hours to obtain blue silica gel particles. This silica gel turned white after absorbing moisture at room temperature in an environment with humidity >65%. Figure 3 As shown, there is a clear difference in color.
[0051] Example 4 Diammonium tetrabromocubic acid and di(triethylammonium tetrabromocubic acid) were mixed in a 1:1.5 ratio and dissolved in a mixed solvent containing water and isopropanol (water to isopropanol mass ratio 85:5), resulting in a copper ion concentration of 3 g / L. A 7 cm diameter cellulose filter paper was soaked in 20 g of the above solution containing the copper-based complex for 0.5 h. The filter paper was then removed and dried in a vacuum drying oven at 90 °C for 0.5 h to obtain purple test paper. This test paper turned white after absorbing moisture. Figure 4 As shown, there is a clear difference in color.
[0052] Example 5 Diammonium tetrachlorocubic acid and di(triethylammonium tetrachlorocubic acid) were mixed in a 1:1.5 ratio and dissolved in a mixed solvent containing water and isopropanol (water to isopropanol mass ratio 90:5), resulting in a copper ion concentration of 3 g / L. A 7 cm diameter cellulose filter paper was soaked in 20 g of the above solution containing the copper-based complex for 0.5 h. The filter paper was then removed and dried in a vacuum drying oven at 90 °C for 0.5 h to obtain yellow test paper. This test paper turned white after absorbing moisture at room temperature with humidity >65%. Figure 5 As shown, there is a clear difference in color.
[0053] Comparative Example 1 A commercially available cobalt chloride aqueous solution was prepared, and porous silica gel or cellulose filter paper was used as a carrier. After drying, a humidity indicator material was obtained that changed from blue to pink after absorbing moisture. However, due to the presence of cobalt chloride, the application of this material is restricted by environmental regulations.
[0054] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A copper-based complex, characterized in that, It has the structure shown in Equation 1: X2[CuY4] Equation I; In Formula 1, X is an ammonium ion or an organic ammonium cation, wherein the organic ammonium cation is a primary amine ion, a secondary amine ion, or a tertiary amine ion; Y is a chloride ion or a bromide ion.
2. The copper-based complex according to claim 1, characterized in that, The substituents in the primary amine ion are C1-C18 alkyl groups; the two substituents in the secondary amine ion are independently C1-C18 alkyl groups; and the three substituents in the tertiary amine ion are independently C1-C18 alkyl groups.
3. The method for preparing the copper-based complex according to claim 1 or 2, characterized in that, The method includes the following steps: performing a complexation reaction between a salt containing X and a salt containing Y in an alcohol solvent, removing the solvent, and obtaining the copper-based complex; wherein the salt containing X is ammonium chloride, ammonium bromide, hydrochloride of an organic amine cation, or hydrobromide of an organic amine cation; and wherein the salt containing Y is copper chloride or copper bromide.
4. The use of the copper-based complex of claim 1 or 2 as a colorimetric agent in humidity indicator materials.
5. A humidity indicating material, characterized in that, It includes a carrier and a copper-based complex adsorbed on the carrier; the copper-based complex is one or more of the copper-based complexes described in claim 1 or 2.
6. The humidity indicating material according to claim 5, characterized in that, The carrier includes granular silica gel or cellulose filter paper.
7. A method for preparing the humidity indicating material according to claim 5 or 6, characterized in that, Includes the following steps: The copper-based complex was dissolved in a mixed solvent to obtain a complex solution; The carrier is immersed in the complex solution for adsorption, and then dried to obtain the humidity indicator material.
8. The preparation method according to claim 7, characterized in that, The mixed solvent is a water-alcohol mixture or a water-alcohol ether mixture; the alcohol includes ethanol and / or isopropanol; the alcohol ether includes diethylene glycol butyl ether.
9. The preparation method according to claim 7, characterized in that, The concentration of copper ions in the complex solution is 0.01 g / L to 5 g / L.
10. The preparation method according to claim 7, characterized in that, The soaking time is 0.5 to 1 hour.