A high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material and its preparation method

By optimizing the composition and processing technology of PA6/PP alloy materials, the problem of synergistic effect of high whiteness, halogen-free flame retardancy and mechanical properties was solved, and high-performance glass fiber reinforced PA6/PP halogen-free flame retardant alloy materials were prepared for application in the fields of electronics, electrical appliances and automotive interiors.

CN123107345APending Publication Date: 2026-11-17中广核俊尔(浙江)新材料有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611196263.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve a balance between high whiteness, halogen-free flame retardancy, mechanical properties, and appearance quality in PA6/PP alloy materials. Problems such as poor compatibility, poor thermal stability of halogen-free flame retardants, and appearance defects caused by glass fiber reinforcement result in unstable material performance during mass production.

Method used

High-whiteness, high-performance glass fiber reinforced PA6/PP halogen-free flame retardant alloy material is prepared by using a specific ratio of PA6, PP chips, alkali-free glass fiber, composite halogen-free flame retardant, composite compatibilizer and high whiteness color powder, through melt blending in a twin-screw extruder and multi-stage vacuum devolatilization.

Benefits of technology

It achieves high whiteness (L value ≥ 96), halogen-free flame retardant UL94 V-0, cantilever beam notched impact strength ≥ 12kJ/m², tensile strength ≥ 110MPa, water absorption ≤ 0.8%, no appearance defects, stable material performance, and is suitable for electronic appliances, automotive interiors and other fields.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material, composed of the following raw materials by weight percentage: PA6 chips 30-50%; PP chips 5-20%; alkali-free glass fiber 15-25%; composite halogen-free flame retardant 15-20%; high-whiteness composite colorant 5-10%; composite compatibilizer 3-6%; stabilizer 0.1-1.2%; %; lubricant 0.1-0.7%. The resulting material can be used in electronic appliances, automotive interiors, and office equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer composite materials technology, specifically relating to a high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material and its preparation method. Background Technology

[0002] PA6, as a general-purpose engineering plastic, possesses excellent mechanical strength, heat resistance, wear resistance, and processability, making it a preferred base material for structural components. However, it suffers from core defects such as high polarity, high water absorption, poor dimensional stability, easy yellowing at high temperatures, and poor compatibility with halogen-free flame retardants. PP, as a non-polar polyolefin material, has advantages such as extremely low water absorption, chemical corrosion resistance, excellent flowability, and controllable cost. However, it suffers from insufficient rigidity, poor heat resistance, weak flame retardancy, and limited mechanical load-bearing capacity.

[0003] Conventional industry techniques utilize PA6 and PP blending to achieve complementary properties, combined with glass fiber reinforcement and halogen-free flame-retardant modification. This effectively reduces material water absorption, improves molding processability, and optimizes structural strength. However, its industrial application has always faced the industry pain point of being unable to simultaneously address the four core technical contradictions of "whiteness, flame retardancy, mechanical properties, and appearance quality." The specific difficulties are as follows: 1. The two phases have extremely different polarities, and compatibility defects lead to multiple performance degradations: PA6, which is highly polar, and PP, which is non-polar, form a thermodynamically incompatible system. Conventional single compatibilizers have weak interfacial bonding forces, and the blended system has severe phase separation, which directly leads to uneven dispersion and floating of glass fibers. Defects such as floating fibers, pitting, orange peel, and delamination appear on the surface of the product. At the same time, the concentration of interfacial stress will significantly reduce the impact, tensile and other mechanical properties of the material, making it impossible to balance appearance and structural strength.

[0004] 2. There is an inherent technical conflict between halogen-free flame retardancy and ultra-high whiteness: Existing mainstream halogen-free flame retardant systems (MCA, ordinary ammonium polyphosphate, metal hydroxide) generally have problems such as large addition amount, poor thermal stability, easy decomposition and yellowing at high temperature, and precipitation of white bloom in the later stage, which will directly reduce the whiteness of the product; while conventional whitening fillers and fluorescent whitening components are prone to side reactions with flame retardant systems, reducing flame retardant efficiency. At the same time, excessive filling will destroy the continuity of the matrix, causing a significant decrease in the toughness and rigidity of the material. It is difficult for the industry to achieve high whiteness and V0 grade halogen-free flame retardancy at the same time.

[0005] 3. The appearance defects of the glass fiber reinforced system are difficult to eradicate, and the high whiteness texture cannot be achieved: Glass fiber itself is an inorganic discolored filler, and the refractive index difference between it and the polymer matrix is ​​large, which easily causes the surface of the product to be hazy, dull, and have poor gloss. At the same time, PA6 and PP have significant differences in crystallization rate and shrinkage rate, and after molding, weld lines, pinholes, and uneven color difference are easy to occur. Conventional modification schemes can only achieve basic whiteness and cannot meet the ultra-high whiteness and high-end appearance requirements of L value ≥ 96.

[0006] 4. Poor thermal and oxygen stability, and insufficient batch stability in mass production: PA6 is prone to degradation and yellowing under high temperature shear, PP small molecule matrix has weak heat resistance, and the thermal decomposition temperature of halogen-free flame retardant overlaps with the matrix processing temperature range. During processing, thermal degradation and discoloration, and additive failure are prone to occur, resulting in large fluctuations in color difference between finished product batches and unstable mechanical properties. Continuous production is prone to problems such as broken strips, mold scale accumulation, and frequent appearance defects.

[0007] This invention innovatively solves the above-mentioned pain points. Summary of the Invention

[0008] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a glass fiber reinforced PA6 / PP alloy material and its preparation method that has high whiteness (L value ≥ 96), halogen-free flame retardancy UL94 V-0 (1.6mm), high rigidity and high toughness, low water absorption, no appearance defects, and can be stably mass-produced. This invention solves the three core problems of synergistic balance of high whiteness, high flame retardancy and high performance, control of appearance defects and process scale-up.

[0009] This invention, through the selection of PA6 and PP chip materials, compounding with halogen-free flame retardants, compounding with high-whiteness pigments, compounding with compatibilizers, and using certain optimized process methods, ultimately produces a high-whiteness, high-performance, halogen-free flame-retardant PA / PP alloy material.

[0010] This invention is achieved through the following technical solutions. A high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material, characterized in that it is composed of the following raw materials by weight percentage: PA6 sections: 30-50%; PP slices 5-20%; 15-25% alkali-free glass fiber; 15-20% composite halogen-free flame retardant; High whiteness composite pigments: 5-10%; Composite compatibilizer 3~6%; Stabilizer 0.1~1.2%; Lubricant 0.1~0.7%.

[0011] The PA6 chips are PA6 chips with a relative viscosity index of 1.8-2.4, preferably 2.45, and most preferably 2.45.

[0012] The PP chips are homopolymer PP chips, with a preferred MFR of 10-20g / 10min and the most preferred MFR of around 20g / 10min for Yangzi Petrochemical K9020.

[0013] The chopped glass fiber is a glass fiber with a chopped length of 3-5 mm and a single filament diameter of 9-13 μm. The preferred size is a chopped length of 3 mm and a single filament diameter of 10 μm. The most preferred size is T435N from Taishan Glass Fiber.

[0014] The composite halogen-free flame retardant is a mixture of coated ammonium polyphosphate, melamine polyphosphate, and organosilicon flame retardant synergist in a certain proportion, with the most preferred ratio being 10:4:4.

[0015] The high whiteness composite pigment is a mixture of coated rutile titanium dioxide, nano zirconium silicate, ultrafine activated precipitated barium sulfate, and Honeywell AC-540A super dispersant in a certain proportion, with the most preferred proportion being 6:0.8:1.2:1.

[0016] The composite compatibilizer is a mixture of PP-g-MA, PA6-g-PP and silane coupling agent KH-560 in a certain proportion, with the most preferred ratio being 3:1.5:0.5.

[0017] The stabilizing additive mainly consists of one or more of N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexamethylenediamine (antioxidant 1098), tris[2,4-di-tert-butylphenyl]phosphite (antioxidant 168), and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (antioxidant 1010). The preferred primary antioxidant is 1010, and the secondary antioxidant is 168, with an addition ratio of 2:1 and a preferred addition amount of 0.6%.

[0018] The lubricant is one or more of calcium stearate, modified ethylene bis-fatty acid amide (TAF), and ethylene-acrylic acid copolymer, preferably TAF, and the preferred addition amount is 0.4%.

[0019] The matrix resin, composite halogen-free flame retardant, and additives are mixed at high speed according to the formula. Short-cut glass fiber is added from the side of the second barrel, and high-whiteness composite color powder is added from the side of the sixth barrel. The mixture is melt-blended using a twin-screw extruder with glass fiber side feeding, multi-stage vacuum devolatilization, and gradient temperature control at 210–250℃. After water cooling, pelletizing, and drying, the finished product is obtained.

[0020] The material obtained by this invention has the following properties: notched impact strength of cantilever beam ≥12kJ / m², tensile strength ≥110MPa, water absorption ≤0.8%, and high whiteness (L value ≥96), UL94 V-0 (1.6mm).

[0021] The material obtained by this invention can be applied to integrated structural and aesthetic components in electronic appliances, automotive interiors, office equipment, etc., which require high whiteness (L value ≥ 96), halogen-free flame retardancy, high mechanical properties, low water absorption, and no appearance defects. Detailed Implementation

[0022] PA6, PP, flame retardant, and titanium dioxide were dried separately.

[0023] The short glass fiber is from Jushi Company; the compound flame retardant is composed of coated ammonium polyphosphate, melamine polyphosphate, and silicone flame retardant synergist in a ratio of 10:4:4. The coated ammonium polyphosphate is Clariant Exolit AP-462, the melamine polyphosphate is BASF Melapur 200, and the silicone flame retardant synergist is Guangzhou Lichao Polymer LC-591; the composite compatibilizer is PP-g-MA, PA6-g-PP, and silane coupling agent KH-560 in a ratio of 3:1.5:0.5, all of which are commercially available; the stabilizer is mainly antioxidant 1010 and auxiliary antioxidant 168 in a ratio of 2:1; the lubricant is TAF, which is commercially available.

[0024] The first compound colorant is composed of coated rutile titanium dioxide, nano-zirconium silicate, ultrafine activated precipitated barium sulfate, and Honeywell AC-540A in a ratio of 6:0.8:1.2:1. The coated rutile titanium dioxide is from Longbai Group LR-108, the nano-zirconium silicate is from Anmi Micro-Nano M-Z600, and the ultrafine activated precipitated barium sulfate is from Yunfu Hongzhi New Materials M-700. The second compound colorant is composed of coated rutile titanium dioxide, nano-zirconium silicate, ultrafine activated precipitated barium sulfate, and lubricant EBS in a ratio of 6:0.8:1.2:1. The coated rutile titanium dioxide is from Longbai Group LR-108. Nano-zirconium silicate: Anmi Micro-Nano M-Z600; Ultrafine activated precipitated barium sulfate: Yunfu Hongzhi New Materials M-700; Lubricant EBS is commercially available.

[0025] The matrix resin, composite halogen-free flame retardant, and additives are mixed at high speed according to the formula. Short-cut glass fiber is added from the side of the second barrel, and high-whiteness composite color powder is added from the side of the sixth barrel. The mixture is melt-blended using a twin-screw extruder with glass fiber side feeding, multi-stage vacuum devolatilization, and gradient temperature control at 210–250℃. After water cooling, pelletizing, and drying, the finished product is obtained.

[0026] The present invention will now be further described in conjunction with Comparative Example 1 and Embodiments 1-9.

[0027] Weigh the raw materials according to the proportions in Table 1, mix them in a high-speed mixer, and then extrude and granulate them into composite materials using a twin-screw extruder. Perform routine physicochemical analysis and glow wire testing on the composite materials obtained in the comparative examples and embodiments described above.

[0028] Table 1 shows the specific proportions of the embodiments and comparative columns 1-9. Material Description Example Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Comparative Example 9 Comparative Example 10 Comparative Example 11 PA6 JHS 2.45 40 42 39 41 39 41 39 35 36 40 40 40 K9020 15 15 15 15 15 15 15 15 15 15 15 15 short fiberglass 20 20 20 20 20 20 20 20 20 20 20 20 Compound flame retardants 15 14 16 15 15 15 15 / 15 15 15 15 APP (not compatible) / / / / / / / 20 / / / / Composite color powder 4 4 4 3 5 4 4 4 / 4 / / Comparison of color powder compound 1 4 / Contrast color powder compound 2 4 Titanium dioxide (not compounded) / / / / / / / / 8 / / / compatibilizer 5 5 5 5 5 4 6 5 5 / / / PP-g-MA (not compounded) 5 5 5 stabilizer 0.6 0.6 0.6 0.6 0.6 0.6 0.6 0.6 0.6 0.6 0.6 0.6 lubricant 0.4 0.4 0.4 0.4 0.4 0.4 0.4 0.4 0.4 0.4 0.4 0.4 Table 2 shows the results of conventional physicochemical property analysis and color and whiteness analysis of the examples and comparative columns 1-9. Test Project Detection methods Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Comparative Example 9 Comparative Example 10 Comparative Example 11 Tensile strength MPa GB / T1040.2-2022 129 130 127 124 125 131 105 125 110 115 130 128 Tensile modulus MPa GB / T1040.2-2022 4898 4950 4715 4811 4998 4977 4256 4891 3789 4331 4860 4890 Cantilever beam notch impact strength GB / T 1843-2008 12.5 13.1 10.9 13.4 10.2 10.8 14.9 5.4 4.9 5.5 12.8 12.4 Vertical burning (1.6mm) UL94 V0 V2 V0 V0 V0 V0 V2 V2 V0 V2 V0 V0 L value / 96.3 96.2 95.5 94.8 96.2 94.3 96.0 92.5 95.5 95.1 92.3 93.8 Appearance / normal normal normal normal normal Slight fiber floating Slight pockmarks Numerous pockmarks Numerous pockmarks Pitting, fusion splice lines, floating fibers normal normal The above embodiments are for illustrative purposes only and are not intended to limit the invention. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the invention. Therefore, all equivalent technical solutions should also fall within the scope of the invention and should be defined by the claims.

Claims

1. A high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material, composed of the following raw materials by weight percentage: PA6 sections: 30-50%; PP slices 5-20%; 15-25% alkali-free glass fiber; 15-20% composite halogen-free flame retardant; High whiteness composite pigments: 5-10%; Composite compatibilizer 3~6%; Stabilizer 0.1~1.2%; Lubricant 0.1~0.7%.

2. The high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material according to claim 1, characterized in that: The PA6 chips are PA6 chips with a relative viscosity index of 1.8-2.

4.

3. The high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material according to claim 1, characterized in that: The PP chips are homopolymer PP.

4. The high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material according to claim 1, characterized in that: The chopped glass fiber is a short-cut glass fiber with a chopped length of 3-5 mm and a single filament diameter of 10-13 μm.

5. The high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material according to claim 1, characterized in that: The composite halogen-free flame retardant is a mixture of coated ammonium polyphosphate, melamine polyphosphate, and organosilicon flame retardant synergist in a certain proportion.

6. The high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material according to claim 1, characterized in that: The high-whiteness composite pigment is a mixture of coated rutile titanium dioxide, nano zirconium silicate, ultrafine activated precipitated barium sulfate, and Honeywell AC-540A superdispersant in a certain proportion.

7. The high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material according to claim 1, characterized in that: The composite compatibilizer is a mixture of PP-g-MA, PA6-g-PP, and silane coupling agent KH-560 in a certain proportion.

8. The high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material according to claim 1, characterized in that: The stabilizer is an antioxidant, which may be one or more of N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexamethylenediamine (antioxidant 1098), tris[2,4-di-tert-butylphenyl]phosphite (antioxidant 168), and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (antioxidant 1010).

9. The high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material according to claim 1, characterized in that: The matrix resin, composite halogen-free flame retardant, and additives are mixed at high speed according to the specified ratio. Short-cut glass fibers are added from the side of the second barrel section, and high-whiteness composite color powder is added from the side of the sixth barrel section. The mixture is melt-blended using a twin-screw extruder with glass fiber side feeding, multi-stage vacuum devolatilization, and gradient temperature control at 210–250℃. After water cooling, pelletizing, and drying, the finished product is obtained. The resulting material has a cantilever beam notched impact strength ≥12.5kJ / m², a tensile strength ≥125MPa, and meets UL94 V-0 (1.6mm).

10. A high-whiteness glass fiber reinforced PA6 / PP halogen-free flame-retardant alloy material is used in electronic appliances, automotive interiors, and office equipment.