A flame-retardant encapsulating film, its preparation method, and a photovoltaic module.
By using a differentiated design on both the front and back sides and a phosphorus-nitrogen-silicon ternary composite flame-retardant system, the problem of balancing flame retardant performance and power generation performance in photovoltaic encapsulation films has been solved, resulting in films with high light transmittance and high flame retardant rating, thus improving long-term stability and power generation efficiency.
Patent Information
- Application Number
- CN202611504833.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing photovoltaic encapsulation films have shortcomings in balancing flame retardancy and power generation performance. Traditional flame retardants are unevenly dispersed and prone to migration and precipitation, resulting in insufficient long-term reliability. Furthermore, existing technologies do not fully utilize the functional differences between the front and back films, leading to low cost-effectiveness.
By adopting a differentiated flame-retardant design on the front and back sides, and combining a phosphorus-nitrogen-silicon ternary composite flame-retardant system, flame-retardant components are chemically bonded to the EVA matrix molecular chain through ester exchange grafting modification, and a light-receiving film on the front side and a backlight-receiving film on the back side are prepared to meet the requirements of high light transmittance and high flame-retardant performance, respectively.
It achieves UL94 V2 flame retardant performance while ensuring high light transmittance, and the back film can reach UL94 V0~5VA level, which improves the aging resistance and power generation efficiency of the film, simplifies the component assembly process, and reduces production costs.
Smart Images

Figure CN123107573A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photovoltaic encapsulation materials technology, and in particular to a flame-retardant encapsulation film, its preparation method, and a photovoltaic module. Background Technology
[0002] Photovoltaic encapsulation film is a key protective material for solar panels, typically using EVA or POE as the main material, both of which are flammable polymers. To improve the fire resistance of the modules, conventional flame-retardant technologies often involve adding high doses of flame retardants to the encapsulation film to achieve a UL94 V0 flame retardancy rating; some also use structural methods such as adding metal baffles to assist in flame retardancy. However, the above flame-retardant technologies still have the following drawbacks: Existing solutions typically require the front-side light-receiving film to also achieve a V0 flame retardancy rating. Since the core requirement for the front-side film is light transmission and power generation, the introduction of large amounts of flame retardants would significantly reduce light transmittance, directly impacting the module's power generation efficiency. This makes it impossible to simultaneously achieve both flame retardancy and power generation performance. Furthermore, current technologies generally do not fully utilize the functional differences between the front and back films. The back-side film has no light transmission restrictions, treating both sides equally and relying on a single film layer to complete all fire protection tasks. This lacks specificity, results in redundant flame retardant filling, and leads to low cost-effectiveness.
[0003] Traditional flame retardant processes mostly involve simple physical blending of flame retardant powder with EVA or POE particles followed by direct extrusion casting. This results in uneven dispersion of the powder within the matrix, leading to the formation of agglomerated particles and a high degree of haze on the cast film surface. Furthermore, the flame retardant is embedded in the polymer matrix solely through intermolecular forces, lacking chemical bond anchoring. Under harsh conditions such as long-term damp-heat aging and potential-induced degradation (PID), it is highly susceptible to migration and precipitation, causing the flame retardant effect to gradually diminish over service life and resulting in insufficient long-term reliability.
[0004] Existing single-component or binary compound flame-retardant systems have limited flame-retardant efficiency. To meet flame-retardant rating standards, it is necessary to further increase the filler content, which further deteriorates light transmittance and processability. Furthermore, the flame-retardant component cannot be stably anchored to the film substrate, exhibiting insufficient resistance to hydrolysis, precipitation, and aging. The flame-retardant effect gradually diminishes with long-term use of the component. The flame-retardant component remains at the level of simple physical doping, making it difficult to eliminate additive migration and interfacial failure.
[0005] In view of this, the present invention is hereby proposed. Summary of the Invention
[0006] The primary objective of this invention is to provide a flame-retardant encapsulating film that, through differentiated flame-retardant design on both sides, a phosphorus-nitrogen-silicon ternary synergistic flame-retardant system, and ester exchange grafting modification, ensures high light transmittance of the front light-receiving film while exhibiting excellent overall flame-retardant performance, and significantly improves the dispersion uniformity and long-term service stability of the flame-retardant components.
[0007] The second objective of this invention is to provide a method for preparing the above-mentioned flame-retardant encapsulating film.
[0008] A third objective of this invention is to provide a photovoltaic module.
[0009] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted: This invention provides a flame-retardant encapsulating film, comprising: a front light-receiving film and a back light-receiving film; The front light-receiving adhesive film, by weight, comprises the following raw materials: 100 parts of EVA resin, 4-15 parts of transparent flame-retardant masterbatch, and 1.25-2.84 parts of the first additive; The transparent flame-retardant masterbatch comprises, by weight, the following raw materials: 100 parts EVA resin, 5-8 parts phosphorus-based flame retardant, 3-5 parts nitrogen-based flame retardant, 2-4 parts silicone powder, 3-5 parts silane oligomer, 5-8 parts silane activator, 0.3-0.5 parts antioxidant, and 0.05-0.1 parts transesterification catalyst; The backlight adhesive film comprises, by weight, the following raw materials: 100 parts of EVA resin, 18-28 parts of high flame retardant masterbatch, and 1.75-5.84 parts of second additive; The high flame retardant masterbatch comprises, by weight, the following raw materials: 100 parts EVA resin, 60-80 parts phosphorus-based flame retardant, 5-8 parts nitrogen-based flame retardant, 4-6 parts silicone powder, 4-8 parts silane activator, 0.5-0.8 parts antioxidant, and 0.1-0.15 parts transesterification catalyst.
[0010] Furthermore, it includes at least one of the following features (1) to (4); (1) The phosphorus-based flame retardant includes aluminum diethylphosphonate and / or piperazine pyrophosphate; (2) The nitrogen-based flame retardant includes melamine cyanurate; (3) The silane activator includes KH570; (4) The transesterification catalyst includes zinc acetylacetonate.
[0011] Furthermore, in the raw materials of the transparent flame retardant masterbatch, the phosphorus-based flame retardant includes aluminum diethylphosphinate; And / or, in the raw materials of the high flame retardant masterbatch, the phosphorus-based flame retardant includes aluminum diethylphosphonate and piperazine pyrophosphate in a mass ratio of (30~40):(30~40).
[0012] Further, the first auxiliary agent, by mass parts, comprises the following components: Crosslinking agent 0.3~0.8 parts, co-crosslinking agent 0.4~0.8 parts, silane coupling agent 0.4~1 parts, antioxidant 0.1~0.15 parts and light stabilizer 0.05~0.09 parts.
[0013] Further, the second auxiliary agent, by mass parts, comprises the following components: The crosslinking agent consists of 0.3 to 0.8 parts, the co-crosslinking agent consists of 0.4 to 0.8 parts, the silane coupling agent consists of 0.4 to 3 parts, the acrylic monomer consists of 0.5 to 1 part, the antioxidant consists of 0.1 to 0.15 parts, and the light stabilizer consists of 0.05 to 0.09 parts.
[0014] Furthermore, it includes at least one of the following features (1) to (5); (1) The crosslinking agent includes TBEC; (2) The crosslinking agent includes TAIC; (3) The silane coupling agent includes KH570; (4) The thickness of the front light-receiving adhesive film is 0.4~0.5mm; (5) The thickness of the backlight adhesive film on the back is 0.4~0.5mm.
[0015] The present invention also provides a method for preparing the flame-retardant encapsulating film as described above, comprising the following steps: a. Premix the raw materials of the high flame retardant masterbatch. During the premixing process, a silane activator is sprayed in by atomization to obtain a mixture. The mixture is melt-extruded through a twin-screw extruder. Then, it is vacuum de-alcoholized, granulated, and dried to obtain the high flame retardant masterbatch. b. Premix the raw materials of the transparent flame retardant masterbatch. During the premixing process, the silane activator is sprayed in by atomization to obtain a mixture. The mixture is melt-extruded through a twin-screw extruder. Then, it is vacuum de-alcoholized, granulated, and dried to obtain the transparent flame retardant masterbatch. c. Mix the raw materials of the front-side light-receiving adhesive film to obtain a mixture; extrude the mixture through a twin-screw extruder to obtain the front-side light-receiving adhesive film; d. Mix the raw materials of the backlight adhesive film to obtain a mixture; extrude the mixture through a twin-screw extruder to obtain the backlight adhesive film.
[0016] Furthermore, it includes at least one of the following features (1) to (4); (1) In step a, the temperature of the premix is 50~65℃ and the time is 10~20min; (2) In step a, the temperature of the melt extrusion is 150~170℃; (3) In step b, the premixing temperature is 50~65℃ and the time is 10~15min; (4) In step b, the temperature of the melt extrusion is 150~165℃.
[0017] Furthermore, it includes at least one of the following features (1) to (4); (1) In step c, EVA resin and transparent flame retardant masterbatch are mixed at 50~65℃, and then the first additive is added and mixed for 0.5~1.5h to obtain a mixture; (2) In step c, the extrusion casting temperature is 85~95℃; (3) In step d, EVA resin and high flame retardant masterbatch are mixed at 50~65℃, and then the second additive is added and mixed for 0.5~1.5h to obtain a mixture; (4) In step d, the extrusion casting temperature is 90~105℃.
[0018] The present invention also provides a photovoltaic module, comprising a front cover plate, a front light-receiving film as described above, a photovoltaic cell array, a back light-receiving film as described above, and a rear cover plate stacked in sequence.
[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: The flame-retardant encapsulating film of this invention adopts a differentiated flame-retardant design on the front and back sides, combined with a phosphorus-nitrogen-silicon ternary compound flame-retardant system; the front light-receiving film uses a low-filler formulation, achieving UL94 V2 flame-retardant performance, with a small amount of flame retardant used, maintaining high light transmittance, and effectively ensuring the power generation efficiency of the module; the backlight film uses a high-filler formulation, achieving UL94 V0~5VA high flame-retardant performance; the front and back films work together to enable the whole to pass the UL94 V0 level combustion test, achieving a balance between flame-retardant performance and power generation performance.
[0020] The method for preparing the flame-retardant encapsulating film of the present invention uses a flame-retardant masterbatch pre-granulation and ester exchange grafting modification process to chemically bond the flame-retardant components to the EVA matrix molecular chain, effectively preventing migration and precipitation, improving the interfacial adhesion performance between the film and glass, and enhancing the film's aging resistance, PID resistance, and long-term damp heat aging stability. Attached Figure Description
[0021] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0022] Figure 1 This is a schematic diagram of the structure of the photovoltaic module of the present invention. Detailed Implementation
[0023] The technical solution of the present invention will be clearly and completely described below with reference to the accompanying drawings and specific embodiments. However, those skilled in the art will understand that the embodiments described below are some embodiments of the present invention, but not all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall be followed. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0024] In some embodiments of the present invention, a flame-retardant encapsulating film is provided, comprising: a front light-receiving film and a back light-receiving film; The front-side light-receiving adhesive film, by weight, comprises the following raw materials: 100 parts EVA resin, 4-15 parts transparent flame-retardant masterbatch, and 1.25-2.84 parts first additive; The transparent flame retardant masterbatch, by weight, comprises the following raw materials: 100 parts EVA resin, 5-8 parts phosphorus-based flame retardant, 3-5 parts nitrogen-based flame retardant, 2-4 parts silicone powder, 3-5 parts silane oligomer, 5-8 parts silane activator, 0.3-0.5 parts antioxidant, and 0.05-0.1 parts transesterification catalyst; The backlight adhesive film, by weight, includes the following raw materials: 100 parts of EVA resin, 18-28 parts of high flame retardant masterbatch, and 1.75-5.84 parts of second additives; The high flame retardant masterbatch, by weight, includes the following raw materials: 100 parts EVA resin, 60-80 parts phosphorus-based flame retardant, 5-8 parts nitrogen-based flame retardant, 4-6 parts silicone powder, 4-8 parts silane activator, 0.5-0.8 parts antioxidant, and 0.1-0.15 parts transesterification catalyst.
[0025] This invention employs a phosphorus-nitrogen-silicon ternary compound flame retardant system. The phosphorus-based flame retardant, nitrogen-based flame retardant, and silicon component work synergistically to rapidly form a dense, heat-insulating, oxygen-barrier, and expanding char layer during combustion, effectively suppressing molten droplet splashing and significantly improving flame retardant efficiency. The ternary synergistic effect allows for the achievement of a high flame retardant rating with a relatively low total filler content, avoiding the performance degradation caused by high filler content required by single or binary compound systems.
[0026] This invention employs a melt transesterification grafting reaction of EVA resin for chemical modification. Silane hydrolysis generates silanol groups, which undergo transesterification with acetate groups on the side chains of EVA molecules to form silanol chemical bonds. This covalently anchors the phosphorus, nitrogen, and silicon flame retardant components onto the EVA molecular chain, replacing the original physical blending mode that relies solely on intermolecular forces. This solves problems such as high-temperature precipitation of flame retardants, damp-heat blooming, and interfacial adhesion attenuation, and improves the hydrolysis resistance, PID resistance, and long-term damp-heat aging stability of the encapsulation film.
[0027] This invention addresses the issue of the lack of light transmission constraints on the backlight side by matching a high-content phosphorus, nitrogen, and silicon flame-retardant masterbatch formula. This allows a single back film to achieve an ultra-high flame-retardant rating of UL94 V0 or even 5VA. The rapid combustion of this film forms a dense, heat-insulating, and oxygen-barrier carbon layer, which serves as the core fire protection barrier for the component and inhibits the ignition of surrounding materials by molten droplets.
[0028] This invention differentiates the front light-receiving film and the back light-receiving film. The front light-receiving film achieves UL94V2 flame retardancy, reducing the amount of flame retardant added while maintaining high light transmittance and ensuring the power generation efficiency of the module. The back light-receiving film has no light transmittance restriction and can achieve UL94 V0~5VA flame retardancy ratings, serving as the main flame retardant barrier. The synergistic effect of the front and back films enables the entire module to pass the UL94 V0 combustion test, achieving a balance between flame retardancy and power generation performance.
[0029] This invention eliminates the need for additional fire protection structures, simplifies component assembly processes, controls production costs, and is adaptable to various high-fire-resistance application scenarios such as BIPV and rooftop photovoltaics.
[0030] In some embodiments of the present invention, the mass fraction of the transparent flame-retardant masterbatch in the raw material of the front light-receiving adhesive film can be 4 parts, 6 parts, 8 parts, 10 parts, 12 parts, 15 parts, and any value between any two of these; the mass fraction of the high flame-retardant masterbatch in the raw material of the back light-receiving adhesive film can be 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, and any value between any two of these; the mass fraction of the phosphorus-based flame retardant in the raw material of the high flame-retardant masterbatch can be 60 parts, 64 parts, 68 parts, 72 parts, 76 parts, 80 parts, and any value between any two of these.
[0031] In some embodiments of the present invention, the phosphorus-based flame retardant includes aluminum diethylphosphonate (ADP) and / or piperazine pyrophosphate (PPy).
[0032] In some embodiments of the present invention, the phosphorus-based flame retardant in the raw materials of the transparent flame retardant masterbatch includes aluminum diethylphosphonate (ADP).
[0033] In some embodiments of the present invention, the phosphorus-based flame retardant in the raw materials of the high flame retardant masterbatch includes aluminum diethylphosphonate (ADP) and piperazine pyrophosphate (PPy) in a mass ratio of (30~40):(30~40); typically, but not limitingly, for example, the mass ratio of aluminum diethylphosphonate (ADP) and piperazine pyrophosphate (PPy) can be 30:30, 30:40, 40:30 and any value between any two of them.
[0034] In some embodiments of the present invention, the nitrogen-based flame retardant includes melamine cyanurate (MCA).
[0035] In some embodiments of the present invention, the silane activator includes KH570.
[0036] In some embodiments of the present invention, the transesterification catalyst includes zinc acetylacetonate.
[0037] In some embodiments of the present invention, the antioxidants in the raw materials of transparent flame retardant masterbatch and high flame retardant masterbatch include, but are not limited to, antioxidant 1076.
[0038] In some embodiments of the present invention, the transparent flame-retardant masterbatch comprises, by weight parts, the following raw materials: 100 parts EVA resin, 5-8 parts aluminum diethylphosphinate (ADP), 3-5 parts melamine cyanurate (MCA), 2-4 parts silicone powder, 3-5 parts silane oligomer, 5-8 parts KH570, 0.3-0.5 parts antioxidant (preferably 0.4 parts antioxidant), and 0.05-0.1 parts zinc acetylacetone (preferably 0.08 parts zinc acetylacetone); wherein, ADP is the phosphorus source, MCA is the nitrogen source, and silicone powder, silane oligomer, and KH570 are silicon components.
[0039] The transparent flame-retardant masterbatch is used for the front-side light-receiving adhesive film and has a low phosphorus and high silicon ratio; zinc acetylacetonate is used to catalyze the transesterification reaction.
[0040] In some embodiments of the present invention, the high flame retardant masterbatch comprises, by weight parts, the following raw materials: 100 parts EVA resin, 30-40 parts aluminum diethylphosphonate (ADP), 30-40 parts piperazine pyrophosphate (PPy), 5-8 parts melamine cyanurate (MCA), 4-6 parts silicone powder, 4-8 parts KH570, 0.5-0.8 parts antioxidant (preferably 0.6 parts), and 0.1-0.15 parts zinc acetylacetonate (preferably 0.12 parts); wherein ADP and PPy are phosphorus sources, MCA is a nitrogen source, and silicone powder and KH570 are silicon components.
[0041] The high flame retardant masterbatch is used for the backlight adhesive film and has a high phosphorus-nitrogen ratio; zinc acetylacetonate is used to catalyze the transesterification reaction.
[0042] Aluminum diethylphosphonate (ADP) is a phosphorus-based halogen-free flame retardant. It decomposes upon heating to capture combustion free radicals and achieves gas-phase flame retardancy. At the same time, it catalyzes the dehydration of EVA to form char, and together with melamine cyanurate, it forms a phosphorus-nitrogen synergistic flame retardant system.
[0043] Melamine cyanurate (MCA) is a nitrogen-synergistic flame retardant. It decomposes endothermally at high temperatures and releases inert gas, which promotes the formation of an expanded char layer and inhibits dripping.
[0044] Piperazine pyrophosphate is a macromolecular intumescent phosphorus-nitrogen flame retardant component. When combined with ADP, it forms an intumescent flame retardant system, which enhances the heat insulation and barrier effect of the char layer.
[0045] Silicone powder, as an organosilicon synergist, improves powder dispersibility and forms a high-temperature resistant ceramic carbon layer during combustion, thus suppressing smoke and retardant flame.
[0046] Silane oligomers are low molecular weight polyorganosiloxanes prepared by controlled partial hydrolysis and polycondensation of alkoxysilane monomers. The molecules carry reactive silanol or alkoxy groups, and the number average molecular weight is 800~3000. They can participate in transesterification reactions, have lower volatility than small molecule silanes, and maintain the transparency of masterbatches.
[0047] KH570 is a silane-activated coupling agent that coats modified flame-retardant powders to improve interfacial compatibility.
[0048] Zinc acetylacetonate is a transesterification catalyst that promotes covalent grafting of silanol groups with EVA acetate bonds, reduces flame retardant precipitation, and does not induce EVA thermal degradation and yellowing. It is suitable for processing transparent flame retardant masterbatches. In some embodiments of the present invention, the first auxiliary agent, by weight parts, comprises the following components: Crosslinking agent 0.3~0.8 parts, co-crosslinking agent 0.4~0.8 parts, silane coupling agent 0.4~1 parts, antioxidant 0.1~0.15 parts and light stabilizer 0.05~0.09 parts.
[0049] In some embodiments of the present invention, the second auxiliary agent comprises, by weight parts, the following components: The crosslinking agent consists of 0.3 to 0.8 parts, the co-crosslinking agent consists of 0.4 to 0.8 parts, the silane coupling agent consists of 0.4 to 3 parts, the acrylic monomer consists of 0.5 to 1 part, the antioxidant consists of 0.1 to 0.15 parts, and the light stabilizer consists of 0.05 to 0.09 parts.
[0050] In some embodiments of the present invention, the crosslinking agent includes, but is not limited to, TBEC.
[0051] In some embodiments of the present invention, the crosslinking agent includes, but is not limited to, TAIC.
[0052] In some embodiments of the present invention, the silane coupling agent includes, but is not limited to, KH570.
[0053] In some embodiments of the present invention, antioxidants include, but are not limited to, antioxidant 1076.
[0054] In some embodiments of the present invention, the light stabilizer includes, but is not limited to, the light stabilizer UV770.
[0055] In some embodiments of the present invention, the front-facing light-receiving adhesive film comprises, by weight parts, the following raw materials: 100 parts EVA resin, 4-15 parts transparent flame retardant masterbatch, 0.3-0.8 parts crosslinking agent, 0.4-0.8 parts co-crosslinking agent, 0.4-1 parts silane coupling agent, 0.1-0.15 parts antioxidant and 0.05-0.09 parts light stabilizer.
[0056] In some embodiments of the present invention, the backlight adhesive film comprises, by weight parts, the following raw materials: 100 parts EVA resin, 18-28 parts high flame retardant masterbatch, 0.3-0.8 parts crosslinking agent, 0.4-0.8 parts co-crosslinking agent, 0.4-3 parts silane coupling agent, 0.5-1 parts acrylic monomer, 0.1-0.15 parts antioxidant and 0.05-0.09 parts light stabilizer.
[0057] This invention employs a differentiated flame-retardant design on both the front and back sides. The flame-retardant rating of the front light-receiving film reaches UL94 V2 level, with a low amount of flame retardant added and a light transmittance of over 90.5%, ensuring the power generation efficiency of the module. The back light-receiving film on the back side has no light transmittance restriction and can achieve an ultra-high flame-retardant rating of UL94 V0 or even 5VA, serving as the main flame-retardant barrier. The synergistic effect of the front and back films enables the entire module to pass the UL94 V0 level combustion test, achieving a balance between flame-retardant performance and power generation performance.
[0058] In some embodiments of the present invention, the flame retardant rating of the front light-receiving adhesive film is UL94 V2; the light transmittance of the front light-receiving adhesive film is 90.5%~92%.
[0059] In some embodiments of the present invention, the flame retardant rating of the backlight adhesive film is UL94 V0~5VA.
[0060] In some embodiments of the present invention, the overall flame retardancy rating of the front light-receiving adhesive film and the back light-receiving adhesive film is UL94 V0.
[0061] In some embodiments of the present invention, the adhesion force between the front light-receiving adhesive film and the glass is 95~140 N / cm.
[0062] In some embodiments of the present invention, the adhesion force between the backlight adhesive film on the back and the glass is 80~100 N / cm.
[0063] In some embodiments of the present invention, the degree of crosslinking of the front light-receiving adhesive film and the back light-receiving adhesive film is independently 80% to 90%.
[0064] In some embodiments of the present invention, the thickness of the photosensitive adhesive film on the front side is 0.4~0.5mm.
[0065] In some embodiments of the present invention, the thickness of the backlight adhesive film on the back side is 0.4~0.5mm.
[0066] In some embodiments of the present invention, a method for preparing the above-mentioned flame-retardant encapsulating film is also provided, comprising the following steps: a. Premix the raw materials of the high flame retardant masterbatch. During the premixing process, the silane activator is sprayed in by atomization to obtain a mixture. The mixture is melt-extruded through a twin-screw extruder. Then, it is vacuum de-alcoholized, granulated, and dried to obtain the high flame retardant masterbatch. b. Premix the raw materials of the transparent flame retardant masterbatch. During the premixing process, the silane activator is sprayed in by atomization to obtain a mixture. The mixture is melt-extruded through a twin-screw extruder. Then, it is vacuum de-alcoholized, granulated, and dried to obtain the transparent flame retardant masterbatch. c. Mix the raw materials of the front-side light-receiving adhesive film to obtain a mixture; extrude the mixture through a twin-screw extruder to obtain the front-side light-receiving adhesive film; d. Mix the raw materials of the backlight adhesive film to obtain a mixture; extrude the mixture through a twin-screw extruder to obtain the backlight adhesive film.
[0067] The preparation process of the differentiated flame-retardant encapsulating film of the present invention is divided into two parts: the first part is the preparation of a low-addition flame-retardant formulation for the front light-receiving film; the second part is the preparation of a high flame-retardant formulation for the back light-receiving film.
[0068] This invention first combines phosphorus, nitrogen, and silicon flame-retardant components with a silane activator, an ester exchange catalyst, and EVA resin through melt extrusion granulation to obtain a reactive phosphorus-nitrogen-silicon ternary flame-retardant masterbatch. During the masterbatch preparation stage, a preliminary ester exchange reaction occurs, where the silanol groups generated by silane hydrolysis react with the acetate bonds on the EVA side chains, preliminarily covalently grafting the flame-retardant components onto the EVA molecular chains. This solves the problems of direct powder blending and agglomeration, easy precipitation, and uneven dispersion.
[0069] Hydrolysis coating process: KH570 is sprayed into the phosphorus-nitrogen-silicon flame retardant powder system in an atomized manner. The trace amount of water vapor in the system promotes the hydrolysis of silane alkoxy groups to generate silanol groups Si-OH. The silanol groups dehydrate and condense with the hydroxyl groups on the powder surface to achieve inorganic powder coating.
[0070] Grafting principle: The reaction components are EVA side chain acetate groups, activated silane-carried methacrylate groups, silanol groups after silane hydrolysis, and active end groups of silane oligomers; zinc acetylacetone activates the carbonyl groups of EVA ester groups, and the active ester / hydroxyl groups on the silane undergo transesterification with the EVA ester groups, removing small molecule acetic acid derivatives, and covalently bonding the silicon-containing flame-retardant grafting sites to the EVA polymer backbone to achieve chemical grafting.
[0071] Secondary transesterification does not require the addition of transesterification catalyst; it relies on the residual transesterification catalyst within the masterbatch for continuous catalysis.
[0072] Since the front film needs to meet both high light transmittance and basic flame retardancy requirements, while the back film can use high flame retardancy additives without light transmittance restrictions, the two formulation systems are quite different. They need to be prepared by using corresponding flame retardant masterbatches for formulation and extrusion casting. During the casting process, secondary transesterification grafting modification is further carried out to strengthen the interface bonding between the flame retardant system and the EVA matrix. Then, deep transesterification anchoring is completed through module lamination (module lamination is a high temperature negative pressure environment with a lamination temperature of 140~150℃, which provides sufficient reaction temperature. The small amount of residual transesterification catalyst in the system can continue to promote the third transesterification). Finally, a synergistic flame retardant encapsulation structure is formed.
[0073] In some embodiments of the present invention, in step a, the premixing temperature is 50~65°C and the time is 10~20 min.
[0074] In some embodiments of the invention, in step a, the melt extrusion temperature is 150~170°C; typically, but not limitingly, for example, the melt extrusion temperature can be 150°C, 155°C, 160°C, 165°C, 170°C, and any value between any two of these.
[0075] In the preparation of high flame retardant masterbatch, the raw materials are premixed at 50~65℃. During the premixing process, silane is atomized and sprayed into the surface of the powder for hydrolysis and coating, forming a large number of Si-OH active hydroxyl groups. Then, the powder is extruded through a twin-screw extruder at 150~170℃ with high screw shear, and a preliminary transesterification reaction occurs, grafting the phosphorus-nitrogen-silicon flame retardant structure onto EVA resin. The powder is then de-alcoholized under vacuum, water-cooled, stretched, granulated, and dried to obtain a high-content phosphorus-nitrogen-silicon type flame retardant masterbatch.
[0076] In some embodiments of the present invention, in step b, the premixing temperature is 50~65°C and the time is 10~15 min.
[0077] In some embodiments of the invention, in step b, the melt extrusion temperature is 150~165°C; typically, but not limitingly, for example, the melt extrusion temperature can be 150°C, 155°C, 160°C, 165°C, and any value between any two of these.
[0078] In the preparation of transparent flame retardant masterbatch, the melt extrusion temperature is 150~165℃, and gentle transesterification is used to ensure high transparency and low haze of the masterbatch, which is then granulated for later use.
[0079] In some embodiments of the present invention, in step c, EVA resin and transparent flame retardant masterbatch are mixed at 50~65°C, and then the first additive is added and mixed for 0.5~1.5 hours to obtain a mixture.
[0080] In some embodiments of the present invention, in step c, the extrusion casting temperature is 85~95°C.
[0081] In the preparation of the front-side light-receiving adhesive film, EVA and transparent flame-retardant masterbatch are mixed at 50~65℃, and the masterbatch is uniformly dispersed; the first auxiliary agent is added and the mixture is mixed again; then it is extruded and cast through a twin-screw extruder at 85~95℃; during the extrusion process, the residual Si-OH continuously undergoes secondary transesterification with EVA acetate, further anchoring the flame-retardant components. The adhesive film has low haze, light transmittance ≥90.5%, and flame retardant rating of UL94 V2.
[0082] In some embodiments of the present invention, in step d, EVA resin and high flame retardant masterbatch are mixed at 50~65°C, and then a second additive is added and mixed for 0.5~1.5h to obtain a mixture.
[0083] In some embodiments of the present invention, in step d, the extrusion casting temperature is 90~105°C.
[0084] In the preparation process of the backlight adhesive film, EVA and high flame retardant masterbatch are mixed at 50~65℃; a second auxiliary agent is added and mixing is continued; then it is extruded and cast through a twin-screw extruder at 90~105℃; phosphorus, nitrogen and silicon components are pre-grafted in the masterbatch, and further ester exchange is carried out during the casting stage. During combustion, a silicon-modified expanded carbon layer is quickly formed, and the flame retardant rating of a single film can reach UL94 V0~5VA.
[0085] See Figure 1 In some embodiments of the present invention, a photovoltaic module is also provided, comprising a front cover plate, the aforementioned front light-receiving adhesive film, a photovoltaic cell array, the aforementioned back light-receiving adhesive film, and a rear cover plate stacked sequentially; preferably, the front cover plate comprises front cover plate photovoltaic patterned glass; and the rear cover plate comprises rear cover plate glass.
[0086] The photovoltaic module of this invention is arranged in a stacked manner from top to bottom: a front cover photovoltaic patterned glass, a front light-receiving encapsulating film, a photovoltaic cell array, a back light-receiving encapsulating film, and a rear cover glass. The entire stacked structure is integrally cured and formed by a vacuum hot-pressing process (negative pressure environment, temperature of 140~150℃) to form a double-glass flame-retardant photovoltaic module. Among them, the front light-receiving encapsulating film is a low-filler, high-transmittance flame-retardant film that has been diluted with flame-retardant masterbatch and modified by ester exchange grafting; the back light-receiving encapsulating film is prepared using a high-content phosphorus-nitrogen-silicon reactive flame-retardant masterbatch.
[0087] When a photovoltaic module encounters a fire source, the front-side light-receiving film slows down the initial spread of the flame and prevents the flame from quickly penetrating the solar cells; the back-side backlighting film quickly forms a dense carbon layer under heat conduction, blocking oxygen and heat transfer, and preventing the molten film drips from igniting surrounding materials; the two work together to enable the module to pass the UL94 V0 level flammability test, meeting the high fire resistance requirements without sacrificing the light transmittance of the front-side film.
[0088] In some embodiments of the present invention, the overall flame retardant rating of the photovoltaic module is UL94 V0.
[0089] In some embodiments of the present invention, the power degradation rate of the photovoltaic module is 0.5%~4.5% for DH 2000h, the power degradation rate is 0.5%~2.9% for PID192h, and the overall power is 360~375W.
[0090] In some embodiments of the present invention, a method for preparing the above-mentioned photovoltaic module is also provided, comprising the following steps: The front cover plate, the front light-receiving adhesive film, the photovoltaic cell array, the back light-receiving adhesive film, and the rear cover plate are stacked sequentially from top to bottom, and then integrally cured by vacuum hot pressing at 140~150℃ for 10~20 minutes to obtain a photovoltaic module.
[0091] Example 1 The method for preparing the flame-retardant encapsulating film provided in this embodiment includes the following steps: a. Add 100 parts of EVA resin, 40 parts of aluminum diethylphosphinate (ADP), 30 parts of piperazine pyrophosphate (PPy), 8 parts of melamine cyanurate (MCA), 6 parts of silicone powder, 8 parts of KH570, 0.6 parts of antioxidant 1076, and 0.12 parts of zinc acetylacetonate to a high-speed mixer and mix at 65°C for 15 minutes. During the mixing process, atomize KH570 and spray it onto the surface of the powder for hydrolysis and coating to obtain a mixture. Melt-extrude the mixture through a twin-screw extruder at 160°C, and then vacuum degassing and de-alcoholizing, water-cooled granulation, and drying to obtain a high flame-retardant masterbatch.
[0092] b. Add 100 parts of EVA resin, 8 parts of aluminum diethylphosphinate (ADP), 5 parts of melamine cyanurate (MCA), 4 parts of silicone powder, 3 parts of silane oligomer, 5 parts of KH570, 0.4 parts of antioxidant 1076, and 0.08 parts of zinc acetylacetonate to a high-speed mixer and mix at 65°C for 15 minutes. During the mixing process, atomize KH570 and spray it onto the surface of the powder for hydrolysis and coating to obtain a mixture. Melt-extrude the mixture through a twin-screw extruder at 155°C, and then vacuum de-alcoholize, water-cooled, granulated, and dried to obtain a transparent flame-retardant masterbatch.
[0093] c. Mix 100 parts of EVA resin and 6 parts of transparent flame retardant masterbatch at 60°C for 10 min; then add 0.8 parts of TBEC, 0.5 parts of TAIC, 0.4 parts of KH570, 0.1 parts of antioxidant 1076, and 0.08 parts of light stabilizer UV770 and mix for 1 h to obtain a mixture; extrude the mixture through a twin-screw extruder at 90°C to obtain a light-receiving film with a thickness of 0.5 mm on the front side.
[0094] d. Mix 100 parts of EVA resin and 24 parts of high flame retardant masterbatch at 65°C for 15 min; then add 0.8 parts of TBEC, 0.5 parts of TAIC, 0.4 parts of KH570, 1 part of acrylic monomer, 0.1 parts of antioxidant 1076, and 0.08 parts of light stabilizer UV770 and mix for 1 h to obtain a mixture; extrude the mixture through a twin-screw extruder at 100°C to obtain a backlight film with a thickness of 0.5 mm.
[0095] The photovoltaic module manufacturing method provided in this embodiment includes the following steps: The photovoltaic patterned glass front cover, the aforementioned front light-receiving adhesive film, the photovoltaic cell array, the aforementioned back light-receiving adhesive film, and the rear cover glass are stacked sequentially from top to bottom, and then integrally cured by vacuum hot pressing at 140°C for 15 minutes to obtain a photovoltaic module.
[0096] This embodiment includes performance testing of the flame-retardant encapsulating film and photovoltaic module: Flame retardant performance testing was conducted in accordance with UL94 2023, "Tests for flammability of plastics for use in equipment and electrical components".
[0097] Multiple layers of the front-side light-receiving adhesive film were hot-pressed together to form a homogeneous board, which was then cut into strips measuring 125mm × 13mm × 3.0mm for vertical burning tests. A 20mm flame was used, applied twice for 10 seconds each time. The afterflame burning times after the two applications were 24s and 25s, respectively (single afterflame burning time ≤ 30s). The sample produced molten drips, which did not ignite the degreased cotton underneath, indicating that the sample's flame retardant performance reached V2 level. Multiple layers of the back-side light-receiving adhesive film were hot-pressed together to form a homogeneous board, which was then cut into strips measuring 125mm × 13mm × 3.0mm. After completing the V1 level test, a 500W (5V) flame resistance test was conducted. The flame was applied for 5 seconds each time, with a 5-second interval between flame removals, and the ignition cycle was repeated 5 times. The sample showed no through-burning, no continuous burning, and the burning drips did not ignite the degreased cotton, indicating that the sample's flame retardant performance reached 5VA level. The above-mentioned composite board samples are used to characterize the intrinsic flame retardant properties of the formulation system, and are not equivalent to the VTM flame retardant rating of a single-layer finished adhesive film.
[0098] The front light-receiving adhesive film and the back light-receiving adhesive film were laminated and pressed into a 125mm×13mm×3mm composite strip. A flame was applied to the front light-receiving adhesive film side, and the flame was applied twice for 10 seconds. The flame could not burn through the entire composite structure, there was no continuous spread of open flame, and a few droplets did not ignite the degreased cotton. The overall flame retardancy rating of the front light-receiving adhesive film and the back light-receiving adhesive film was determined to be V0.
[0099] The degree of crosslinking of the adhesive film was tested according to GB / T 29848-2018; the adhesive strength was tested according to GB / T 29848-2018; and the light transmittance was measured using a Shimadzu UV-2600 ultraviolet spectrophotometer.
[0100] The cross-linking degree of the front light-receiving adhesive film is 85.2%, and the adhesion strength between the front light-receiving adhesive film and the glass is 134 N / cm; the cross-linking degree of the back light-receiving adhesive film is 82.7%, and the adhesion strength between the back light-receiving adhesive film and the glass is 88 N / cm; the light transmittance of the front light-receiving adhesive film is 91.6%.
[0101] The initial power of the photovoltaic module is measured according to GB / T 9535.1-2022, the DH 2000h power degradation rate of the photovoltaic module is measured according to GB / T 9535.2-2022, and the PID 192h power degradation rate of the photovoltaic module is measured according to IEC TS 62804 1:2025.
[0102] The initial power of the photovoltaic module is 367W; the power degradation rate of the photovoltaic module DH 2000h is 2.8%, the power degradation rate of the photovoltaic module PID 192h is 1.8%; the leaching rate of the flame retardant extracted by toluene 24h is 2.1%.
[0103] Example 2 The method for preparing the flame-retardant encapsulating film provided in this embodiment includes the following steps: a. Add 100 parts of EVA resin, 30 parts of aluminum diethylphosphinate (ADP), 30 parts of piperazine pyrophosphate (PPy), 8 parts of melamine cyanurate (MCA), 6 parts of silicone powder, 8 parts of KH570, 0.6 parts of antioxidant 1076, and 0.12 parts of zinc acetylacetonate to a high-speed mixer and mix at 65°C for 15 minutes. During the mixing process, atomize KH570 and spray it onto the surface of the powder for hydrolysis and coating to obtain a mixture. Melt extrude the mixture at 150°C using a twin-screw extruder, and then vacuum de-alcoholize, water-cooled, granulated, and dried to obtain a high flame-retardant masterbatch.
[0104] b. Add 100 parts of EVA resin, 8 parts of aluminum diethylphosphinate (ADP), 5 parts of melamine cyanurate (MCA), 4 parts of silicone powder, 3 parts of silane oligomer, 5 parts of KH570, 0.4 parts of antioxidant 1076, and 0.08 parts of zinc acetylacetonate to a high-speed mixer and mix at 65°C for 15 minutes. During the mixing process, KH570 is atomized and sprayed onto the surface of the powder for hydrolysis and coating to obtain a mixture. The mixture is melt-extruded at 150°C using a twin-screw extruder, and then subjected to vacuum degassing and de-alcoholization, water-cooled granulation, and drying to obtain a transparent flame-retardant masterbatch.
[0105] c. Mix 100 parts of EVA resin and 15 parts of transparent flame retardant masterbatch at 60°C for 10 min; then add 0.8 parts of TBEC, 0.5 parts of TAIC, 0.4 parts of KH570, 0.1 parts of antioxidant 1076, and 0.08 parts of light stabilizer UV770 and mix for 1 h to obtain a mixture; extrude the mixture through a twin-screw extruder at 90°C to obtain a light-receiving film with a thickness of 0.5 mm on the front side.
[0106] d. Mix 100 parts of EVA resin and 28 parts of high flame retardant masterbatch at 65°C for 15 min; then add 0.8 parts of TBEC, 0.5 parts of TAIC, 0.4 parts of KH570, 1 part of acrylic monomer, 0.1 parts of antioxidant 1076, and 0.08 parts of light stabilizer UV770 and mix for 1 h to obtain a mixture; extrude the mixture through a twin-screw extruder at 100°C to obtain a backlight film with a thickness of 0.5 mm.
[0107] The photovoltaic module manufacturing method provided in this embodiment includes the following steps: The photovoltaic patterned glass front cover, the aforementioned front light-receiving adhesive film, the photovoltaic cell array, the aforementioned back light-receiving adhesive film, and the rear cover glass are stacked sequentially from top to bottom, and then integrally cured by vacuum hot pressing at 140°C for 15 minutes to obtain a photovoltaic module.
[0108] This embodiment demonstrates the performance testing of the flame-retardant encapsulating film and photovoltaic modules. The testing methods are the same as in Embodiment 1. The flame retardant rating of the front light-receiving adhesive film is V2; the flame retardant rating of the back light-receiving adhesive film is V0; the overall flame retardant rating of the front light-receiving adhesive film and the back light-receiving adhesive film is V0.
[0109] The cross-linking degree of the front light-receiving adhesive film is 81.2%, and the adhesion strength between the front light-receiving adhesive film and the glass is 97 N / cm; the cross-linking degree of the back light-receiving adhesive film is 80.5%, and the adhesion strength between the back light-receiving adhesive film and the glass is 81 N / cm; the light transmittance of the front light-receiving adhesive film is 90.5%.
[0110] The initial power of the photovoltaic module is 361W; the power degradation rate of the photovoltaic module DH 2000h is 3.3%, and the power degradation rate of the photovoltaic module PID 192h is 2.5%; the leaching rate of the toluene-extracted flame retardant is 2.0% after 24h.
[0111] Example 3 The method for preparing the flame-retardant encapsulating film provided in this embodiment includes the following steps: a. Add 100 parts of EVA resin, 30 parts of aluminum diethylphosphinate (ADP), 30 parts of piperazine pyrophosphate (PPy), 5 parts of melamine cyanurate (MCA), 4 parts of silicone powder, 4 parts of KH570, 0.6 parts of antioxidant 1076, and 0.12 parts of zinc acetylacetonate to a high-speed mixer and mix at 65°C for 15 minutes. During the mixing process, atomize KH570 and spray it onto the surface of the powder for hydrolysis and coating to obtain a mixture. Melt extrude the mixture at 160°C using a twin-screw extruder, and then vacuum de-alcoholize, water-cooled, granulated, and dried to obtain a high flame-retardant masterbatch.
[0112] b. Add 100 parts of EVA resin, 5 parts of aluminum diethylphosphinate (ADP), 3 parts of melamine cyanurate (MCA), 2 parts of silicone powder, 3 parts of silane oligomer, 5 parts of KH570, 0.4 parts of antioxidant 1076, and 0.08 parts of zinc acetylacetonate to a high-speed mixer and mix at 65°C for 15 minutes. During the mixing process, KH570 is atomized and sprayed onto the surface of the powder for hydrolysis and coating to obtain a mixture. The mixture is melt-extruded at 160°C using a twin-screw extruder, and then subjected to vacuum degassing and de-alcoholization, water-cooled granulation, and drying to obtain a transparent flame-retardant masterbatch.
[0113] c. Mix 100 parts of EVA resin and 12 parts of transparent flame retardant masterbatch at 60℃ for 10 min; then add 0.8 parts of TBEC, 0.5 parts of TAIC, 0.4 parts of KH570, 0.1 parts of antioxidant 1076 and 0.08 parts of light stabilizer UV770 and mix for 1 h to obtain a mixture; extrude the mixture through a twin-screw extruder at 95℃ to obtain a light-receiving film with a thickness of 0.5 mm on the front.
[0114] d. Mix 100 parts of EVA resin and 28 parts of high flame retardant masterbatch at 65°C for 15 min; then add 0.8 parts of TBEC, 0.5 parts of TAIC, 0.4 parts of KH570, 1 part of acrylic monomer, 0.1 parts of antioxidant 1076, and 0.08 parts of light stabilizer UV770 and mix for 1 h to obtain a mixture; extrude the mixture through a twin-screw extruder at 95°C to obtain a backlight film with a thickness of 0.5 mm.
[0115] The photovoltaic module manufacturing method provided in this embodiment includes the following steps: The photovoltaic patterned glass front cover, the aforementioned front light-receiving adhesive film, the photovoltaic cell array, the aforementioned back light-receiving adhesive film, and the rear cover glass are stacked sequentially from top to bottom, and then integrally cured by vacuum hot pressing at 140°C for 15 minutes to obtain a photovoltaic module.
[0116] The performance testing methods for the flame-retardant encapsulating film and photovoltaic module in this embodiment are the same as those in Embodiment 1. The flame retardant rating of the front light-receiving adhesive film is V2; the flame retardant rating of the back light-receiving adhesive film is V0; the overall flame retardant rating of the front light-receiving adhesive film and the back light-receiving adhesive film is V0.
[0117] The cross-linking degree of the front light-receiving adhesive film is 82.4%, and the adhesion strength between the front light-receiving adhesive film and the glass is 112 N / cm; the cross-linking degree of the back light-receiving adhesive film is 80.9%, and the adhesion strength between the back light-receiving adhesive film and the glass is 87 N / cm; the light transmittance of the front light-receiving adhesive film is 90.8%.
[0118] The initial power of the photovoltaic module is 365W; the power degradation rate of the photovoltaic module DH 2000h is 3.0%, and the power degradation rate of the photovoltaic module PID 192h is 2.0%; the leaching rate of the flame retardant extracted by toluene in 24h is 2.5%.
[0119] Comparative Example 1 The method for preparing the flame-retardant encapsulating film provided in this comparative example includes the following steps: 100 parts of EVA resin, 8 parts of aluminum diethylphosphinate (ADP), 5 parts of melamine cyanurate (MCA), 4 parts of silicone powder, 3 parts of silane oligomer, 5 parts of KH570, 0.4 parts of antioxidant 1076, and 0.08 parts of zinc acetylacetonate were mixed at 65°C for 10 min. Then, 0.8 parts of TBEC, 0.5 parts of TAIC, 0.4 parts of KH570, 0.1 parts of antioxidant 1076, and 0.08 parts of light stabilizer UV770 were added and mixed for 1 h to obtain a mixture. The mixture was then extruded and cast using a twin-screw extruder at 90°C to obtain a light-receiving film with a thickness of 0.5 mm on the front side.
[0120] 100 parts of EVA resin, 40 parts of aluminum diethylphosphonate (ADP), 30 parts of piperazine pyrophosphate (PPy), 8 parts of melamine cyanurate (MCA), 6 parts of silicone powder, 8 parts of KH570, 0.6 parts of antioxidant 1076, and 0.12 parts of zinc acetylacetonate were mixed at 65°C for 15 min. Then, 0.8 parts of TBEC, 0.5 parts of TAIC, 0.4 parts of KH570, 1 part of acrylic monomer, 0.1 parts of antioxidant 1076, and 0.08 parts of light stabilizer UV770 were added and mixed for 1 h to obtain a mixture. The mixture was then extruded and cast using a twin-screw extruder at 100°C to obtain a backlight film with a thickness of 0.5 mm.
[0121] The method for preparing the photovoltaic module provided in this comparative example is based on Example 1.
[0122] This comparative study demonstrates the performance testing of flame-retardant encapsulating film and photovoltaic modules. The test methods are as described in Example 1. The flame retardant rating of the front light-receiving adhesive film is V2; the flame retardant rating of the back light-receiving adhesive film is V1; the overall flame retardant rating of the front light-receiving adhesive film and the back light-receiving adhesive film is V1.
[0123] The cross-linking degree of the front light-receiving adhesive film is 82.4%, and the adhesion strength between the front light-receiving adhesive film and the glass is 128 N / cm; the cross-linking degree of the back light-receiving adhesive film is 78.3%, and the adhesion strength between the back light-receiving adhesive film and the glass is 94 N / cm; the light transmittance of the front light-receiving adhesive film is 88.3%.
[0124] The initial power of the photovoltaic module was 342W; the power degradation rate of the photovoltaic module after DH 2000h was 3.9%, and there was obvious blooming on the surface; the power degradation rate of the photovoltaic module after PID 192h was 2.3%. The leaching rate of the flame retardant extracted with toluene after 24h was 10.3%.
[0125] Comparative Example 2 The preparation method of the flame-retardant encapsulating film provided in this comparative example is the same as that in Example 1, the only difference is that silicone powder was not added in step a; and silicone powder and silane oligomer were not added in step b.
[0126] The method for preparing the photovoltaic module provided in this comparative example is based on Example 1.
[0127] This comparative study demonstrates the performance testing of flame-retardant encapsulating film and photovoltaic modules. The test methods are as described in Example 1. The flame retardant rating of the front light-receiving adhesive film is V2; the flame retardant rating of the back light-receiving adhesive film is V1; the overall flame retardant rating of the front light-receiving adhesive film and the back light-receiving adhesive film is V1; combustion produces a large number of molten droplets, and the smoke density increases significantly.
[0128] The cross-linking degree of the front light-receiving adhesive film is 83.2%, and the adhesion strength between the front light-receiving adhesive film and the glass is 118 N / cm; the cross-linking degree of the back light-receiving adhesive film is 81.4%, and the adhesion strength between the back light-receiving adhesive film and the glass is 87 N / cm; the light transmittance of the front light-receiving adhesive film is 90.9%.
[0129] The initial power of the photovoltaic module was 363W; the power degradation rate of the photovoltaic module over DH 2000h was 3.5%; the power degradation rate of the photovoltaic module over PID 192h was 2%. The leaching rate of the flame retardant extracted with toluene over 24h was 5.7%.
[0130] Comparative Example 3 The preparation method of the flame-retardant encapsulating film provided in this comparative example is the same as that in Example 1, zinc acetylacetone was not added in step a; and zinc acetylacetone was not added in step b.
[0131] The method for preparing the photovoltaic module provided in this comparative example is based on Example 1.
[0132] This comparative study demonstrates the performance testing of flame-retardant encapsulating film and photovoltaic modules. The test methods are as described in Example 1. The flame retardant rating of the front light-receiving adhesive film is V2; the flame retardant rating of the back light-receiving adhesive film is V1; the overall flame retardant rating of the front light-receiving adhesive film and the back light-receiving adhesive film is V1.
[0133] The cross-linking degree of the front light-receiving adhesive film is 83.1%, and the adhesion strength between the front light-receiving adhesive film and the glass is 101 N / cm; the cross-linking degree of the back light-receiving adhesive film is 79.8%, and the adhesion strength between the back light-receiving adhesive film and the glass is 72 N / cm; the light transmittance of the front light-receiving adhesive film is 89.5%.
[0134] The initial power of the photovoltaic module was 349W; the power degradation rate of the photovoltaic module after DH 2000h was 5.2%, and a large amount of flame retardant was released after damp heat aging; the power degradation rate of the photovoltaic module after PID 192h was 3.4%. The flame retardant dissolution rate extracted by toluene after 24h was 15.2%.
[0135] Comparative Example 4 The method for preparing the flame-retardant encapsulating film provided in this comparative example includes the following steps: 100 parts of EVA resin, 20 parts of aluminum diethylphosphonate (ADP), and 10 parts of melamine cyanurate (MCA) were mixed at 65°C for 10 min. Then, 0.8 parts of TBEC, 0.5 parts of TAIC, 0.4 parts of KH570, 0.1 parts of antioxidant 1076, and 0.08 parts of light stabilizer UV770 were added and mixed for 1 h to obtain a mixture. The mixture was then extruded and cast using a twin-screw extruder at 90°C to obtain a light-receiving film with a thickness of 0.5 mm on the front side.
[0136] 100 parts of EVA resin, 20 parts of aluminum diethylphosphonate (ADP), and 10 parts of melamine cyanurate (MCA) were mixed at 65°C for 10 min. Then, 0.8 parts of TBEC, 0.5 parts of TAIC, 0.4 parts of KH570, 1 part of acrylic monomer, 0.1 parts of antioxidant 1076, and 0.08 parts of light stabilizer UV770 were added and mixed for 1 h to obtain a mixture. The mixture was then extruded and cast using a twin-screw extruder at 90°C to obtain a backlight film with a thickness of 0.5 mm.
[0137] This comparative study demonstrates the performance testing of flame-retardant encapsulating film and photovoltaic modules. The test methods are as described in Example 1. The flame retardant rating of the front light-receiving adhesive film is V1; the flame retardant rating of the back light-receiving adhesive film is V1; the overall flame retardant rating of the front light-receiving adhesive film and the back light-receiving adhesive film is V1.
[0138] The crosslinking degree of the front light-receiving adhesive film is <75%, and the peel strength between the front light-receiving adhesive film and the glass is <80N / cm; the crosslinking degree of the back light-receiving adhesive film is <75%, and the peel strength between the back light-receiving adhesive film and the glass is <80N / cm; the light transmittance of the front light-receiving adhesive film is 74.4%.
[0139] The photovoltaic module's initial power was 323W, but it experienced a significant drop in power; bonding failure occurred after aging. The photovoltaic module's power degradation rate after DH2000h was >10%, with a large amount of flame retardant leaching after damp heat aging; the photovoltaic module's power degradation rate after PID192h was >10%. The toluene-extracted flame retardant dissolution rate after 24h was >15%.
[0140] Test case The performance of the encapsulant film and photovoltaic modules of Examples 1-3 and Comparative Examples 1-4 was tested, and the results are shown in Tables 1, 2 and 3.
[0141] Flame retardancy rating: Refer to UL94-2023 "Test for flammability of plastics for equipment and electrical components"; the front light-receiving adhesive film is pressed into a 125mm×13mm×3.0mm sample for flame retardancy rating test; the back light-receiving adhesive film is pressed into a 125mm×13mm×3.0mm sample for flame retardancy rating test; the front light-receiving adhesive film and the back light-receiving adhesive film are laminated together to form a 125mm×13mm×3.0mm sample for overall flame retardancy rating test.
[0142] Transmittance: Measured by Shimadzu UV-2600 ultraviolet spectrophotometer.
[0143] Crosslinking degree: The crosslinking degree of the film was tested according to GB / T 29848-2018. The film was cut into particles smaller than 3mm × 3mm, and 0.50g ± 0.01g was weighed. The particles were placed in a stainless steel wire mesh bag to obtain the sample. The sample was extracted with xylene at 140℃ for 5h under reflux. After extraction, it was vacuum dried to constant weight, cooled and weighed, and then measured according to D. The crosslinking degree is calculated as ×100%, where W1 is the mass of the empty stainless steel wire mesh bag, W2 is the total mass of the sample before extraction, and W3 is the total mass of the sample after extraction. Three parallel samples are used, and the average value is taken.
[0144] The adhesion strength between the film and glass is measured according to GB / T 29848-2018, the initial power of the photovoltaic module is measured according to GB / T 9535.1-2022, the power degradation rate of the photovoltaic module DH 2000h is measured according to GB / T 9535.2-2022, and the power degradation rate of the photovoltaic module PID 192h is measured according to IEC TS 62804-1:2025.
[0145] Flame retardant dissolution rate: Toluene extraction for 24 hours. The flame retardant dissolution rate was determined using a Soxhlet extraction test with toluene: A sample film was taken, cut into 20mm × 20mm pieces, surface dust was wiped off with lint-free paper, and the sample was dried in a vacuum oven at 60℃ for 2 hours. After drying, the sample was removed and placed in a desiccator to cool to room temperature. The sample was weighed and recorded as the initial mass m0. The sample was placed in a Soxhlet extractor, toluene solvent was added, and the mixture was heated to maintain reflux for 24 hours. After extraction, the film sample was removed, and the surface was rinsed with a small amount of fresh toluene. The rinsed film sample was dried in a vacuum oven at 60℃ to constant weight, cooled, and weighed. All extract and rinsing liquid were collected, combined, and then removed by rotary evaporation. The resulting residue was dried in a vacuum oven at 60℃ to constant weight and weighed to obtain the total extract mass m0. 总萃 Blank films were prepared with identical raw materials, processing techniques, and crosslinking conditions except for the absence of flame-retardant components. Parallel tests were conducted using identical Soxhlet extraction conditions to obtain the dissolution mass m of the blank films under these conditions. 空白溶胶 Flame retardant dissolution rate (%) Method Description: When the degree of crosslinking of the film is less than 100%, a small amount of uncrosslinked linear EVA sol will be dissolved during the toluene extraction process. This method uses a blank film of the same process to test and deducts the mass contribution of EVA sol to obtain the total amount of flame retardant dissolved, which is used to evaluate the overall migration and dissolution performance of the composite flame retardant system.
[0146] Table 1
[0147] Table 2
[0148] Table 3
[0149] Although the present invention has been illustrated and described with specific embodiments, it should be understood that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; those skilled in the art should understand that modifications can be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein, without departing from the spirit and scope of the present invention; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention; therefore, this means that all such substitutions and modifications that fall within the scope of the present invention are included in the appended claims.
Claims
1. A flame-retardant encapsulating film, characterized in that, include: Front-facing light-receiving adhesive film and back-facing light-receiving adhesive film; The front-side light-receiving adhesive film comprises, by weight, the following raw materials: 100 parts EVA resin, 4-15 parts transparent flame retardant masterbatch, and 1.25-2.84 parts first additive; The transparent flame-retardant masterbatch comprises, by weight, the following raw materials: 100 parts EVA resin, 5-8 parts phosphorus-based flame retardant, 3-5 parts nitrogen-based flame retardant, 2-4 parts silicone powder, 3-5 parts silane oligomer, 5-8 parts silane activator, 0.3-0.5 parts antioxidant, and 0.05-0.1 parts transesterification catalyst; The backlight adhesive film comprises, by weight, the following raw materials: 100 parts of EVA resin, 18-28 parts of high flame retardant masterbatch, and 1.75-5.84 parts of second additive; The high flame retardant masterbatch comprises, by weight, the following raw materials: 100 parts EVA resin, 60-80 parts phosphorus-based flame retardant, 5-8 parts nitrogen-based flame retardant, 4-6 parts silicone powder, 4-8 parts silane activator, 0.5-0.8 parts antioxidant, and 0.1-0.15 parts transesterification catalyst.
2. The flame-retardant encapsulating film according to claim 1, characterized in that, Includes at least one of the following features (1) to (4); (1) The phosphorus-based flame retardant includes aluminum diethylphosphonate and / or piperazine pyrophosphate; (2) The nitrogen-based flame retardant includes melamine cyanurate; (3) The silane activator includes KH570; (4) The transesterification catalyst includes zinc acetylacetonate.
3. The flame-retardant encapsulating film according to claim 2, characterized in that, In the raw materials of the transparent flame retardant masterbatch, the phosphorus-based flame retardant includes aluminum diethylphosphinate; And / or, in the raw materials of the high flame retardant masterbatch, the phosphorus-based flame retardant includes aluminum diethylphosphonate and piperazine pyrophosphate in a mass ratio of (30~40):(30~40).
4. The flame-retardant encapsulating film according to claim 1, characterized in that, The first auxiliary agent comprises, by mass parts, the following components: Crosslinking agent 0.3~0.8 parts, co-crosslinking agent 0.4~0.8 parts, silane coupling agent 0.4~1 parts, antioxidant 0.1~0.15 parts and light stabilizer 0.05~0.09 parts.
5. The flame-retardant encapsulating film according to claim 1, characterized in that, The second auxiliary agent, by mass parts, comprises the following components: The crosslinking agent consists of 0.3 to 0.8 parts, the co-crosslinking agent consists of 0.4 to 0.8 parts, the silane coupling agent consists of 0.4 to 3 parts, the acrylic monomer consists of 0.5 to 1 part, the antioxidant consists of 0.1 to 0.15 parts, and the light stabilizer consists of 0.05 to 0.09 parts.
6. The flame-retardant encapsulating film according to claim 4 or 5, characterized in that, Includes at least one of the following features (1) to (5); (1) The crosslinking agent includes TBEC; (2) The crosslinking agent includes TAIC; (3) The silane coupling agent includes KH570; (4) The thickness of the front light-receiving adhesive film is 0.4~0.5mm; (5) The thickness of the backlight adhesive film on the back is 0.4~0.5mm.
7. The method for preparing the flame-retardant encapsulating film according to any one of claims 1 to 6, characterized in that, Includes the following steps: a. Premix the raw materials of the high flame retardant masterbatch. During the premixing process, a silane activator is sprayed in by atomization to obtain a mixture. The mixture is melt-extruded through a twin-screw extruder. Then, it is vacuum de-alcoholized, granulated, and dried to obtain the high flame retardant masterbatch. b. Premix the raw materials of the transparent flame retardant masterbatch. During the premixing process, the silane activator is sprayed in by atomization to obtain a mixture. The mixture is melt-extruded through a twin-screw extruder. Then, it is vacuum de-alcoholized, granulated, and dried to obtain the transparent flame retardant masterbatch. c. Mix the raw materials of the front-side light-receiving adhesive film to obtain a mixture; extrude the mixture through a twin-screw extruder to obtain the front-side light-receiving adhesive film; d. Mix the raw materials of the backlight adhesive film to obtain a mixture; extrude the mixture through a twin-screw extruder to obtain the backlight adhesive film.
8. The method for preparing the flame-retardant encapsulating film according to claim 7, characterized in that, Includes at least one of the following features (1) to (4); (1) In step a, the temperature of the premix is 50~65℃ and the time is 10~20min; (2) In step a, the temperature of the melt extrusion is 150~170℃; (3) In step b, the premixing temperature is 50~65℃ and the time is 10~15min; (4) In step b, the temperature of the melt extrusion is 150~165℃.
9. The method for preparing the flame-retardant encapsulating film according to claim 7, characterized in that, Includes at least one of the following features (1) to (4); (1) In step c, EVA resin and transparent flame retardant masterbatch are mixed at 50~65℃, and then the first additive is added and mixed for 0.5~1.5h to obtain a mixture; (2) In step c, the extrusion casting temperature is 85~95℃; (3) In step d, EVA resin and high flame retardant masterbatch are mixed at 50~65℃, and then the second additive is added and mixed for 0.5~1.5h to obtain a mixture; (4) In step d, the extrusion casting temperature is 90~105℃.
10. A photovoltaic module, characterized in that, It includes a front cover plate, a front light-receiving adhesive film as described in any one of claims 1 to 6, a photovoltaic cell array, a back light-receiving adhesive film as described in any one of claims 1 to 6, and a rear cover plate stacked in sequence.