A high-strength bainitic steel with pre-introduced cementite and its preparation method
By using a three-stage austenitic process and a two-stage isothermal quenching method, the austenitizing temperature gradient and cementite precipitation are controlled, solving the problems of complex and costly preparation of high-strength bainitic steel. This results in a bainitic steel microstructure with high strength and good plasticity, suitable for large-size components.
Patent Information
- Application Number
- CN202611512064.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for preparing high-strength bainitic steel are complex and costly. Excessive addition of alloying elements leads to uneven performance and increased smelting costs. Traditional heat treatment processes are inefficient and difficult to apply to large-size components.
A high-strength bainitic steel with a gradient structure is formed by using a three-stage austenitizing process combined with a two-stage isothermal quenching method, which controls the austenitizing temperature gradient and cementite precipitation. This includes first-stage austenitizing, second-stage austenitizing, and third-stage austenitizing, with element distribution and cementite precipitation controlled respectively.
It significantly improves the strength and plasticity of bainitic steel, reduces production costs and time, and obtains a bainitic steel structure with high strength and good plasticity, avoiding microstructure coarsening and cracking, making it suitable for large-size components.
Smart Images

Figure CN123108241A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of iron and steel metallurgy technology, and particularly relates to a high-strength bainitic steel with pre-introduced cementite and its preparation method. Background Technology
[0002] High-strength bainitic steel, as an important material system for obtaining high-strength nanostructures, has always been a research hotspot for performance improvement. Traditional methods for obtaining nanostructures are difficult to apply to large-size components, while directly obtaining nanostructures in bulk materials through heat treatment processes shows significant advantages. Carbides play a crucial role in the complex microstructure of bainitic steel. The formation of grain boundary cementite before the bainitic phase transformation can reduce the carbon concentration at the cementite / austenite interface, lower the bainite nucleation activation energy, and accelerate the phase transformation. This allows for the formation of a multiphase structure within the original austenite grains, interwoven with nanoscale cementite particles, bainitic ferrite, and thin-film retained austenite, thus combining ultra-high strength with good plasticity, providing a new approach for the fabrication of large-size, high-performance metal components. Patent CN119530676A proposes a high-strength, high-toughness, low-carbon bainitic steel and its preparation method. It involves adding a small amount of rare earth element Eu and performing multiple forgings with different forging ratios to plastically deform and temper the low-carbon bainitic steel, controlling the type, quantity, and size of carbides to optimize the mechanical properties of the bainitic steel. However, its process is complex, and the excessive addition of alloying elements increases smelting costs. Patent CN108676987A proposes a method for preparing high-silicon super bainitic steel containing nano-cementite. Through rolling, cooling, and tempering, a small amount of carbides (1-5% volume fraction) is obtained in the bainitic steel, accelerating the formation of bainitic ferrite and increasing its volume fraction within the same time frame. This results in a more uniform and fine microstructure, promoting the precipitation of nano-cementite and significantly improving the strength and toughness of the high-silicon super bainitic steel containing nano-cementite. However, the addition of a magnetic field increases the need for experimental equipment and also raises experimental costs. Patent CN121046715A discloses an ultrafine lower bainitic steel and its preparation method. Through the synergistic effect of microalloying and multi-stage hot working processes, the addition of Cu and Ti elements significantly optimizes the preparation efficiency and surface properties of the lower bainitic microstructure. The two elements work together to refine the lower bainitic lamellars to a width ≤0.5μm, resulting in a stable surface roughness (Ra) of 0.05~0.10μm after polishing. However, significant microstructural differences between the core and surface layers may lead to overall steel performance issues, and the simultaneous addition of Cu and Ti elements increases costs during the smelting process.CN117778685A discloses a heat treatment process for promoting the formation of bundled bainite in high-carbon silicon-containing steel. The chemical composition of the high-carbon silicon-containing steel, by mass percentage, includes: C: 0.94~0.96%, Si: 1.31~1.33%, Mn: 0.43~0.45%, Cr: 1.07~1.09%, with the remainder being Fe and unavoidable impurities, including P≤0.04% and S≤0.04%. According to the above chemical composition ratio, an ingot is obtained by smelting, and then forged at 1050℃ to a size of 50mm × 50mm square bars are forged and then air-cooled to room temperature. The air-cooled material undergoes homogenization annealing to ensure uniform chemical composition. The homogenized annealed material is then heat-treated. This patent optimizes the heat treatment process, employing a two-step austenitization method to significantly promote the formation of bundled bainite, thereby increasing the proportion of bundled bainite. Combined with the positive effects of alloying elements, a nearly 90% bundled bainite structure is ultimately obtained. Solid solution strengthening is used to improve the tensile strength and hardness of the steel, achieving a hardness ≥66HRC and a tensile strength ≥2000MPa. However, this patent does not introduce cementite to promote phase transformation. Furthermore, the carbon and chromium content in the alloying elements is as high as 0.94~0.96% and 1.07~1.09%, respectively. According to the mechanical properties of strong plasticity, while increasing carbon content can significantly improve strength and hardness, it greatly reduces plasticity, resulting in greater brittleness. Therefore, even though this invention has high strength and hardness, its limited plasticity restricts its application in conventional production environments. Summary of the Invention
[0003] To address the aforementioned technical problems, this invention proposes a high-strength bainitic steel with pre-introduced cementite and its preparation method.
[0004] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a method for preparing high-strength bainitic steel with pre-introduced cementite, which is achieved through a three-stage austenitizing process plus two-stage isothermal quenching. The first-stage austenitizing temperature is based on complete austenitization, the second-stage austenitizing temperature controls element distribution, and the third-stage austenitizing temperature is based on the precipitation of cementite.
[0005] Furthermore, the method for preparing the pre-introduced cementite high-strength bainitic steel includes the following steps: (1) The high-strength bainitic steel to be treated is heated to a first preset temperature for austenitization treatment to obtain high-strength bainitic steel after austenitization treatment. The first preset temperature is 900℃~950℃. (2) The high-strength bainitic steel after austenitization treatment is cooled to a second preset temperature at a first cooling rate, and then subjected to a first heat preservation to form a ferrite-austenite dual-phase structure in the high-strength bainitic steel. Then, the temperature is raised to a third preset temperature at a first heating rate to obtain a cementite-austenite dual-phase structure. The first cooling rate is 10℃ / s~30℃ / s, the second preset temperature is 800~830℃, the first heating rate is 10℃ / s~20℃ / s, and the third preset temperature is 830℃~900℃. (3) Cool the high-strength bainitic steel to the fourth preset temperature at the second rapid cooling rate, and then raise it to the fifth preset temperature at the second heating rate to form a cementite-bainite structure. The second rapid cooling rate is 10℃ / s~20℃ / s, the fourth preset temperature is 200℃~230℃, the second heating rate is 20℃ / s~30℃ / s, and the fifth preset temperature is 230~260℃.
[0006] The high-strength bainitic steel matrix of this invention has a pearlitic structure, and a gradient structure transitioning from cementite-austenite to cementite-bainite is formed through a stepped isothermal process. Specifically, this invention first heats the high-strength bainitic steel to a first preset temperature to form a high-strength bainitic steel with an austenitic phase structure, then cools it to a second preset temperature to form a ferrite-austenite dual-phase structure, then raises it to a third preset temperature to obtain a cementite-austenite dual-phase structure, and finally performs double-stage isothermal quenching to achieve a gradient structure cementite-bainitic high-strength bainitic steel.
[0007] Further, in step (1), the high-strength bainitic steel matrix to be treated is a pearlitic structure, and its composition, by mass percentage, includes: C: 0.65~0.85%, Mn: 0.5~2.0%, Cr: 0.2~0.4%, Si: 2.0~2.8%, P<0.02%, S<0.02%, Ti: 0.01~0.02%, Ni: 0~0.01%, Mo: 0~0.01%, Al: 0.01~0.04%, Cu: 0.01~0.02%, with the balance being Fe and unavoidable impurities; Regardless of percentages, the above elements satisfy the following relationships: 1.07 ≤ D ≤ 6.02, 0.19 ≤ d ≤ 1.2: D=(1.2[C]+2[Mn])×(0.5[Si]-[Cr]); d=(180[Ti]+210[Al]) / 1000[Cu].
[0008] Furthermore, in step (1), the heat preservation time at the first preset temperature is 20~40 minutes.
[0009] Furthermore, in step (2), the heat preservation time at the second preset temperature is 30 min to 1 h; The heat preservation time at the third preset temperature is 20~40 minutes.
[0010] Furthermore, in step (3), the heat preservation time at the fourth preset temperature is 2 minutes; The heat preservation time at the fifth preset temperature is 2 to 8.5 hours.
[0011] The present invention also provides a high-strength bainitic steel pre-introduced with cementite prepared according to the above method, the microstructure of which consists of bainitic ferrite laths, retained austenite and martensite, the average size of the bainitic ferrite laths being 30~60 nm; the volume fraction of retained austenite being 20%~40%, with an average size of 0.4 μm~3.5 μm; and the volume fraction of cementite being 2~4.5%.
[0012] Furthermore, the high-strength bainitic steel with pre-introduced cementite has a tensile strength > 2000 MPa, a yield strength > 1700 MPa, and an elongation > 10%.
[0013] Compared with the prior art, the present invention has the following advantages and technical effects: (1) In view of the problem that the traditional bainitic high-strength bainitic steel requires a long isothermal time to improve production efficiency and thus causes serious heat loss, the present invention utilizes the austenitizing temperature gradient process to generate cementite structure in the gradient process, accelerate the subsequent phase transformation rate, reduce the time required for the process flow, and achieve the effect of green short process to obtain high-strength bainitic steel.
[0014] (2) The austenitizing temperature gradient process is designed. The second-stage austenitizing isotherm is used in advance to make the steel in a lower austenitizing temperature state, so that the high-strength bainitic steel diffuses elements after high-temperature austenitizing, thereby promoting the precipitation of carbides in the third-stage austenitizing. Moreover, the third-stage temperature is lower than the first-stage temperature, and no large internal stress is generated during rapid cooling. The ferrite and pearlite transformation range is avoided, the designed target structure is obtained, and cracking is not easy to occur.
[0015] (3) Through the design of gradient structure, the matrix of high-strength bainitic steel is obtained by isothermal treatment of third-order austenitization and isothermal quenching, resulting in ultrafine bainitic or ultrafine bainitic-martensite structure, which significantly refines the grains and improves strength and plasticity. At the same time, the matrix structure is cementite + bainitic structure, which also significantly improves the strength and plasticity of traditional high-carbon bainitic steel. Attached Figure Description
[0016] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 SEM image of the matrix microstructure of the high-strength bainitic steel with pre-introduced cementite prepared in Example 1 of this invention; Figure 2 SEM image of the matrix microstructure of the high-strength bainitic steel with pre-introduced cementite prepared in Example 2 of this invention; Figure 3 This is a SEM image of the matrix structure of the high-strength bainitic steel prepared in Comparative Example 2 of the present invention. Detailed Implementation
[0017] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0018] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0019] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0020] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be obvious to those skilled in the art. This specification and embodiments are merely exemplary.
[0021] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0022] The embodiments of the present invention provide a method for preparing high-strength bainitic steel with pre-introduced cementite, which is achieved by a three-stage austenitizing process plus a two-stage isothermal quenching. The first-stage austenitizing temperature is based on complete austenitization, the second-stage austenitizing temperature controls the element distribution, and the third-stage austenitizing temperature is based on the precipitation of cementite.
[0023] In a preferred embodiment of the present invention, the method for preparing high-strength bainitic steel with pre-introduced cementite includes the following steps: (1) The high-strength bainitic steel to be treated is heated to the first preset temperature for austenitization treatment to obtain high-strength bainitic steel after austenitization treatment (i.e., high-strength bainitic steel with austenitic phase structure is obtained after this treatment). The first preset temperature is 900℃~950℃ and the holding time is 20~40min. (2) Cool the high-strength bainitic steel after austenitization treatment to the second preset temperature at the first cooling rate, and then perform the first heat preservation to form a ferrite-austenite dual-phase structure of the high-strength bainitic steel. Then raise the temperature to the third preset temperature at the first heating rate to obtain a cementite-austenite dual-phase structure. The first cooling rate is 10℃ / s~30℃ / s, the second preset temperature is 800~830℃, and the heat preservation time is 30min~1h. The first heating rate is 10℃ / s~20℃ / s, the third preset temperature is 830℃~900℃, and the heat preservation time is 20~40min. (3) Cool the high-strength bainitic steel to the fourth preset temperature at the second rapid cooling rate, and then raise it to the fifth preset temperature at the second heating rate to form a cementite-bainite structure. The second rapid cooling rate is 10℃ / s~20℃ / s, the fourth preset temperature is 200℃~230℃, and the holding time is 2min. The second heating rate is 20℃ / s~30℃ / s, the fifth preset temperature is 230~260℃, and the holding time is 2~8.5h.
[0024] In a preferred embodiment of the present invention, in step (1), the high-strength bainitic steel matrix to be treated is a pearlitic structure, and its composition, by mass percentage, includes: C: 0.65~0.85%, Mn: 0.5~2.0%, Cr: 0.2~0.4%, Si: 2.0~2.8%, P<0.02%, S<0.02%, Ti: 0.01~0.02%, Ni: 0~0.01%, Mo: 0~0.01%, Al: 0.01~0.04%, Cu: 0.01~0.02%, with the balance being Fe and unavoidable impurities; Regardless of percentages, the above elements satisfy the following relationships: 1.07 ≤ D ≤ 6.02, 0.19 ≤ d ≤ 1.2. D=(1.2[C]+2[Mn])×(0.5[Si]-[Cr]); d=(180[Ti]+210[Al]) / 1000[Cu].
[0025] For example, the chemical composition of the high-strength bainitic steel to be treated, by mass percentage, is: C: 0.76%, Mn: 0.77%, Cr: 0.51%, Si: 2.69%, P: 0.0015%, S: 0.0015%, Ti: 0.005%, Ni: 0.007%, Mo: 0.001%, Al: 0.036%, with the balance being Fe and unavoidable impurities.
[0026] This invention does not limit the method of austenitization treatment; any conventional method in the art may be used. For example, austenitization treatment may be a hot forming process that includes heating high-strength bainitic steel to the austenitization temperature, such as hot rolling or forging, or it may be without a hot forming process.
[0027] The present invention also provides a high-strength bainitic steel pre-introduced with cementite prepared according to the above method, the microstructure of which consists of bainitic ferrite laths, retained austenite and martensite, the average size of the bainitic ferrite laths being 30~60 nm; the volume fraction of retained austenite being 20%~40%, with an average size of 0.4 μm~3.5 μm; and the volume fraction of cementite being 2~4.5%.
[0028] This invention provides a design concept—by pre-controlling the precipitation (morphology, size, distribution) of cementite, it becomes a beneficial means of regulation.
[0029] In a preferred embodiment of the present invention, the high-strength bainitic steel with pre-introduced cementite has a tensile strength > 2000 MPa, a yield strength > 1700 MPa, and an elongation > 10%.
[0030] In this invention, the tensile property test standard refers to GB / T 228.1 2021.
[0031] Unless otherwise specified, the room temperature in this invention is 25±2℃.
[0032] All raw materials used in the embodiments of the present invention were obtained through commercial purchase.
[0033] It should be noted that any aspects not described in detail in this invention are conventional practices in the field and are not the focus of this invention.
[0034] The technical solution of the present invention will be further illustrated by the following embodiments.
[0035] Example 1 The chemical composition of the high-strength bainitic steel to be treated, by mass percentage, is as follows: C: 0.72%, Mn: 1.2%, Cr: 0.25%, Si: 2.69%, P: 0.0015%, S: 0.0015%, Ti: 0.01%, Ni: 0.007%, Mo: 0.001%, Al: 0.036%, Cu: 0.012%, with the balance being Fe and unavoidable impurities, D=3.57, d=0.78.
[0036] A method for preparing high-strength bainitic steel with pre-introduced cementite, comprising the following steps: The high-strength bainitic steel to be treated, processed into a square ingot shape, was austenitized in air at 900℃ for 30 min. The austenitized high-strength bainitic steel was then cooled to 800℃ and held for 30 min at an air cooling rate of 12℃ / s. Subsequently, it was heated to 840℃ at an air heating rate of 15℃ / s and held for 30 min. Then, it was cooled to 210℃ at a water mist cooling rate of 15℃ / s and held for 2 min. After that, it was heated to 230℃ at a salt bath heating rate of 20℃ / s (potassium nitrate and sodium nitrite in a mass ratio of 1:1, the same below) and held for 8.5 h. Finally, it was air-cooled to room temperature to obtain high-strength bainitic steel with pre-introduced cementite.
[0037] The SEM image of the matrix microstructure of the high-strength bainitic steel with pre-introduced cementite prepared in this embodiment is shown below. Figure 1 ,Depend on Figure 1 It can be seen that the matrix structure is martensitic-bainitic, with bainitic ferrite lath size of 33 nm, blocky retained austenite size of 0.79 μm, retained austenite volume fraction of 19.3%, cementite fraction of 4.2%, yield strength of 1748 MPa, tensile strength of 2052 MPa, and elongation of 10.6%.
[0038] Example 2 The chemical composition of the high-strength bainitic steel to be treated, by mass percentage, is as follows: C: 0.76%, Mn: 0.77%, Cr: 0.32%, Si: 2.69%, P: 0.0015%, S: 0.0015%, Ti: 0.015%, Ni: 0.007%, Mo: 0.001%, Al: 0.036%, Cu: 0.015%, with the balance being Fe and unavoidable impurities, D=2.51, d=0.68.
[0039] A method for preparing high-strength bainitic steel with pre-introduced cementite, comprising the following steps: The high-strength bainitic steel to be treated, processed into a square ingot shape, was austenitized at 920℃ for 30 minutes in air. The austenitized high-strength bainitic steel was then cooled to 810℃ at an air cooling rate of 18℃ / s and held for 40 minutes. Subsequently, it was heated to 870℃ at an air heating rate of 20℃ / s and held for 30 minutes. Then, it was cooled to 220℃ at a salt bath cooling rate of 20℃ / s and held for 2 minutes. After that, it was heated to 250℃ at a salt bath heating rate of 25℃ / s and held for 7.2 hours. Finally, it was air-cooled to room temperature to obtain high-strength bainitic steel with pre-introduced cementite.
[0040] The high-strength bainitic steel with pre-introduced cementite prepared in this embodiment has an ultrafine bainitic structure, with bainitic ferrite lath size of 45 nm, blocky retained austenite size of 0.74 μm, retained austenite volume fraction of 21.2%, cementite fraction of 3.2%, yield strength of 1846 MPa, tensile strength of 2272 MPa, and elongation of 11.0%.
[0041] Example 3 The chemical composition of the high-strength bainitic steel to be treated, by mass percentage, is as follows: C: 0.79%, Mn: 1.6%, Cr: 0.36%, Si: 2.42%, P: 0.0015%, S: 0.0015%, Ti: 0.018%, Ni: 0.007%, Mo: 0.001%, Al: 0.036%, Cu: 0.016%, with the balance being Fe and unavoidable impurities, D=3.53, d=0.68.
[0042] A method for preparing high-strength bainitic steel with pre-introduced cementite, comprising the following steps: The high-strength bainitic steel to be treated, which was processed into a square ingot shape, was austenitized in air at 950℃ for 30 min. The austenitized high-strength bainitic steel was then cooled to 820℃ and held for 50 min at a water mist cooling rate of 26℃ / s. Subsequently, it was heated to 850℃ and held for 50 min at an air heating rate of 18℃ / s. Then, it was cooled to 220℃ and held for 2 min at an air cooling rate of 10℃ / s. Finally, it was heated to 260℃ in a salt bath at a rate of 28℃ / s and held for 2.2 h. Finally, it was air cooled to room temperature to obtain high-strength bainitic steel with pre-introduced cementite.
[0043] The high-strength bainitic steel with pre-introduced cementite prepared in this embodiment has an ultrafine bainitic structure, with bainitic ferrite lath size of 38 nm, blocky retained austenite size of 0.75 μm, retained austenite volume fraction of 22.6%, cementite fraction of 4.2%, yield strength of 1822 MPa, tensile strength of 2105 MPa, and elongation of 11.8%.
[0044] Comparative Example 1 The chemical composition of the high-strength bainitic steel to be treated, by mass percentage, is as follows: C: 0.76%, Mn: 0.77%, Cr: 0.32%, Si: 2.69%, P: 0.0015%, S: 0.0015%, Ti: 0.015%, Ni: 0.007%, Mo: 0.001%, Al: 0.036%, Cu: 0.015%, with the balance being Fe and unavoidable impurities, D=2.51, d=0.68.
[0045] The high-strength bainitic steel to be treated, which was processed into a square ingot shape, was subjected to austenitization treatment at 920℃ for 30 minutes in air. The temperature was then reduced to 350℃ at an air cooling rate of 8℃ / s, held for 7.5 hours, and air-cooled to room temperature to obtain the final treated high-strength bainitic steel.
[0046] The high-strength bainitic steel prepared in this comparative example has an ultrafine bainitic structure with a bainitic ferrite lath size of 58 nm, a blocky retained austenite size of 3.17 μm, a retained austenite volume fraction of 31.6%, a cementite fraction of 0%, a yield strength of 1176 MPa, a tensile strength of 1728 MPa, and an elongation of 21.3%.
[0047] Because this comparative example did not undergo the second and third stages of austenitization, no cementite precipitated, thus failing to accelerate the subsequent phase transformation process and resulting in a coarsened microstructure. Comparing this to the above examples, the size of the bainitic ferrite laths and the size of the blocky retained austenite are significantly increased, leading to a higher retained austenite content. This results in a significant decrease in the strength of the comparative example, but due to the increased soft phase, the elongation is increased.
[0048] Comparative Example 2 The chemical composition of the high-strength bainitic steel to be treated is the same as in Example 1.
[0049] The high-strength bainitic steel to be treated, which was processed into a square ingot shape, was austenitized under air conditions at 850℃ for 30 minutes. The temperature was then reduced to 350℃ at an air cooling rate of 10℃ / s, held for 7.5 hours, and air-cooled to room temperature to obtain the final treated high-strength bainitic steel.
[0050] Figure 3 The image shows the SEM image of the matrix microstructure of the high-strength bainitic steel prepared in this comparative example. The microstructure of the high-strength bainitic steel prepared in this comparative example is an ultrafine bainitic microstructure with a bainitic ferrite lath size of 60 nm, a blocky retained austenite size of 1.45 μm, a retained austenite volume fraction of 16%, a cementite fraction of 3.6%, a yield strength of 1217 MPa, a tensile strength of 1624 MPa, and an elongation of 10.3%.
[0051] Because this comparative example only underwent the third stage of austenitization, lacking the homogenizing effect of the first two stages, although the precipitated cementite refined the microstructure, the microstructure size was relatively large compared to the example, resulting in poor strength and plasticity. Compared to Comparative Example 1, due to the lower austenitization temperature, less alloying element dissolved into the matrix, resulting in less residual austenite and lower strength.
[0052] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing high-strength bainitic steel with pre-introduced cementite, characterized in that, It is achieved through a three-stage austenitizing process plus a two-stage isothermal quenching. The first-stage austenitizing temperature is based on complete austenitization, the second-stage austenitizing temperature controls element distribution, and the third-stage austenitizing temperature is based on the precipitation of cementite.
2. The method for preparing high-strength bainitic steel with pre-introduced cementite according to claim 1, characterized in that, Includes the following steps: (1) The high-strength bainitic steel to be treated is heated to a first preset temperature for austenitization treatment to obtain high-strength bainitic steel after austenitization treatment. The first preset temperature is 900℃~950℃. (2) The high-strength bainitic steel after austenitization treatment is cooled to a second preset temperature at a first cooling rate, and then subjected to a first heat preservation to form a ferrite-austenite dual-phase structure in the high-strength bainitic steel. Then, the temperature is raised to a third preset temperature at a first heating rate to obtain a cementite-austenite dual-phase structure. The first cooling rate is 10℃ / s~30℃ / s, the second preset temperature is 800~830℃, the first heating rate is 10℃ / s~20℃ / s, and the third preset temperature is 830℃~900℃. (3) Cool the high-strength bainitic steel to the fourth preset temperature at the second rapid cooling rate, and then raise it to the fifth preset temperature at the second heating rate to form a cementite-bainite structure. The second rapid cooling rate is 10℃ / s~20℃ / s, the fourth preset temperature is 200℃~230℃, the second heating rate is 20℃ / s~30℃ / s, and the fifth preset temperature is 230~260℃.
3. The method for preparing high-strength bainitic steel with pre-introduced cementite according to claim 2, characterized in that, In step (1), the composition of the high-strength bainitic steel to be treated, by mass percentage, includes: C: 0.65~0.85%, Mn: 0.5~2.0%, Cr: 0.2~0.4%, Si: 2.0~2.8%, P<0.02%, S<0.02%, Ti: 0.01~0.02%, Ni: 0~0.01%, Mo: 0~0.01%, Al: 0.01~0.04%, Cu: 0.01~0.02%, with the balance being Fe and unavoidable impurities; Regardless of percentages, the above elements satisfy the following relationships: 1.07 ≤ D ≤ 6.02, 0.19 ≤ d ≤ 1.2: D=(1.2[C]+2[Mn])×(0.5[Si]-[Cr]); d=(180[Ti]+210[Al]) / 1000[Cu].
4. The method for preparing high-strength bainitic steel with pre-introduced cementite according to claim 2, characterized in that, In step (1), the heat preservation time at the first preset temperature is 20~40 minutes.
5. The method for preparing high-strength bainitic steel with pre-introduced cementite according to claim 2, characterized in that, In step (2), the heat preservation time at the second preset temperature is 30 min to 1 h; The heat preservation time at the third preset temperature is 20~40 minutes.
6. The method for preparing high-strength bainitic steel with pre-introduced cementite according to claim 2, characterized in that, In step (3), the heat preservation time at the fourth preset temperature is 2 minutes; The heat preservation time at the fifth preset temperature is 2 to 8.5 hours.
7. A high-strength bainitic steel with pre-introduced cementite, characterized in that, The high-strength bainitic steel prepared according to any one of claims 1 to 6 has a microstructure consisting of bainitic ferrite laths, retained austenite, and martensite, wherein the average size of the bainitic ferrite laths is 30 to 60 nm; the volume fraction of retained austenite is 20% to 40%, with an average size of 0.4 μm to 3.5 μm; and the volume fraction of cementite is 2% to 4.5%.
8. The high-strength bainitic steel with pre-introduced cementite according to claim 7, characterized in that, Its tensile strength is >2000MPa, yield strength is >1700MPa, and elongation is >10%.
Citation Information
Patent Citations
Preparation method for high-silicon super bainite steel containing nanometer cementite
CN108676987A
Heat treatment process for promoting formation of high-carbon silicon-containing steel bundle-shaped bainite
CN117778685A
High-toughness low-carbon bainite steel and preparation method thereof
CN119530676A
Superfine lower bainite steel and preparation method thereof
CN121046715A