A temperature gradient graphitization annealing process for cast iron components
By calculating the local target annealing temperature and constructing a heat flow blocking zone, combined with directional cooling airflow and power compensation energy control, the problem of inconsistent microstructure and mechanical properties of variable cross-section cast iron parts during the annealing process was solved, and a uniform annealing effect for cast iron components was achieved.
Patent Information
- Application Number
- CN202611618452.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing annealing processes for cast iron components cannot effectively solve the problems of mismatched phase transformation conditions in different regions of variable cross-section cast iron components, temperature difference in different regions affected by transverse heat transfer, local temperature drop caused by phase transformation heat absorption, and inconsistent eutectoid transformation time in different regions, resulting in heterogeneity of microstructure and inconsistent mechanical properties.
By calculating the local target annealing temperature of each physical section, applying spatial non-uniform heat flow, and constructing a heat flow blocking zone at the boundary of adjacent sections, combined with directional cooling airflow and power compensation energy control, synchronous annealing of each section is achieved.
It achieves the annealing requirements of different regions of variable cross-section cast iron components, reduces the difference in microstructure, and improves the consistency of microstructure and mechanical properties of each section.
Smart Images

Figure CN123108243A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of ferrous metal heat treatment technology, and particularly relates to a temperature gradient graphitization annealing process for cast iron components. Background Technology
[0002] Heat treatment of ferrous metal castings typically employs annealing with overall furnace heating. This involves maintaining the furnace at a set temperature for a specified time, allowing the metastable structure within the cast iron to gradually transform into an equilibrium structure. This eliminates casting stress and improves machinability. For variable cross-section cast iron components with significant differences in wall thickness, the heat dissipation conditions vary across different physical sections. Therefore, during solidification and cooling after casting, the cooling rates of each section often differ considerably. Thin-walled areas, affected by rapid cooling, are prone to forming high-hardness eutectic cementite and white cast iron structures; thick-walled areas, with slower heat dissipation, are more likely to form coarse graphite flakes and a coarse-grained matrix. Traditional furnace heating equipment and its fixed structural constraints make it difficult to provide independent temperature environments for different cross-sections of the same component in physical space.
[0003] In addition to the aforementioned hardware limitations, existing annealing process control methods also have shortcomings. For example, Chinese invention patent application CN101988143A discloses an annealing process for castable iron, which involves heating the cast iron billet to 900-980℃ and holding it for 3 hours, followed by cooling and air cooling after removal from the furnace. This technical solution is based on the ideal assumption that the overall structure of the component is uniform and the phase transformation kinetics are consistent. It ignores the objective law that the initial microstructure and phase transformation driving force of different sections of the variable cross-section component are significantly different due to the difference in solidification modulus. For variable cross-section cast iron components containing alternating thin and thick walls, if the above-mentioned uniform nominal heating temperature and holding time are used, the thick-walled area is very likely to experience severe coarsening of graphite flakes and overheating degradation of matrix grains due to prolonged exposure to a high-temperature environment of 900-980℃. Furthermore, this process fails to provide a control mechanism for blocking transverse heat conduction paths and aligning the cooling sequence across sections, and cannot eliminate the microstructure heterogeneity and phase transformation stress between sections.
[0004] Therefore, during the annealing process of variable cross-section cast iron components, it is still necessary to solve problems such as the mismatch of phase transformation conditions in different regions, the influence of transverse heat transfer on regional temperature difference, the local temperature drop caused by phase transformation heat absorption, and the inconsistent eutectoid transformation time in different regions, in order to improve the consistency of matrix structure and mechanical properties in different sections of the component. Summary of the Invention
[0005] To address the problems in the background art, the technical solution of the present invention is as follows: A temperature field gradient graphitization annealing process for cast iron components, comprising the following steps: Step S1: Obtain the ratio of the volume to the heat dissipation surface area of each physical section of the variable cross-section cast iron component, and determine the solidification modulus of each physical section. Step S2: Calculate the local target annealing temperature of each physical section based on the solidification modulus. Add the quotient obtained by dividing the basic phase transformation threshold temperature and the gradient compensation coefficient by the solidification modulus to obtain the local target annealing temperature, thus forming an inverse constraint relationship that the smaller the solidification modulus, the higher the local target annealing temperature. Step S3: Apply spatial non-uniform heat flow to the variable cross-section cast iron component so that each physical section reaches the corresponding local target annealing temperature; Step S4: Maintain the local target annealing temperature for graphitization heat preservation. Apply directional cooling airflow to the boundary of adjacent physical sections where the difference in solidification modulus is greater than a set threshold to construct a heat flow blocking zone, cut off the lateral heat conduction path, and collect the hysteresis deviation of the heating rate of each physical section relative to the heat power input during the heat preservation period and calculate the hysteresis deviation change rate. When the hysteresis deviation change rate is greater than zero, inject power compensation energy into the physical section that produces the hysteresis deviation to offset the local temperature drop caused by the endothermic decomposition of eutectic cementite. Step S5: After the heat preservation is completed, the delayed start cooling time is calculated based on the local target annealing temperature and the configured local cooling rate of each physical section. The physical section with a larger solidification modulus is controlled to delay the start cooling time relative to the physical section with a smaller solidification modulus, so as to guide each physical section to enter the eutectoid transformation temperature range synchronously.
[0006] Preferably, in step S2, the local target annealing temperature is calculated according to the following formula: ,in, This refers to the local target annealing temperature of the corresponding physical section. It is the basic phase transformation threshold temperature, and its value range covers the lower limit temperature of austenitization of variable cross-section cast iron component materials; For gradient compensation coefficients, This represents the solidification modulus of the corresponding physical region.
[0007] Preferably, the basic phase transformation threshold temperature is set to 780℃ and the gradient compensation coefficient is set to 56℃·cm; for the thin-walled physical section with a solidification modulus of 0.4cm, the calculated local target annealing temperature is 920℃; for the thick-walled physical section with a solidification modulus of 1.2cm, the calculated local target annealing temperature is 826℃.
[0008] Preferably, step S4 includes step S41, where at the boundary where the difference in solidification modulus between adjacent physical sections is greater than 0.3 cm, an annular jet device is activated to apply a cooling airflow of 12 L / s to 15 L / s to the boundary, carrying away the lateral heat transferred from the higher-temperature physical section to the lower-temperature physical section, and maintaining the spatial temperature difference between adjacent physical sections.
[0009] Preferably, step S4 includes step S42, during the graphitization heat preservation period, when the rate of change of hysteresis deviation is greater than zero, the induction heating power density corresponding to the physical section that generates hysteresis deviation is increased, and the injected power compensation energy is used to offset the local temperature drop caused by the decomposition and absorption of latent heat of phase change of eutectic cementite; when the rate of change of hysteresis deviation is less than or equal to zero, the power compensation energy is controlled to decrease to zero within a 5-minute buffer time, so that the local target annealing temperature remains stable.
[0010] Preferably, in step S5, the eutectoid transformation temperature range is 720°C to 740°C, and the delayed start-up cooling time of the thick-walled physical section with a larger solidification modulus relative to the thin-walled physical section with a smaller solidification modulus is calculated using the following formula: ,in, To delay the start-up cooling time, and These are the local target annealing temperatures for the thin-walled and thick-walled physical sections, respectively. and The local cooling rates are configured for the thin-walled and thick-walled physical sections, respectively. The upper limit of the eutectoid transformation temperature range is set to 740℃.
[0011] Preferably, step S5 includes step S51, where a local cooling rate of 3°C / min is configured for the thin-walled physical section with a solidification modulus of 0.4cm, and a local cooling rate of 9°C / min is configured for the thick-walled physical section with a solidification modulus of 1.2cm; the thin-walled physical section is controlled to start cooling first, and after the thin-walled physical section has cooled for 50.44min, the thick-walled physical section is controlled to start cooling, guiding the thin-walled physical section and the thick-walled physical section to reach and pass through the eutectoid transformation temperature range of 720°C to 740°C simultaneously.
[0012] Preferably, step S3 includes step S31, in which an induction heating device equipped with multiple independent and controllable heating zones is used to apply a spatially non-uniform heat flow to the variable cross-section cast iron component; the thin-walled physical section with a solidification modulus of 0.4 cm is heated to 920°C at a heating rate of 15°C / min, and the thick-walled physical section with a solidification modulus of 1.2 cm is heated to 826°C at a heating rate of 10°C / min.
[0013] Preferably, in step S4, the time for maintaining graphitization under a non-uniform temperature field is set to 240 min. During the holding period, the eutectic cementite in the thin-walled physical section with a solidification modulus of 0.4 cm decomposes into austenite and flocculent graphite, and the diffusion flux of carbon atoms to the existing graphite sheet in the thick-walled physical section with a solidification modulus of 1.2 cm is suppressed, thereby preventing graphite sheet coarsening and austenite grain growth.
[0014] Preferably, step S5 includes step S52, in which the variable cross-section cast iron component is cooled to room temperature after each physical section has simultaneously passed through the eutectoid transformation temperature range of 720°C to 740°C, so that each physical section of the variable cross-section cast iron component obtains a uniformly distributed ferrite and pearlite mixed matrix structure.
[0015] Compared with existing technologies, the temperature gradient graphitization annealing process for cast iron components of the present invention has the following advantages: 1. In the temperature field gradient graphitization annealing process of cast iron components, the corresponding local target annealing temperature is set according to the solidification modulus of each physical section, so that the thin-walled area can obtain the temperature conditions required for the decomposition of eutectic cementite, while avoiding the aggravation of graphite flake coarsening and austenite grain growth in the thick-walled area due to excessive temperature. In this way, the annealing requirements of different areas of the variable cross-section cast iron component can be taken into account. While removing the white iron structure in the thin-walled area, the coarsening of the structure in the thick-walled area is suppressed, and the difference in structure between different cross sections is reduced.
[0016] 2. When there is a large temperature difference between adjacent physical sections, the directional cooling airflow can remove the transverse heat conduction at the interface and form a heat flow blocking zone, which can reduce the heat transfer from the high temperature area to the low temperature area and prevent the temperature difference between the areas from shrinking rapidly due to the thermal conductivity of the metal. This allows different physical sections to maintain their respective required temperatures more stably during the graphitization heat preservation period, providing stable temperature conditions for annealing different areas of the variable cross-section cast iron component.
[0017] 3. During the graphitization heat preservation process, timely replenishment of power compensation energy according to the hysteresis deviation change rate can compensate for the local heat loss caused by the decomposition and heat absorption of eutectic cementite, reduce the temperature drop during the phase transformation, and keep the thin-walled area relatively stable near the local target annealing temperature, which is conducive to the continuous decomposition of eutectic cementite. After the phase transformation heat absorption weakens, the compensation is gradually reduced to avoid the temperature overshoot caused by the compensation power being withdrawn too quickly or continuously input, thereby improving the stability of temperature control during the heat preservation stage. Attached Figure Description
[0018] Figure 1 This is a flowchart of the local annealing control process for the variable cross-section cast iron component of the present invention; Figure 2 This is a diagram illustrating the closed-loop monitoring and physical interaction of the annealing equipment of this invention. Detailed Implementation
[0019] The technical solutions of the embodiments of this application will be clearly described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of this application are within the scope of protection of this application.
[0020] A temperature gradient graphitization annealing process for cast iron components includes the following steps: Step S1: Obtain the ratio of the volume to the heat dissipation surface area of each physical section of the variable cross-section cast iron component, and determine the solidification modulus of each physical section. Step S2: Calculate the local target annealing temperature of each physical section based on the solidification modulus. Add the quotient obtained by dividing the basic phase transformation threshold temperature and the gradient compensation coefficient by the solidification modulus to obtain the local target annealing temperature, thus forming an inverse constraint relationship that the smaller the solidification modulus, the higher the local target annealing temperature. Step S3: Apply spatial non-uniform heat flow to the variable cross-section cast iron component so that each physical section reaches the corresponding local target annealing temperature; Step S4: Maintain the local target annealing temperature for graphitization heat preservation. Apply directional cooling airflow to the boundary of adjacent physical sections where the difference in solidification modulus is greater than a set threshold to construct a heat flow blocking zone, cut off the lateral heat conduction path, and collect the hysteresis deviation of the heating rate of each physical section relative to the heat power input during the heat preservation period and calculate the hysteresis deviation change rate. When the hysteresis deviation change rate is greater than zero, inject power compensation energy into the physical section that produces the hysteresis deviation to offset the local temperature drop caused by the endothermic decomposition of eutectic cementite. Step S5: After the heat preservation is completed, the delayed start cooling time is calculated based on the local target annealing temperature and the configured local cooling rate of each physical section. The physical section with a larger solidification modulus is controlled to delay the start cooling time relative to the physical section with a smaller solidification modulus, so as to guide each physical section to enter the eutectoid transformation temperature range synchronously.
[0021] Preferably, in step S2, the local target annealing temperature is calculated according to the following formula: ,in, This refers to the local target annealing temperature of the corresponding physical section. It is the basic phase transformation threshold temperature, and its value range covers the lower limit temperature of austenitization of variable cross-section cast iron component materials; For gradient compensation coefficients, This represents the solidification modulus of the corresponding physical region.
[0022] Preferably, the basic phase transformation threshold temperature is set to 780℃ and the gradient compensation coefficient is set to 56℃·cm; for the thin-walled physical section with a solidification modulus of 0.4cm, the calculated local target annealing temperature is 920℃; for the thick-walled physical section with a solidification modulus of 1.2cm, the calculated local target annealing temperature is 826℃.
[0023] Preferably, step S4 includes step S41, where at the boundary where the difference in solidification modulus between adjacent physical sections is greater than 0.3 cm, an annular jet device is activated to apply a cooling airflow of 12 L / s to 15 L / s to the boundary, carrying away the lateral heat transferred from the higher-temperature physical section to the lower-temperature physical section, and maintaining the spatial temperature difference between adjacent physical sections.
[0024] Preferably, step S4 includes step S42, during the graphitization heat preservation period, when the rate of change of hysteresis deviation is greater than zero, the induction heating power density corresponding to the physical section that generates hysteresis deviation is increased, and the injected power compensation energy is used to offset the local temperature drop caused by the decomposition and absorption of latent heat of phase change of eutectic cementite; when the rate of change of hysteresis deviation is less than or equal to zero, the power compensation energy is controlled to decrease to zero within a 5-minute buffer time, so that the local target annealing temperature remains stable.
[0025] Preferably, in step S5, the eutectoid transformation temperature range is 720°C to 740°C, and the delayed start-up cooling time of the thick-walled physical section with a larger solidification modulus relative to the thin-walled physical section with a smaller solidification modulus is calculated using the following formula: ,in, To delay the start-up cooling time, and These are the local target annealing temperatures for the thin-walled and thick-walled physical sections, respectively. and The local cooling rates are configured for the thin-walled and thick-walled physical sections, respectively. The upper limit of the eutectoid transformation temperature range is set to 740℃.
[0026] Preferably, step S5 includes step S51, where a local cooling rate of 3°C / min is configured for the thin-walled physical section with a solidification modulus of 0.4cm, and a local cooling rate of 9°C / min is configured for the thick-walled physical section with a solidification modulus of 1.2cm; the thin-walled physical section is controlled to start cooling first, and after the thin-walled physical section has cooled for 50.44min, the thick-walled physical section is controlled to start cooling, guiding the thin-walled physical section and the thick-walled physical section to reach and pass through the eutectoid transformation temperature range of 720°C to 740°C simultaneously.
[0027] Preferably, step S3 includes step S31, in which an induction heating device equipped with multiple independent and controllable heating zones is used to apply a spatially non-uniform heat flow to the variable cross-section cast iron component; the thin-walled physical section with a solidification modulus of 0.4 cm is heated to 920°C at a heating rate of 15°C / min, and the thick-walled physical section with a solidification modulus of 1.2 cm is heated to 826°C at a heating rate of 10°C / min.
[0028] Preferably, in step S4, the time for maintaining graphitization under a non-uniform temperature field is set to 240 min. During the holding period, the eutectic cementite in the thin-walled physical section with a solidification modulus of 0.4 cm decomposes into austenite and flocculent graphite, and the diffusion flux of carbon atoms to the existing graphite sheet in the thick-walled physical section with a solidification modulus of 1.2 cm is suppressed, thereby preventing graphite sheet coarsening and austenite grain growth.
[0029] Preferably, step S5 includes step S52, in which the variable cross-section cast iron component is cooled to room temperature after each physical section has simultaneously passed through the eutectoid transformation temperature range of 720°C to 740°C, so that each physical section of the variable cross-section cast iron component obtains a uniformly distributed ferrite and pearlite mixed matrix structure.
[0030] Example 1: This example uses the heat treatment of a ductile iron steering knuckle for a passenger car as an example. This component includes a solidification modulus. For the thin-walled flange area of 0.4cm and solidification modulus The bearing housing region has a thick wall of 1.2 cm, while the thin-walled flange region contains eutectic cementite. The thick-walled bearing housing region is prone to graphite flakes and grain coarsening; the basic phase transformation threshold temperature... Set to 780℃, gradient compensation coefficient Set to 56℃·cm, according to the relationship The local target annealing temperature of the thin-walled flange region was calculated. The target annealing temperature for the thick-walled bearing housing area is 920℃. It is 826℃, of which, This refers to the local target annealing temperature. Based on the fundamental phase transition threshold temperature, For gradient compensation coefficients, To correspond to the solidification modulus of the physical sections, a spatial annealing temperature difference of 94°C is formed between the two physical sections, so that the thin-walled flange area and the thick-walled bearing housing area have different thermodynamic driving forces.
[0031] An induction heating device equipped with multiple independently controllable heating zones is used, along with directional air nozzles to apply a non-uniform heat flow to the steering knuckle. The input power density of the induction coil corresponding to the thin-walled flange area is controlled, raising it to 920℃ at a heating rate of 15℃ / min, while the induction coil corresponding to the thick-walled bearing seat area is controlled, raising it to 826℃ at a heating rate of 10℃ / min. The solidification modulus difference at the boundary between the two physical zones is 0.8cm. When it exceeds the 0.3cm threshold, the annular jet device at the boundary is activated, according to the formula... A directional cooling airflow with a flow rate of 14.82 L / s was determined and applied, wherein, For directional cooling airflow, The baseline airflow rate is set to 12 L / s. The flow gradient adjustment coefficient is set to 0.25. The target annealing temperature for the thin-walled flange area is 920℃. The target annealing temperature for the thick-walled bearing housing region is 826℃. The reference temperature difference is set to 100℃. The directional cooling airflow carries away heat transferred laterally along the metal matrix through gas convection, cutting off the lateral heat conduction path from the high-temperature thin-walled flange area to the low-temperature thick-walled bearing housing area, creating a heat flow blocking zone, and maintaining a 94℃ spatial annealing temperature difference between the two physical sections. The directional cooling airflow forms a strong local convective heat transfer boundary at the outer surface of the interface between the two physical sections, while the metal interior maintains continuous heat conduction. When the high-temperature thin-walled flange area generates longitudinal heat conduction flux from the metal interior to the low-temperature thick-walled bearing housing area, the high-speed airflow at the outer surface of the interface will... The surface heat transfer coefficient of the region is increased to 850W / (m²·K), making the radial heat dissipation thermal resistance at the interface lower than the axial internal thermal conduction thermal resistance of the component. After the internal longitudinal heat flow reaches the interface zone, it is deflected radially towards the surface along the wall thickness and is removed by high-speed airflow through convection heat transfer, forming a continuous local heat sink accumulation zone at the interface. The thin-walled flange area continuously receives induction heating energy supply, the thick-walled bearing seat area maintains low-power heating, and the interface continuously undergoes strong convection heat removal. The three together maintain the stepped longitudinal temperature distribution inside the component at the interface, keeping the 94℃ space annealing temperature difference stable.
[0032] During the 240-minute heat preservation under a non-uniform temperature field, the system collects the actual heating rate of each physical section in real time. In the initial 30 minutes of the decomposition reaction of eutectic cementite in the thin-walled flange area, the hysteresis deviation of the actual heating rate relative to the heat power input is extracted, and the hysteresis deviation change rate is calculated. The rate is 1.8℃ / min; when the hysteresis deviation rate is greater than zero, the induction heating power density in the thin-walled flange area is increased by 8% to inject power to compensate for energy. To counteract the localized temperature drop caused by the absorption of latent heat of phase transformation during the decomposition of eutectic cementite, the target local annealing temperature of 920℃ is maintained in the thin-walled flange area, and the eutectic cementite decomposes into austenite and nodular graphite; when the rate of change of hysteresis deviation is less than or equal to zero, the control power compensates for the energy. The temperature gradually decreases to zero within a 5-minute buffer period to prevent temperature overshoot at the end of the phase transformation; in the thick-walled bearing housing region, the phase transformation rate is reduced at 826℃, limiting the diffusion flux of carbon atoms into the existing graphite sheets and inhibiting graphite sheet coarsening and austenite grain growth. The rate of change of hysteresis deviation, To compensate for power loss, during the real-time extraction and dynamic power control of hysteresis bias, the system controller synchronously acquires the actual surface temperature of the component output from the infrared temperature measurement array and the high-frequency power value of the current input induction coil at a period of 50ms. Based on the input power value, the metal mass of the thin-walled flange area, and the constant-pressure specific heat capacity of cast iron at the local target annealing temperature, the input high-frequency power value is directly divided by the product of the metal mass of the thin-walled flange area and the constant-pressure specific heat capacity to calculate the calibrated heating rate value without latent heat absorption during phase change, which is the reference heating rate. Subtracting the first-order time derivative of the theoretical reference heating rate from the actual measured temperature yields the hysteresis bias caused by the endothermic phase change of eutectic cementite. Then, the hysteresis bias is calculated by sampling 10 consecutive times. The hysteresis deviation within the cycle is fitted with a linear regression, and the slope is used to obtain the hysteresis deviation change rate. When the hysteresis deviation change rate is greater than 0, the controller adopts a proportional feedforward control algorithm, and outputs a pulse width modulation trigger pulse to the corresponding induction coil in the thin-walled flange area according to the linear gain coefficient that increases the induction heating power density by 4.44% for every 1℃ / min increase in the hysteresis deviation change rate, so as to dynamically increase the induction heating power density to offset the phase change heat flux. When the hysteresis deviation change rate decreases to 0 or below, the controller starts a 5-minute linear decay timer, and the power compensation energy is smoothly reduced to zero at a fixed slope of 1.6% per minute, so as to control the temperature fluctuation amplitude in the thin-walled flange area within 0.5℃.
[0033] After the insulation is completed, the differential cooling system is activated to reduce the local cooling rate of the thin-walled flange area. The local cooling rate of the thick-walled bearing housing area is set at 3℃ / min. The speed is set to 9℃ / min, representing the upper limit of the eutectoid transformation temperature range. Set to 740℃; according to the formula The delayed start-up cooling time of the thick-walled bearing housing region relative to the thin-walled flange region was calculated. It is 50.44 min, of which, To delay the start-up cooling time, The target annealing temperature for the thin-walled flange area is 920℃. The target annealing temperature for the thick-walled bearing housing region is 826℃. The local cooling rate for the thin-walled flange area is 3℃ / min. The local cooling rate for the thick-walled bearing housing area is 9℃ / min. The upper limit of the eutectoid transformation temperature range is 740℃. The cooling of the thin-walled flange area is started first, and the cooling of the thick-walled bearing seat area is started 50.44 minutes after it cools down, so that the two physical sections reach 740℃ at the same time and cross the eutectoid transformation temperature range of 740℃ to 720℃ at their respective configured local cooling rates, thereby eliminating thermal stress and phase transformation stress during the cooling process.
[0034] After the component completes the eutectoid transformation and cools to room temperature, the eutectic cementite in the thin-walled flange region is completely decomposed, and the graphite flake size in the thick-walled bearing seat region is suppressed. All physical sections obtain a uniformly distributed ferrite and pearlite mixed matrix structure. By using the inverse constraint relationship between the local target annealing temperature and the solidification modulus, combined with the heat flow blocking zone and phase transformation endothermic power compensation, and implementing differential cooling control based on the difference in the phase transformation starting point during the cooling stage, the variable cross-section cast iron component obtains consistent microstructure transformation and mechanical properties despite differences in geometric structure.
[0035] Example 2: In this example, a ductile iron steering knuckle for passenger vehicles was used for annealing testing. The test platform included an induction heating coil with multiple independently controllable heating zones, a ring-shaped jet device, a multi-channel infrared radiation temperature measurement array, and an online thermal stress monitoring sensor. The steering knuckle used for testing included a solidification modulus... For the thin-walled flange area of 0.4cm and solidification modulus For the 1.2cm thick-walled bearing seat area, the eutectic cementite volume fraction in the thin-walled flange area before annealing was 14.2%, and the average length of graphite flakes in the thick-walled bearing seat area was 32.5μm. The experiment included five control groups and one sample group based on the present invention: Control group A underwent global uniform furnace heating annealing at 860℃; Control group B used gradient temperature control but did not activate the annular jet device; Control group C used gradient temperature control and activated the annular jet device, but cut off the power compensation energy injection; Control group D adjusted the gradient compensation coefficient... The temperature is set to 100℃·cm; control group E does not perform delayed start-up cooling, and the thin-walled flange area and the thick-walled bearing seat area start cooling simultaneously. The sample group of this invention adopts zoned heating, heat flow interruption, power compensation and delayed start-up cooling control, wherein the basic phase change threshold temperature is... 780℃, gradient compensation coefficient The local target annealing temperature for the thin-walled flange area is 56℃·cm. The target annealing temperature for the thick-walled bearing housing area is 920℃. The temperature is 826℃, and the corresponding preset space temperature difference is 94℃; the reference airflow rate is... The flow rate is 12 L / s, and the flow gradient adjustment coefficient is... The reference temperature difference is 0.25. 100℃, directional cooling airflow rate The local cooling rate in the thin-walled flange area is 14.82 L / s. The local cooling rate of the thick-walled bearing housing area is 3℃ / min. The rate is 9℃ / min, representing the upper limit of the eutectoid transformation temperature range. The temperature is 740℃, and the start-up cooling time is delayed. The measurement time is 50.44 min. The heating power supply adopts a feedback controller with a power modulation response time of no more than 10 ms. The infrared radiation temperature measurement array has a measurement accuracy of ±0.5℃ in the range of 800℃ to 1000℃, and the sampling frequency is 20 Hz.
[0036] The induction heating equipment adopts a coaxial segmented dual-heating zone structure. The inner diameter of the induction coil in the first zone is 160mm, which is set around the outer periphery of the thin-walled flange area with a radial gap of 15mm. The inner diameter of the induction coil in the second zone is 110mm, which is sleeved on the outer periphery of the thick-walled bearing seat area with a radial gap of 12mm. A 25mm thick corundum ceramic thermal insulation and magnetic isolation ring is set axially between the two zone coils. The annular jet device is coaxially set inside the thermal insulation and magnetic isolation ring. Sixteen micro-orifice nozzles with an inward inclination angle of 45° and an aperture of 2mm are evenly opened in the circumference of the ring. Each nozzle faces the interface transition zone surface at the abrupt change of the component cross section. The multi-channel infrared radiation temperature measurement array includes four sets of optical probes, which are respectively aimed at the outer edge of the thin-walled flange, the front end of the interface zone, the rear end of the interface zone, and the geometric center of the thick-walled bearing seat. Each optical probe is connected to the multi-channel data acquisition card of the main control processor through a shielded coaxial cable to continuously collect the temperature changes of each physical section.
[0037] During the experiment, an infrared radiation thermometer continuously recorded the temperature changes of each sample group during the heating, graphitization holding, and cooling stages. After the samples were annealed and cooled to room temperature, metallographic samples were cut from the thin-walled flange area and the thick-walled bearing seat area, respectively. The residual eutectic cementite volume fraction in the thin-walled flange area and the average length of graphite flakes in the thick-walled bearing seat area were determined using a metallographic microscope. Tensile samples were prepared according to GB / T228.1-2021 to test the tensile strength of the thin-walled flange area and the thick-walled bearing seat area, as well as the elongation after fracture of the entire component. The residual phase transformation stress after the component completed the eutectoid transformation was detected using an X-ray stress meter.
[0038] From the temperature field changes during the heating and graphitization holding stages, after uniform heating, the transverse temperature difference at the interface of control sample group A was only 3.2℃; although control sample group B used gradient temperature control, the annular jet device was not turned on, and transverse heat conduction continued between the high-temperature thin-walled flange area and the low-temperature thick-walled bearing seat area, reducing the transverse temperature difference at the interface to 31.5℃; after turning on the annular jet device, the transverse temperature difference at the interface of control sample group C remained at 93.8℃; the transverse temperature differences at the interface of control sample groups D and E were 94.2℃ and 94.1℃, respectively; the sample group of the present invention used directional cooling airflow to remove transverse heat conduction at the interface, and the transverse temperature difference at the interface remained at 93.9℃. Thus, after the annular jet device was turned on, it was able to maintain a temperature difference at the interface corresponding to the local target annealing temperature of the two physical sections, whereas when only gradient heating was used, the transverse heat conduction inside the metal would significantly reduce this temperature difference.
[0039] During the endothermic decomposition of eutectic cementite, the phase change endothermic temperature drop was 12.4℃ for control sample A and 11.8℃ for control sample B. After cutting off the power compensation energy injection in control sample C, the phase change endothermic temperature drop was 10.5℃, and the temperature in the thin-walled flange area dropped to 909.5℃, with the corresponding residual eutectic cementite volume fraction remaining at 1.6%. After maintaining power compensation control, control samples D and E showed phase change endothermic temperature drops of 0.8℃ and 0.6℃, respectively. The hysteresis deviation change rate was detected in the samples of this invention. Power compensation energy is injected into the thin-walled flange area at a rate of 1.8℃ / min. The phase change heat absorption temperature drop is controlled at 0.5℃. During this process, the hysteresis deviation change rate is used to trigger the power compensation of the corresponding heating protection zone, so that the thin-walled flange area continues to maintain a temperature close to its local target annealing temperature during the decomposition heat absorption of eutectic cementite.
[0040] The temperature field and power compensation conditions are further reflected in the metallographic structure after annealing. In control sample A, the residual eutectic cementite volume fraction in the thin-walled flange region was 4.8%, and the average length of graphite flakes in the thick-walled bearing seat region reached 68.2 μm; control sample B showed 2.1% and 54.6 μm respectively; control sample C showed 1.6% and 35.8 μm respectively; and control sample D adopted... After a gradient compensation coefficient of 100℃·cm, the local target annealing temperature of the thin-walled flange area reached 1030℃, and the volume fraction of residual eutectic cementite was 0.0%. However, the average length of graphite flakes in the thick-walled bearing seat area reached 72.4μm, and grain coarsening and surface decarburization occurred simultaneously. In the control sample group E, the volume fraction of residual eutectic cementite in the thin-walled flange area was 0.0%, and the average length of graphite flakes in the thick-walled bearing seat area was 36.1μm. In the sample group of this invention, the volume fraction of residual eutectic cementite in the thin-walled flange area was 0.0%, and the eutectic cementite decomposed to form austenite and flocculent graphite. The average length of graphite flakes in the thick-walled bearing seat area was 35.2μm. The above microstructure data correspond to the actual temperature field state of each sample group: when uniformly heated or with spatial temperature difference decay, there is a different degree of cementite residue in the thin-walled flange area; when the local target annealing temperature is too high, the coarsening of graphite flakes in the thick-walled bearing seat area is more obvious.
[0041] During the cooling stage, the residual phase transformation stress of each sample group also changed with the eutectoid transformation sequence. The residual phase transformation stresses of the components in control sample group A, control sample group B, control sample group C, and control sample group D were 185.6 MPa, 142.3 MPa, 98.4 MPa, and 125.8 MPa, respectively. Control sample group E did not use delayed start cooling. The thin-walled flange area entered the eutectoid transformation first, while the thick-walled bearing seat area was still in the austenitic state. The eutectoid transformation sequence of the two physical sections was staggered, and the residual phase transformation stress of the component was 168.4 MPa. The sample group of the present invention controlled the cooling start time of the two physical sections according to the local target annealing temperature and local cooling rate, so that the two physical sections entered and crossed the eutectoid transformation temperature range simultaneously, and the residual phase transformation stress of the component was 22.4 MPa.
[0042] The tensile test results after annealing correspond to the aforementioned changes in microstructure and residual stress. In control sample A, the tensile strength of the thin-walled flange area was 720.5 MPa, and the tensile strength of the thick-walled bearing housing area was 410.2 MPa, a difference of 310.3 MPa. The elongation after fracture of the entire component was 3.2%. In control sample B, the tensile strengths of the two areas were 685.4 MPa and 465.8 MPa, respectively, with an elongation after fracture of 5.1%. In control sample C, the tensile strengths were 640.2 MPa and 512 MPa, respectively. The tensile strength of the thin-walled flange region of the present invention was 632.5 MPa, and the tensile strength of the thick-walled bearing seat region was 628.4 MPa, with a difference of 4.1 MPa. The elongation after fracture of the entire component was 12.5%. The tensile strength of the thin-walled flange region of the present invention was 632.5 MPa, and the tensile strength of the thick-walled bearing seat region was 628.4 MPa, with a difference of 4.1 MPa.
[0043] The corresponding results of each sample group in the three stages of heating, graphitization holding and cooling show that the inverse constraint relationship between the local target annealing temperature and the solidification modulus is used to control the annealing temperature of the thin-walled flange area and the thick-walled bearing seat area respectively. The heat flow blocking zone is used to maintain the spatial temperature difference between the two physical sections. The power compensation energy is used to reduce the local temperature drop caused by the endothermic decomposition of eutectic cementite. The delayed start-up cooling keeps the eutectoid transformation sequence of the two physical sections coordinated. After the combined effect of various controls, the eutectic cementite in the thin-walled flange area is decomposed, the coarsening of graphite flakes in the thick-walled bearing seat area is suppressed, and the difference in residual phase transformation stress and tensile strength between the two physical sections is reduced, so that each physical section of the component obtains a mixed matrix structure of ferrite and pearlite.
[0044] Example 3: In this example, ductile iron components with abrupt changes in cross-section and batch-to-batch fluctuations in material composition are selected for annealing treatment, wherein the solidification modulus of the extremely thin-walled region is... The solidification modulus of the ultra-thick-walled region is 0.3 cm. The austenitizing lower limit temperature of this batch of ductile iron was determined using a microcalorimeter, with a thickness of 1.5 cm. Based on this, the basic phase transformation threshold temperature was determined. The temperature was determined to be 780℃. In the abrupt change region of the cross-section where the solidification modulus difference reached 1.2cm, annealing calibration experiments were conducted using specimens with solidification moduli ranging from 0.3cm to 1.5cm. Based on the basic phase transformation threshold temperature of 780℃, multiple gradient compensation coefficients were set in the range of 50℃·cm to 60℃·cm with a step size of 2℃·cm. After metallographic microscopy, when the gradient compensation coefficient was 56℃·cm, the volume fraction of eutectic cementite in the ultrathin-walled region dropped to zero within 240min of holding time, while the austenite grain size in the ultrathick-walled region remained within 40μm. Thus, the gradient compensation coefficient was determined to be 56℃·cm. According to the inverse constraint relationship between the local target annealing temperature and the solidification modulus, the local target annealing temperature in the ultrathin-walled region was calculated to be 967℃, and in the ultrathick-walled region it was 817℃, forming a spatial annealing temperature difference of 150℃ between the two physical regions.
[0045] In gradient compensation coefficient During the calibration process, the physical regions with smaller solidification moduli experienced greater undercooling during casting and crystallization, resulting in a corresponding increase in the volume fraction of eutectic cementite and the diffusion activation barrier. The thermodynamic driving force required for the complete decomposition of eutectic cementite and the diffusion process varied with temperature. Based on this, the Arrhenius diffusion equation and the grain growth kinetic equation were used for constraint. When the eutectic cementite in the ultrathin-walled region could completely dissolve within 240 min and the grain size in the ultrathick-walled region was less than 40 μm, these were used as the convergence conditions for the iteration. The iteration was conducted within the range of 50 °C·cm to 60 °C·cm to obtain 56 °C·cm.
[0046] During the application of non-uniform heat flow in space, the solidification modulus difference at the boundary between the two physical sections was 1.2 cm, exceeding the set threshold of 0.3 cm. Therefore, the annular jet device was activated, and the reference airflow rate was adjusted. Set to 12L / s, flow gradient adjustment coefficient The value is set to 0.25, with local target annealing temperatures of 967℃ and 817℃ for the ultra-thin-walled and ultra-thick-walled regions, respectively, and the reference temperature difference is [missing value]. The temperature was set to 100°C, thus obtaining the directional cooling airflow rate. The flow rate is 16.5L / s; within the upper limit of 18L / s flow rate of the regulating valve, a 16.5L / s compressed air jet is output, so that the boundary transition zone forms a local strong convective heat transfer boundary, which carries away the heat that is conducted laterally along the metal matrix from the high temperature zone of 967℃ to the low temperature zone of 817℃, constructs a heat flow blocking zone, and maintains a space annealing temperature difference of 150℃.
[0047] The 0.3cm threshold is determined based on the difference in solidification modulus and corresponding temperature difference between adjacent physical sections. When the solidification modulus difference is less than 0.3cm, the calculated local target annealing temperature difference is less than 25℃, and the boundary temperature drop caused by lateral heat conduction is insufficient to affect the graphitization process of the ultrathin wall region. When the solidification modulus difference reaches or exceeds 0.3cm, the temperature difference between the two physical sections reaches more than 40℃, the lateral heat conduction heat flux density exceeds the critical diffusion threshold, and the boundary of the ultrathin wall region experiences a temperature drop of more than 15℃ without the application of directional cooling airflow. Therefore, 0.3cm is used as the start-up threshold for the annular jet device.
[0048] After entering the graphitization and heat preservation stage, a multi-channel infrared radiation thermometer array continuously collects the temperature of each physical section at a sampling frequency of 20Hz. During the initial 30 minutes of the solid-state decomposition reaction of the eutectic cementite in the ultra-thin-walled region, the hysteresis deviation between the actual heating rate and the input heat power is extracted and the hysteresis deviation change rate is calculated. When the hysteresis deviation change rate is greater than zero, incremental power compensation energy is injected into the ultra-thin-walled region. To compensate for the local temperature drop caused by the absorption of latent heat of phase transformation during the decomposition of eutectic cementite, the corresponding induction heating power density is increased, maintaining the ultra-thin wall region at 967℃; when the hysteresis deviation rate is less than or equal to zero, the power compensation energy is controlled. During the 5-minute buffer time The slope is gradually reduced to zero to limit temperature overshoot and surface decarburization at the end of the phase transition.
[0049] During the constant temperature holding process, the heating rate and hysteresis deviation are taken from the dynamic correction process of the closed-loop temperature control system. After reaching the local target annealing temperature, the eutectic cementite decomposes and absorbs heat, causing the temperature in the ultra-thin wall region to decrease. After detecting the temperature change, the temperature control system outputs a heating load increase command to make the temperature rise back to the local target annealing temperature. When the latent heat of phase change is continuously absorbed, the actual temperature rise rate deviates from the theoretical rise rate corresponding to the input heat power. By collecting the heating rate response hysteresis and its change with time during this correction cycle, the power compensation energy is dynamically controlled.
[0050] After the insulation is completed, the local cooling rate of the ultra-thin wall region The local cooling rate for the ultra-thick wall region is configured to be 2℃ / min. The speed is set to 10℃ / min, representing the upper limit of the eutectoid transformation temperature range. The temperature is set to 740℃. The delayed start-up cooling time is calculated based on the local target annealing temperature and local cooling rate of the two physical zones. The delayed start-up cooling time of the ultra-thick wall region relative to the ultra-thin wall region was found to be 105.8 min. The ultra-thin wall region was controlled to start cooling first, and the ultra-thick wall region was controlled to start cooling 105.8 min later, so that the two physical sections with a starting cooling temperature difference of 150℃ reached 740℃ at the same time. Then, they synchronously crossed the eutectoid transformation temperature range of 740℃ to 720℃ with their respective configured local cooling rates.
[0051] During the differentiated cooling process, for the thin-walled flange area with a high natural heat dissipation rate, the induction heating coil of the corresponding heating zone is used to apply low-frequency electromagnetic supplementary heating at 10% to 15% of the rated power to compensate for the natural radiation and convection heat dissipation of the surface, limiting its net heat dissipation cooling rate to 3℃ / min; after the thick-walled bearing seat area starts cooling, the porous air-cooled spray ring arranged on its surface is opened to continuously spray atomized airflow at a pressure of 0.35MPa to enhance surface convection heat transfer, increasing its cooling rate to 9℃ / min. At the same time, an air curtain is maintained at the junction of the two physical sections to reduce the lateral heat transfer under reverse temperature difference conditions.
[0052] After the component cools to room temperature, the eutectic cementite in the ultrathin-walled region transforms into nodular graphite, and the average length of the graphite flakes in the ultrathick-walled region is controlled within 38.2 μm. The residual phase transformation stress of the entire component is 25.1 MPa. Under the combined effect of the above annealing parameters, heat flow interruption zone, power compensation energy, and delayed start-up cooling, the ultrathin-walled region and the ultrathick-walled region complete graphitization and heat preservation according to their respective local target annealing temperatures, and coordinately enter the eutectoid transformation temperature range during the cooling stage.
[0053] Example 4: This example combines Figures 1 to 2 This paper describes a temperature gradient graphitization annealing process for cast iron components, such as... Figure 1As shown, in step S1, the ratio of the volume to the heat dissipation surface area of each physical section of the variable cross-section cast iron component is obtained, and the solidification modulus of each physical section is determined. In step S2, the local target annealing temperature of each physical section is calculated based on the solidification modulus. The local target annealing temperature is obtained by adding the quotient obtained by dividing the basic phase transformation threshold temperature and the gradient compensation coefficient by the solidification modulus, forming a reverse constraint relationship that the smaller the solidification modulus, the higher the local target annealing temperature. In step S3, a spatial non-uniform heat flow is applied to the variable cross-section cast iron component to make each physical section reach the corresponding local target annealing temperature. In step S4, the local target annealing temperature is maintained by graphitization insulation. When the difference in solidification modulus is greater than the set threshold, the local target annealing temperature is maintained. Directional cooling airflow is applied at the junction of the physical sections to construct a heat flow blocking zone and cut off the lateral heat conduction path. During the heat preservation period, the hysteresis deviation of the heating rate of each physical section relative to the heat power input is collected and the hysteresis deviation change rate is calculated. When the hysteresis deviation change rate is greater than zero, power compensation energy is injected into the physical section that produces the hysteresis deviation to offset the local temperature drop caused by the endothermic decomposition of eutectic cementite. In step S5, after the heat preservation is completed, the delayed start cooling time is calculated based on the local target annealing temperature of each physical section and the configured local cooling rate. The physical section with a larger solidification modulus is controlled to delay the start cooling time relative to the physical section with a smaller solidification modulus, and finally, each physical section is guided to enter the eutectoid transformation temperature range synchronously.
[0054] like Figure 2 As shown, the infrared temperature measurement array continuously collects the temperature of each section and transmits the monitoring data to the main control processor. The main control processor dynamically increases the induction heating power based on the input signal. The main control processor outputs control commands to the induction heating device, the annular jet device, and the differential cooling system respectively. After receiving the command, the induction heating device applies a spatially non-uniform heat flow to the variable cross-section cast iron component. After receiving the command, the annular jet device applies a cooling airflow to the junction of the variable cross-section cast iron component. After receiving the command, the differential cooling system delays the cooling of the variable cross-section cast iron component according to the cooling rate. Under the above physical interaction, the variable cross-section cast iron component synchronously enters the eutectoid transformation zone. The temperature status of the variable cross-section cast iron component is continuously fed back to the infrared temperature measurement array to form a closed-loop monitoring.
[0055] Example 5: Before annealing different batches of steering knuckles, baseline calibration was performed to address the infrared emissivity deviation caused by surface oxide scale and blank roughness. The calibration component was installed in the heating chamber, and thermocouple sensors were attached to the thin-walled flange area and the thick-walled bearing housing area, respectively. The induction coil was controlled to preheat uniformly to 400℃ at a heating rate of 100℃ / h. Simultaneously, the physicochemical temperature measured by the thermocouples and the radiation signal output by the infrared radiation temperature measurement array were acquired. The emissivity correction coefficient at a wavelength of 1.5μm was extracted by comparing the two, and the infrared radiation temperature measurement array was corrected accordingly. The sampling emissivity of the column is used to match the temperature measurement results with the actual surface condition of the component. After temperature measurement calibration is completed, a 5kW reference low-power pulse is applied to the induction coil to obtain the initial high-frequency induction damping of the corresponding induction coils in the thin-walled flange area and the thick-walled bearing seat area, and to determine the initial calibration mapping relationship between the induction power density and the surface temperature rise rate. When the deviation of the measured damping relative to the reference value exceeds 5%, the pulse width modulation duty cycle reference of the induction heating power supply is automatically corrected, and the in-situ baseline calibration of the temperature measurement path and the power coupling channel is completed before the formal application of the non-uniform heat flow in space.
[0056] During the initial high-frequency induction damping extraction process, the high-frequency sampling circuit built into the heating power supply detects the instantaneous values of the resonant voltage and resonant current across the induction coil at a frequency of 1MHz during the application of the reference low-power pulse. Based on the phase difference and amplitude ratio of the two, the equivalent series resistance in the equivalent impedance is calculated. This equivalent series resistance characterizes the electromagnetic coupling state between the workpiece and the induction coil. When the blank clamping gap or surface oxide layer fluctuation causes the measured damping to drift more than 5% relative to the reference value, the controller adjusts the pulse width modulation duty cycle of the full-bridge inverter in reverse according to the damping change rate, so that the energy coupling efficiency is restored to the calibration reference line and the temperature rise rate of each physical section is kept in the corresponding calibration state.
[0057] During continuous operation of the equipment, the thermal expansion of the induction coil and the dust accumulation at the nozzle of the annular jet device cause the heat flow blocking state at the interface to drift. The infrared radiation temperature measurement array continuously monitors the attenuation rate of the transverse temperature gradient at the transition zone between the thin-walled flange area and the thick-walled bearing seat area. When the actual temperature difference at the interface drifts downward by more than 2°C relative to the preset 94°C spatial temperature difference, the system increases the directional cooling airflow in steps of 0.5L / s to increase the convective heat dissipation at the interface, remove the excess heat conducted laterally along the metal matrix, and restore the actual temperature difference at the interface to the preset 94°C. At the same time, the power input of the induction heating power supply and the component heating response curve during the graphitization insulation stage are collected to calculate the rate of change of high-frequency induction heating efficiency with operating time. When the thermal drift of the coil gap causes the heating efficiency to decrease by more than 3%, the control system corrects the compensation increment of the induction power density to offset the power coupling parameter drift caused by continuous operation. After the above calibration and dynamic correction, the component continuously completes 500 annealing cycles, and the metallographic structure and mechanical properties of each physical section remain consistent.
[0058] Example 6: This example acquires three-dimensional geometric point cloud data of a diesel engine ductile iron crankshaft with continuous variable cross-section characteristics. The crankshaft is divided into multiple physical segments along its axial direction, including the connecting rod journal segment and the crankshaft main journal segment. The discrete voxel summation method is used to calculate the volume-to-heat dissipation surface area ratio of each physical segment, and the solidification modulus of the thin-walled connecting rod journal segment is calculated. The solidification modulus of the thick-walled section of the main journal is 0.35 cm. It is 1.4 cm; the basic phase transition threshold temperature. Set to 780℃, gradient compensation coefficient Set to 56℃·cm, according to the relationship The local target annealing temperature of the thin-walled section of the connecting rod journal was calculated. The target local annealing temperature for the thick-walled section of the main journal is 940℃. The temperature is 820℃, creating a 120℃ spatial annealing temperature difference between the two physical sections.
[0059] The solidification modulus difference at the junction of the thin-walled section of the connecting rod journal and the thick-walled section of the main journal is 1.05 cm, exceeding the set threshold of 0.3 cm. Therefore, the annular jet device at the junction is activated, and the reference airflow rate is set to [missing information]. Set to 12L / s, flow gradient adjustment coefficient Set to 0.25, reference temperature difference. Set to 100℃, according to the formula The directional cooling airflow rate was calculated. The flow rate is 15.6 L / s. A directional cooling airflow of 15.6 L / s is applied to the junction of the two physical sections to remove the heat that is transversely conducted along the crankshaft metal matrix, cut off the transverse heat transfer path from the 940℃ high-temperature thin-walled section to the 820℃ low-temperature thick-walled section, and form a heat flow blocking zone to maintain a preset 120℃ spatial annealing temperature difference at the junction.
[0060] In the induction heating equipment, multiple independent high-frequency inverter power supplies are set up for each physical section of the crankshaft. A ring-shaped water-cooled copper electromagnetic shielding plate is set between the induction coils of the connecting rod journal and the main journal to reduce the electromagnetic cross-coupling of the high-frequency magnetic field between adjacent physical sections. The ring jet device is composed of two semi-circular stainless steel air collecting ring pipes spliced together. The inner wall of the ring pipe is equipped with double rows of staggered micro-contraction nozzles along the circumference. The angle between the nozzle axis and the crankshaft axis is 60°. The jet airflow forms a continuous annular high-speed air curtain with a thickness of 8mm on the metal surface at the junction, and the output flow rate is adjusted by an air pressure reducing proportional valve and a digital mass flow meter.
[0061] The system was subjected to graphitization and holding for 240 minutes under a non-uniform temperature field. The actual heating rate of each physical section of the crankshaft was continuously collected. During the initial 30 minutes of eutectic cementite decomposition in the thin-walled section of the connecting rod journal, the hysteresis deviation of the actual heating rate relative to the heat power input was extracted, and the rate of change of hysteresis deviation was calculated. In this embodiment, the hysteresis deviation change rate was measured to be 1.6℃ / min. When the hysteresis deviation change rate is greater than zero, the induction heating power density of the thin-walled section of the connecting rod journal is increased by 7%, and power compensation energy is injected into this physical section. To compensate for the local temperature drop caused by the absorption of latent heat of phase transformation during the decomposition of eutectic cementite, the temperature is maintained at the local target annealing temperature of 940℃. The eutectic cementite decomposes to form austenite and nodular graphite. When the rate of change of hysteresis deviation is less than or equal to zero, the power is controlled to compensate for energy loss. The temperature gradually decreases to zero within a 5-minute buffer period, while the thick-walled section of the main journal remains at 820°C, limiting the diffusion flux of carbon atoms into the existing graphite sheet and inhibiting graphite sheet coarsening and austenite grain growth.
[0062] After the graphitization insulation is completed, the differential cooling system is activated to reduce the local cooling rate of the thin-walled section of the connecting rod journal. The cooling rate is set to 2.5℃ / min to reduce the local cooling rate of the thick-walled section of the main journal. The speed is set to 8.5℃ / min, representing the upper limit of the eutectoid transformation temperature range. Set to 740℃, according to the formula Calculate the delayed start-up cooling time of the thick-walled section of the main journal relative to the thin-walled section of the connecting rod journal. After 70.59 min, the thin-walled section of the connecting rod journal was cooled first, and after 70.59 min of cooling, the thick-walled section of the main journal was cooled first, so that the two physical sections reached 740℃ at the same time. Then, they were cooled synchronously through the eutectoid transformation temperature range of 740℃ to 720℃ with their respective configured local cooling rates.
[0063] The differential cooling system features an air-liquid mixing spray cooling sleeve around the thick-walled section of the main journal, while the thin-walled section of the connecting rod journal is weakly heated by pulses with a small duty cycle applied by an independent induction coil. During the cooling process, the main controller adjusts the opening of the air-liquid mixing proportional solenoid valve of the thick-walled section cooling sleeve using a proportional-integral-derivative algorithm based on the real-time deviation between the infrared temperature measurement value and the preset cooling curve. This closed-loop adjustment of the spray flow rate and compressed air pressure at a frequency of 10 times per second maintains a local cooling rate of 8.5℃ / min for the thick-walled section of the main journal. Simultaneously, the low-frequency heating duty cycle of the induction coil in the thin-walled section of the connecting rod journal is adjusted to maintain a local cooling rate of 2.5℃ / min for this physical section.
[0064] After the crankshaft completes the eutectoid transformation and cools to room temperature, the eutectic cementite in the thin-walled section of the connecting rod journal is completely decomposed, and the average length of the graphite flakes in the thick-walled section of the main journal is controlled within 36.8 μm. A uniformly distributed ferrite and pearlite mixed matrix structure is formed in each physical section. The residual phase transformation stress of the entire crankshaft is 24.2 MPa. The tensile strengths of the thin-walled section of the connecting rod journal and the thick-walled section of the main journal are 638.2 MPa and 634.5 MPa, respectively, with a cross-sectional strength difference of 3.7 MPa.
[0065] The embodiments of this application have been described above with reference to the accompanying drawings. Unless otherwise specified, the embodiments and features in the embodiments of this application can be combined with each other. This application is not limited to the specific embodiments described above. The specific embodiments described above are merely illustrative and not restrictive. Those skilled in the art can make many other forms under the guidance of this application without departing from the spirit of this application and the scope of protection of this invention, and all of these forms are within the protection scope of this application.
Claims
1. A temperature gradient graphitization annealing process for cast iron components, characterized in that, Includes the following steps: Step S1: Obtain the ratio of the volume to the heat dissipation surface area of each physical section of the variable cross-section cast iron component, and determine the solidification modulus of each physical section. Step S2: Calculate the local target annealing temperature of each physical section based on the solidification modulus. Add the quotient obtained by dividing the basic phase transformation threshold temperature and the gradient compensation coefficient by the solidification modulus to obtain the local target annealing temperature, thus forming an inverse constraint relationship that the smaller the solidification modulus, the higher the local target annealing temperature. Step S3: Apply spatial non-uniform heat flow to the variable cross-section cast iron component so that each physical section reaches the corresponding local target annealing temperature; Step S4: Maintain the local target annealing temperature for graphitization heat preservation. Apply directional cooling airflow to the boundary of adjacent physical sections where the difference in solidification modulus is greater than a set threshold to construct a heat flow blocking zone, cut off the lateral heat conduction path, and collect the hysteresis deviation of the heating rate of each physical section relative to the heat power input during the heat preservation period and calculate the hysteresis deviation change rate. When the hysteresis deviation change rate is greater than zero, inject power compensation energy into the physical section that produces the hysteresis deviation to offset the local temperature drop caused by the endothermic decomposition of eutectic cementite. Step S5: After the heat preservation is completed, the delayed start cooling time is calculated based on the local target annealing temperature and the configured local cooling rate of each physical section. The physical section with a larger solidification modulus is controlled to delay the start cooling time relative to the physical section with a smaller solidification modulus, so as to guide each physical section to enter the eutectoid transformation temperature range synchronously.
2. The temperature gradient graphitization annealing process for cast iron components according to claim 1, characterized in that, In step S2, the local target annealing temperature is calculated according to the following formula: ,in, This refers to the local target annealing temperature of the corresponding physical section. It is the basic phase transformation threshold temperature, and its value range covers the lower limit temperature of austenitization of variable cross-section cast iron component materials; For gradient compensation coefficients, This represents the solidification modulus of the corresponding physical region.
3. The temperature gradient graphitization annealing process for cast iron components according to claim 2, characterized in that, The basic phase transition threshold temperature was set to 780℃, and the gradient compensation coefficient was set to 56℃·cm. For the thin-walled physical section with a solidification modulus of 0.4cm, the calculated local target annealing temperature was 920℃. For the thick-walled physical section with a solidification modulus of 1.2cm, the calculated local target annealing temperature was 826℃.
4. The temperature gradient graphitization annealing process for cast iron components according to claim 1, characterized in that, In step S4, including step S41, at the boundary where the difference in solidification modulus between adjacent physical sections is greater than 0.3 cm, the annular jet device is turned on to apply a cooling airflow with a flow rate of 12 L / s to 15 L / s to the boundary, so as to remove the lateral heat conducted from the higher temperature physical section to the lower temperature physical section and maintain the spatial temperature difference between adjacent physical sections.
5. The temperature gradient graphitization annealing process for cast iron components according to claim 1, characterized in that, In step S4, including step S42, during the graphitization heat preservation period, when the rate of change of hysteresis deviation is greater than zero, the induction heating power density corresponding to the physical section that generates hysteresis deviation is increased, and the injected power compensation energy is used to offset the local temperature drop caused by the decomposition and absorption of latent heat of phase transformation of eutectic cementite; when the rate of change of hysteresis deviation is less than or equal to zero, the power compensation energy is controlled to decrease to zero within a 5-minute buffer time to keep the local target annealing temperature stable.
6. The temperature gradient graphitization annealing process for cast iron components according to claim 1, characterized in that, In step S5, the eutectoid transformation temperature range is 720℃ to 740℃. The delayed start-up cooling time of the thick-walled physical section with a larger solidification modulus relative to the thin-walled physical section with a smaller solidification modulus is calculated using the following formula: ,in, To delay the start-up cooling time, and These are the local target annealing temperatures for the thin-walled and thick-walled physical sections, respectively. and The local cooling rates are configured for the thin-walled and thick-walled physical sections, respectively. The upper limit of the eutectoid transformation temperature range is set to 740℃.
7. The temperature gradient graphitization annealing process for cast iron components according to claim 6, characterized in that, In step S5, including step S51, a local cooling rate of 3℃ / min is configured for the thin-walled physical section with a solidification modulus of 0.4cm, and a local cooling rate of 9℃ / min is configured for the thick-walled physical section with a solidification modulus of 1.2cm; the thin-walled physical section is controlled to start cooling first, and after the thin-walled physical section has been cooled for 50.44min, the thick-walled physical section is controlled to start cooling, guiding the thin-walled physical section and the thick-walled physical section to reach and pass through the eutectoid transformation temperature range of 720℃ to 740℃ simultaneously.
8. The temperature gradient graphitization annealing process for cast iron components according to claim 1, characterized in that, In step S3, including step S31, an induction heating device equipped with multiple independent and controllable heating zones is used to apply a spatially non-uniform heat flow to the variable cross-section cast iron component; the thin-walled physical section with a solidification modulus of 0.4 cm is heated to 920°C at a heating rate of 15°C / min, and the thick-walled physical section with a solidification modulus of 1.2 cm is heated to 826°C at a heating rate of 10°C / min.
9. The temperature gradient graphitization annealing process for cast iron components according to claim 1, characterized in that, In step S4, the time for maintaining graphitization under a non-uniform temperature field is set to 240 min. During the holding period, the eutectic cementite in the thin-walled physical section with a solidification modulus of 0.4 cm decomposes into austenite and flocculent graphite, and the diffusion flux of carbon atoms to the existing graphite sheet in the thick-walled physical section with a solidification modulus of 1.2 cm is suppressed, preventing graphite sheet coarsening and austenite grain growth.
10. The temperature gradient graphitization annealing process for cast iron components according to claim 1, characterized in that, In step S5, including step S52, after each physical section simultaneously passes through the eutectoid transformation temperature range of 720°C to 740°C, the variable cross-section cast iron component is cooled to room temperature, so that each physical section of the variable cross-section cast iron component obtains a uniformly distributed ferrite and pearlite mixed matrix structure.
Citation Information
Patent Citations
Annealing process of castable iron
CN101988143A