A method for recycling valuable metals from waste ternary lithium battery black powder
By combining P204 semi-extraction and real-time controlled 984 extraction technology with P507 extraction and lithium concentration treatment, the problem of incomplete separation of copper and manganese in waste ternary lithium battery black powder has been solved, achieving efficient and clean recovery of valuable metals and improving recovery rate and economic efficiency.
Patent Information
- Application Number
- CN202611263489.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for recovering valuable metals from waste ternary lithium battery black powder suffer from problems such as incomplete separation of copper and manganese, resource waste, and high energy consumption. In particular, fluctuations in copper content cause traditional process parameters to fail, making it difficult to achieve high-purity separation and efficient recovery.
After copper and manganese were separated by P204 semi-extraction, the copper ion concentration was monitored in real time, and the ratio and extraction stage of 984 extraction were adaptively adjusted. Combined with P507 semi-extraction and full extraction, copper and manganese were separated. Cobalt, magnesium, nickel and lithium were separated by lithium concentration treatment. A dynamic control system was established to adapt to raw material fluctuations.
It achieves high-purity separation of copper and manganese, reduces concentration energy consumption, improves recovery rate and economic efficiency, avoids resource waste, and provides an efficient and clean technology for the recovery of valuable metals.
Smart Images

Figure CN123108317A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of secondary battery technology, specifically to a method for recycling and processing valuable metals from waste ternary lithium batteries. Background Technology
[0002] In the context of new energy development, spent ternary lithium batteries occupy a central position among spent secondary batteries. After discharge, dismantling, crushing, sorting, and separation, they yield black powder containing various valuable metal elements such as lithium, nickel, manganese, and copper, which seriously harm the environment and human health. Therefore, it is necessary to rationally recycle spent ternary lithium batteries, recovering the economically valuable metals from their black powder, realizing the recycling of valuable metal resources in secondary batteries, and reducing heavy metal pollution in the environment.
[0003] While hydrometallurgy is currently the mainstream process for recycling valuable metals from spent ternary lithium battery black powder, offering advantages such as high leaching rates and relatively low costs, it is prone to generating harmful gases like chlorine and sulfur trioxide during acid leaching, posing significant environmental challenges. Emerging salt fusion roasting technology, while improving the leaching rate of valuable metals, neglects the separation of trace amounts of copper in the black powder, resulting in crude copper-manganese mixed salts that fail to meet high-purity separation requirements. Furthermore, copper foil is often mixed into the black powder during dismantling, causing significant fluctuations in copper content. Traditional acid leaching-extraction-precipitation processes often employ a fixed ratio (O / A) and extraction stage, lacking the ability to dynamically adapt to copper content fluctuations, thus failing to achieve efficient copper-manganese separation. This not only wastes valuable metal resources but also increases recycling costs. Summary of the Invention
[0004] To address the aforementioned technical problems, this application provides a method for recycling and processing valuable metals from waste ternary lithium battery black powder, thereby resolving the existing issues.
[0005] The present application discloses a method for recycling and processing valuable metals from waste ternary lithium battery black powder, which adopts the following technical solution: The obtained waste ternary lithium battery black powder raw material was subjected to acid leaching and iron and aluminum removal, and P204 semi-extraction was used to strip out a mixed solution rich in copper and manganese and raffinate 1. The mass concentration of copper ions in the mixture is detected in real time, the significance of the copper concentration deviating from the standard mass concentration range is calculated, and the ratio and extraction stage of 984 extraction are adaptively adjusted. The mixture is then subjected to 984 extraction according to the adjusted ratio and extraction stage to complete the separation of copper and manganese and obtain manganese-containing raffinate. The raffinate 1 was subjected to P507 semi-extraction, P507 full extraction and lithium concentration treatment in sequence to complete the separation of cobalt, magnesium, nickel and lithium.
[0006] Preferably, the specific process of using P204 semi-extraction to strip out the mixture rich in copper and manganese includes: The liquid after iron and aluminum removal was subjected to countercurrent extraction using P204 extractant to obtain a loaded organic phase and raffinate 1. The organic phase of the countercurrent extraction was a mixture of 20% P204, 5% TBP and sulfonated kerosene. The O / A ratio of the countercurrent extraction was set to 1:2, and the number of countercurrent extraction stages was 11. The loaded organic phase was back-extracted using a 2.6 mol / L sulfuric acid solution to obtain a mixed solution containing copper sulfate and manganese sulfate.
[0007] Preferably, the calculation of the significant deviation of the copper concentration from the standard mass concentration range, and the adaptive adjustment of the ratio and extraction stage of 984 extraction, includes: Obtain the current copper ion mass concentration of the mixture. And obtain the preset standard mass concentration range of copper ions. ;like If the concentration is within the standard mass concentration range, the ratio and extraction stage of the 984 extraction are set to the preset standard ratio and standard extraction stage, respectively. , These represent the preset lower limit of standard mass concentration and the preset upper limit of standard mass concentration, respectively. like Less than Through formula Calculate the significance The standard comparison is reduced based on the degree of significance, and the adjusted extraction stage is maintained at the standard extraction stage. Represents the hyperbolic tangent function; like Greater than Through formula Calculate the significance The standard comparison and standard extraction stages were amplified based on the degree of significance, and were used as adjusted comparison and extraction stages.
[0008] Preferably, the specific process of using the comparison based on the significance reduction standard as the adjusted comparison is as follows: Calculate the product of the preset reduction factor and the obtained significance level, multiply the difference between the value 1 and the product by the preset standard comparison to obtain the adjusted comparison.
[0009] Preferably, the specific process for comparing based on the significance amplification standard is as follows: Calculate the product of the preset amplification factor and the obtained significance level, multiply the sum of the product of the value 1 and the product by a preset standard, and obtain the adjusted comparison.
[0010] Preferably, the process of amplifying the standard extraction stage based on the significance level includes: The adjusted extraction level is obtained by multiplying the calculated significance level by the range of the preset extraction level interval, and adding the preset lower limit of the extraction level.
[0011] Preferably, the step of performing 984 extraction on the mixture according to the adjusted ratio and extraction stage to complete the copper-manganese separation and obtain the manganese-containing raffinate is as follows: First, the pH of the mixture is adjusted using an alkaline neutralizing agent; the organic phase of the 984 extractant is a mixture of 30% 984 and sulfonated kerosene, the extraction ratio is set to the adjusted ratio, and the flow rate ratio of the pumped organic phase to the mixture is controlled to be equal to the adjusted ratio, and the number of countercurrent extraction stages is set to the adjusted number of extraction stages; after completing the countercurrent extraction, the copper-loaded organic phase and raffinate 2 are obtained, wherein raffinate 2 is a manganese-containing raffinate; The copper-loaded organic phase was back-extracted using a 1.5 mol / L sulfuric acid solution to obtain a copper sulfate solution.
[0012] Preferably, the specific operation of performing P507 semi-extraction is as follows: The raffinate 1 was subjected to countercurrent extraction using P507 extractant to obtain an organic phase loaded with cobalt and magnesium, as well as raffinate 3. The organic phase of the countercurrent extraction was a mixture of 25% P507, 5% TBP and sulfonated kerosene, with a nickel soap saponification rate of 60%. The extraction ratio was set to 1:1.5, and the number of countercurrent extraction stages was 11. The organic phase loaded with cobalt and magnesium was subjected to serial stepwise back-extraction: first, back-extraction was performed with a 1.5 mol / L sulfuric acid solution to obtain a magnesium sulfate solution, and then back-extraction was performed with a 2.6 mol / L sulfuric acid solution to obtain a cobalt sulfate solution.
[0013] Preferably, the specific process of the P507 full extraction is as follows: The raffinate 3 was subjected to countercurrent extraction using P507 extractant to obtain a nickel-rich organic phase and raffinate 4. The organic phase for countercurrent extraction was a mixture of 25% P507, 5% TBP and sulfonated kerosene. The organic phase was subjected to saponification treatment to maintain the saponification rate at 60%~70%. The extraction ratio was set to 1.5:1 and the number of countercurrent extraction stages was 8. The nickel-rich organic phase was back-extracted using a 2.6 mol / L sulfuric acid solution to obtain a nickel sulfate solution.
[0014] Preferably, the specific operation of the lithium concentration treatment includes: evaporating and concentrating the raffinate 4 until the lithium mass concentration in the solution reaches 15~20g / L, to obtain a mixed concentrate containing lithium sulfate and sodium sulfate.
[0015] This application has at least the following beneficial effects: To address the shortcomings of traditional processes that treat trace amounts of copper as impurities for removal or only produce crude mixed salts, this application separates copper and manganese midway through the main process after acid leaching for impurity removal. Utilizing the excellent selectivity of 984 extractant for copper ions, high-purity separation of copper and manganese is achieved, avoiding the low-value waste of copper resources. This synergistic process not only improves the purity of copper-manganese separation but also prevents the volume expansion of the lithium solution in the subsequent raffinate 1, significantly reducing concentration energy consumption and improving the overall economic efficiency and synergy of the process.
[0016] To address the issue of fluctuating copper content in black powder raw materials leading to the failure of fixed extraction parameters, this application establishes an adaptive control system based on real-time monitoring. By monitoring the mass concentration of copper ions in the mixed solution in real time, the system accurately calculates the significance of its deviation from the standard range and dynamically adjusts the ratio (O / A) and extraction stage of 984 extraction accordingly. This mechanism ensures that ineffective consumption of extractant and resource waste are avoided at low copper concentrations, while guaranteeing sufficient transfer of copper ions into the organic phase at high copper concentrations. This effectively resolves the contradiction between raw material fluctuations and fixed process parameters, significantly improves the copper ion extraction rate and copper-manganese separation purity, and enhances the process's adaptability and robustness to high-copper raw materials.
[0017] After copper and manganese are separated by P204 semi-extraction, the raffinate 1 is sequentially subjected to P507 semi-extraction, full extraction, and lithium concentration treatment, achieving precise separation of cobalt, magnesium, nickel, and lithium. This approach avoids the interference of incomplete copper and manganese separation in traditional processes on subsequent nickel, cobalt, and lithium extraction, improving the purity and recovery rate of each metal product. Simultaneously, the adaptive control mechanism reduces ineffective solvent recycling and energy consumption, lowers acid and alkali consumption and secondary pollution, achieving efficient, clean, and high-value recovery of valuable metals from waste ternary lithium battery black powder, providing the industry with a replicable short-process, low-energy-consumption recovery technology paradigm. Attached Figure Description
[0018] Figure 1 This application provides a flowchart of the steps involved in the recycling and processing of valuable metals from waste ternary lithium batteries. Detailed Implementation
[0019] Four tons of waste ternary lithium battery black powder raw materials were obtained. The black powder mainly contains valuable metals such as iron, aluminum, copper, manganese, cobalt, magnesium, nickel and lithium, as shown in Table 1.
[0020] Table 1. Main components of black powder from waste ternary lithium batteries (wt%)
[0021] To achieve efficient recovery of valuable metals from waste ternary lithium battery black powder, especially to improve the purity of copper and manganese ion separation, this application proposes a method for recovering and processing valuable metals from waste ternary lithium battery black powder. Figure 1The flowchart for recycling and processing valuable metals from waste ternary lithium batteries mainly includes the following steps: Step 1: The obtained waste ternary lithium battery black powder raw material is subjected to acid leaching and iron and aluminum removal, and P204 semi-extraction is used to strip out a mixed solution rich in copper and manganese and raffinate 1.
[0022] (101) Acid leaching: Add black powder to the reaction vessel and add reducing agent (sodium sulfite) and sulfuric acid for reduction acid leaching. The pH value of the acid leaching solution is maintained in the range of 2 to 3, the liquid-solid ratio is 4:1, the heating temperature is 60 to 80℃, and the reaction time is 2 to 3 hours. After the reaction is completed, filter to obtain leaching residue (mainly containing carbon powder and a small amount of undissolved matter) and leaching solution.
[0023] (102) Removal of iron and aluminum: Using crude nickel hydroxide or crude cobalt hydroxide as a neutralizing agent, the pH of the leachate is adjusted to 4~4.5 to remove iron and aluminum as much as possible. Since a small amount of cobalt and nickel may also form precipitates in this reaction environment, the iron and aluminum slag will also contain a small amount of cobalt and nickel. The iron, aluminum, cobalt and nickel slag (about 120 kg after acid washing to recover cobalt and nickel) and the liquid after removing iron and aluminum are obtained by pressure filtration.
[0024] (103) P204 Semi-extraction (Simultaneous enrichment of copper and manganese): The liquid after iron and aluminum removal is semi-extracted using P204 extractant. The organic phase consists of 20% P204 (di(2-ethylhexyl)phosphoric acid) + 5% TBP (tributyl phosphate) + sulfonated kerosene, with an O / A ratio of 1:2. After 11 stages of countercurrent extraction, copper and manganese are introduced into the organic phase. After the countercurrent extraction is completed, the loaded organic phase (mainly containing copper and manganese valuable metals) and raffinate 1 (mainly containing nickel, cobalt, magnesium, and lithium valuable metals) are obtained. Then, the loaded organic phase is counter-extracted with 2.6 mol / L sulfuric acid to obtain a mixed solution containing copper sulfate and manganese sulfate. In this step, copper and manganese are "stripped away halfway" from the main process route, creating favorable conditions for subsequent copper-manganese separation and nickel-cobalt-magnesium-lithium separation. Countercurrent extraction is a well-known technology, and the specific implementation process will not be described in detail.
[0025] Step 2: Real-time detection of copper ion mass concentration in the mixture, calculation of the degree of deviation of copper concentration from the standard mass concentration range, adaptive adjustment of the ratio and extraction stage of 984 extraction, and 984 extraction of the mixture according to the adjusted ratio and extraction stage to complete copper-manganese separation and obtain manganese-containing raffinate.
[0026] Because the copper content in waste ternary lithium battery black powder is relatively low, current processes for recycling valuable metals from waste ternary lithium battery black powder mainly use P204 and P507 (2-ethylhexylphosphonic acid mono-2-ethylhexyl ester) as extractants. In these processes, the handling of trace amounts of copper often faces a dilemma: some processes treat it as an impurity and remove it directly, or only produce it as a crude copper-manganese mixed salt with low value, or even completely abandon recycling altogether. This crude approach not only makes it difficult to achieve high-purity separation of copper and manganese, but also leads to a serious waste of valuable metal resources and low recycling efficiency. Based on the excellent selectivity of 984 extractant (referring to LIX984 copper extractant) for copper ions, this application utilizes its characteristic of preferentially extracting copper ions and enriching them in the organic phase, while retaining manganese ions in the aqueous raffinate, thus achieving efficient separation and high-purity purification of copper and manganese ions.
[0027] (201) 984 extraction to separate copper and manganese: 984 extractant was used to extract a mixture of copper sulfate and manganese sulfate, wherein the organic phase was 30% 984 + sulfonated kerosene. By selecting a suitable phase ratio and extraction stage, the copper ions in the mixture were fully introduced into the organic phase, while the manganese ions remained in the raffinate.
[0028] Copper foil is often mixed in with the black powder from waste ternary lithium batteries during the dismantling process, causing significant fluctuations in the copper content of the raw materials. If the 984 extraction process still uses a fixed phase ratio and extraction stage, it will be difficult to adapt to this fluctuation: if the phase ratio or extraction stage is insufficient, copper ions cannot be fully transferred into the organic phase, resulting in a decrease in recovery rate; conversely, an excessively high phase ratio or extraction stage will lead to ineffective consumption of extractant and waste of resources. Therefore, this application establishes a dynamic control mechanism to flexibly adjust the extraction parameters according to the real-time copper content, so as to balance efficient copper recovery and economical utilization of extractant.
[0029] To obtain the real-time mass concentration of copper ions in the leachate of spent ternary lithium battery black powder, the mixed solution in the main delivery pipeline is introduced into a buffer storage container. An alkaline neutralizing agent is then added to the buffer storage container to adjust and maintain its pH value within the suitable weakly acidic range for 984 extraction (e.g., 1.5~2.5). The mixed solution is monitored online using inductively coupled plasma optical emission spectrometry (ICP-AES). After the analysis data is output, based on the matching relationship between copper ion concentration and the extraction equilibrium model, the ratio and extraction stage of the 984 extraction process are adaptively calculated and adjusted. Subsequently, the mixed solution in the buffer storage tank is pumped into the 984 extraction subprocess according to the optimized parameters via a metering pump, achieving precise matching between extraction parameters and raw material fluctuations, laying the foundation for subsequent high-purity copper-manganese separation.
[0030] In conventional ternary cathode materials, the copper content is extremely low (e.g., the copper content in NCM111 cathode material is only about 0.0015%). However, due to the mixing of copper foil during battery dismantling, the copper content in waste black powder can reach 1% to 2% or even higher. In actual waste ternary lithium battery black powder processing, the copper content is generally about 1.7%. To establish a process benchmark for the copper ion concentration in the mixture after P204 semi-extraction, this application defines a standard mass concentration range. This range is based on historical production data from multiple batches (with raw material copper content controlled within the range of 1.6% to 1.8%). , These represent the lower and upper limits of the copper ion mass concentration in the mixed solution within this batch range, respectively. This range serves as a reference for subsequent adaptive adjustment of the 984 extraction process parameters. When the real-time detected concentration deviates from this range, the system will trigger a parameter correction mechanism to ensure the stability and efficiency of copper-manganese separation.
[0031] 984 extractant is mainly used to extract copper ions. Generally, the ratio of copper to manganese (O / A) and the number of extraction stages directly affect the extraction rate of copper ions during the extraction and separation of copper and manganese using 984. The mass concentration of copper ions usually directly affects the O / A ratio and the number of extraction stages. In order to ensure that copper ions are fully converted into the organic phase and that the consumption cost of 984 extractant is low, a high copper ion mass concentration usually requires a high O / A ratio and a high number of extraction stages, while a low copper ion mass concentration usually requires a low O / A ratio and a low number of extraction stages.
[0032] To assess the extent to which the copper ion concentration in the mixed solution deviates from the standard concentration range during the current recycling process of valuable metals from waste ternary lithium battery black powder, the copper ion concentration P in the mixed solution during the current recycling process of valuable metals from waste ternary lithium battery black powder was obtained.
[0033] If P is within the standard mass concentration range Within this embodiment, the ratio O / A and extraction stages in the copper-manganese extraction and separation process of 984 are set as standard ratio and standard extraction stages, respectively. In this embodiment, the standard ratio and standard extraction stages are set to 1:1 and 3 stages, respectively, based on the recovery of valuable metals. It should be noted that the ratios used in the calculations are all algebraic operations performed using floating-point ratios of the organic phase to the aqueous phase volumes. , These represent the preset lower limit and upper limit of the standard mass concentration, respectively.
[0034] If P is less than This indicates that the copper ion concentration in the mixture is low at this point, and the ratio O / A should be appropriately reduced to avoid excessive ineffective extraction and wasting the 984 extractant resources. Specifically, calculations... , This is used to characterize the degree to which the copper ion concentration in the mixed solution deviates significantly from the standard concentration range during the current recycling process of valuable metals from spent ternary lithium battery black powder. Based on the fluctuations in copper content in the aforementioned black powder raw materials, it is known that the copper ion concentration in the mixed solution typically does not deviate significantly from the standard concentration range during subsequent recycling. To avoid drastic fluctuations in the adjustment ratio due to a sharp drop in the original solution concentration, which could affect extraction stability, a hyperbolic tangent function is introduced here. A smoothing shrinkage mapping is performed to normalize the significance level to the interval between 0 and 1. Then, the following is used... Adjust the O / A ratio to obtain the adaptively adjusted ratio. The ,in, Compared to the standard, This represents the reduction factor, ensuring that the adjusted comparison value ranges within... Within this embodiment, therefore Values .
[0035] It should be noted that the relative O / A range in the 984 extraction and separation process of copper and manganese is generally [range missing]. The number of extraction stages is generally not less than 3. The upper limit of the number of extraction stages can be limited by the implementer based on the specific conditions of the recovery process equipment. In this embodiment, the upper limit of the number of extraction stages is 6. Since the standard number of extraction stages is 3, the number of stages cannot be reduced further. Therefore, P is less than 6. The extraction stage is still set to 3 stages.
[0036] Compared with the 984 extractant, which is based on the adaptive copper ion mass concentration, copper ions are fully introduced into the organic phase, avoiding copper ion waste and improving the purity of copper-manganese separation.
[0037] If P is greater than This indicates that the copper ion concentration in the mixture is high at this point. The ratio of O / A and the number of extraction stages should be appropriately increased to prevent insufficient entry of copper ions into the organic phase, which would result in low copper-manganese separation purity. Specifically, calculations... In extremely rare cases, such as during the disassembly of lithium batteries, the internal copper foil may be almost completely crushed and mixed into the black powder raw material, resulting in... For cases greater than 1, the hyperbolic tangent function is used. Normalization is performed. Then, the following steps are taken: Adjusting the O / A ratio to obtain The ,in This represents the magnification factor, ensuring that the adjusted relative value ranges from 100%. ,therefore Set it to 2. Simultaneously use... Adjusting the extraction stage to obtain ,in, This indicates rounding up to the nearest integer, ensuring that the extraction level is an integer. These represent the lower and upper limits of the extraction stage, with values of 3 and 6 respectively.
[0038] Taking a ratio of 1:1 and three extraction stages as an example, the inlet and outlet of the first stage extraction tower in countercurrent extraction serve as the inlet of the mixed liquid (aqueous phase) and the outlet of the 984 extractant (organic phase), respectively. The inlet and outlet of the third stage extraction tower serve as the inlet of the 984 extractant and the outlet of the mixed liquid, respectively. The valves between the first, second, and third stage extraction towers are open to maintain normal communication between the first to third stage extraction towers. For every 1 volume of organic phase pumped in, there is a corresponding 1 volume of aqueous phase pumped in. Since the inlet areas of the organic phase and aqueous phase in the extraction towers are the same in this embodiment, the flow rate ratio of the pumped organic phase and aqueous phase is equal to the ratio.
[0039] Compared to traditional fixed extraction stages, adaptive extraction stages can be set according to the mass concentration of copper ions in the mixture, avoiding the situation where the extraction stages are set too small or too large, resulting in insufficient entry of copper ions into the organic phase or waste of 984 extractant.
[0040] Furthermore, in the 984 extraction and separation process for copper and manganese, a ratio of O / A is set... The number of extraction stages is After extraction, an organic phase (mainly containing copper, a valuable metal) and raffinate 2 (mainly containing manganese, a valuable metal) are obtained. Raffinate 2 is a manganese sulfate solution. Then, the organic phase is back-extracted with 1.5 mol / L sulfuric acid to obtain a copper sulfate solution.
[0041] This step, through adaptive ratio and extraction stages, can fully convert copper ions in the mixture into the organic phase, while avoiding the waste of 984 extractant caused by setting too many extraction stages, thereby achieving high-purity separation of copper and manganese and extracting a single valuable metal product.
[0042] Step 3: The raffinate 1 is subjected to P507 semi-extraction, P507 full extraction and lithium concentration treatment in sequence to complete the separation of cobalt, magnesium, nickel and lithium.
[0043] (301) P507 semi-extraction (simultaneous enrichment of cobalt and magnesium): The raffinate 1 obtained from the P204 semi-extraction was extracted using P507 extractant. The organic phase consisted of 25% P507 + 5% TBP + sulfonated kerosene, with a nickel soap saponification rate of 60% and an O / A ratio of 1:1.5. After 11 stages of countercurrent extraction, cobalt and magnesium entered the organic phase together. After the countercurrent extraction was completed, the organic phase (mainly containing valuable metals such as cobalt and magnesium) and raffinate 3 (mainly containing valuable metals such as nickel and lithium) were obtained. Then, a serial stepwise back-extraction was performed. First, a magnesium sulfate solution was obtained by back-extraction with a 1.5 mol / L sulfuric acid solution, and then a cobalt sulfate solution was obtained by back-extraction with a 2.6 mol / L sulfuric acid solution. This step achieved simultaneous enrichment and separate separation of cobalt and magnesium.
[0044] (302) P507 full extraction (nickel-lithium separation): The P507 extractant was used to extract the raffinate 3 obtained from the P507 semi-extraction. The organic phase was 25% P507 + 5% TBP + sulfonated kerosene. The organic phase was saponified to maintain the saponification rate at 60%~70%. The extraction ratio O / A = 1.5:1. After 8 stages of countercurrent extraction, nickel was extracted into the organic phase, while lithium remained in the raffinate. After the countercurrent extraction was completed, the organic phase (mainly containing nickel valuable metal) and raffinate 4 (mainly containing lithium and sodium valuable metal) were obtained. Then, the organic phase was back-extracted with 2.6 mol / L sulfuric acid solution to obtain nickel sulfate solution.
[0045] (303) Lithium Concentration: The raffinate 4 is finally concentrated by evaporation to a lithium mass concentration of 15~20 g / L, yielding a mixed concentrate of lithium sulfate and sodium sulfate, which can be used to further prepare industrial-grade lithium salt products. In this process, lithium ions do not accumulate throughout and flow as an aqueous phase through the extraction tank, with minimal volume expansion. This significantly reduces the amount of water that needs to be evaporated during subsequent lithium concentration, allowing for controllable concentration ratios and significant energy savings. The preparation of industrial-grade lithium salt products is a well-known technology, and the specific implementation process will not be elaborated further.
Claims
1. A method for recycling and processing valuable metals from waste ternary lithium battery black powder, characterized in that, The method includes the following steps: The obtained waste ternary lithium battery black powder raw material was subjected to acid leaching and iron and aluminum removal, and P204 semi-extraction was used to strip out a mixed solution rich in copper and manganese and raffinate 1. The mass concentration of copper ions in the mixture is detected in real time, the significance of the copper concentration deviating from the standard mass concentration range is calculated, and the ratio and extraction stage of 984 extraction are adaptively adjusted. The mixture is then subjected to 984 extraction according to the adjusted ratio and extraction stage to complete the separation of copper and manganese and obtain manganese-containing raffinate. The raffinate 1 was subjected to P507 semi-extraction, P507 full extraction and lithium concentration treatment in sequence to complete the separation of cobalt, magnesium, nickel and lithium.
2. The method for recycling valuable metals from waste ternary lithium battery black powder as described in claim 1, characterized in that, The specific process of using P204 semi-extraction to strip out the mixed solution rich in copper and manganese includes: The liquid after iron and aluminum removal was subjected to countercurrent extraction using P204 extractant to obtain a loaded organic phase and raffinate 1. The organic phase of the countercurrent extraction was a mixture of 20% P204, 5% TBP and sulfonated kerosene. The O / A ratio of the countercurrent extraction was set to 1:2, and the number of countercurrent extraction stages was 11. The loaded organic phase was back-extracted using a 2.6 mol / L sulfuric acid solution to obtain a mixed solution containing copper sulfate and manganese sulfate.
3. The method for recycling and processing valuable metals from waste ternary lithium battery black powder as described in claim 1, characterized in that, The calculation of the significance of the copper concentration deviating from the standard mass concentration range, and the adaptive adjustment of the ratio and extraction stage of 984 extraction, includes: Obtain the current copper ion mass concentration of the mixture. And obtain the preset standard mass concentration range of copper ions. ;like If the concentration is within the standard mass concentration range, the ratio and extraction stage of the 984 extraction are set to the preset standard ratio and standard extraction stage, respectively. , These represent the preset lower limit of standard mass concentration and the preset upper limit of standard mass concentration, respectively. like Less than Through formula Calculate the significance The standard comparison is reduced based on the degree of significance, and the adjusted extraction stage is maintained at the standard extraction stage. Represents the hyperbolic tangent function; like Greater than Through formula Calculate the significance The standard comparison and standard extraction stages were amplified based on the degree of significance, and were used as adjusted comparison and extraction stages.
4. The method for recycling and processing valuable metals from waste ternary lithium battery black powder as described in claim 3, characterized in that, The specific process of using the adjusted comparison based on the significance reduction standard is as follows: Calculate the product of the preset reduction factor and the obtained significance level, multiply the difference between the value 1 and the product by the preset standard comparison to obtain the adjusted comparison.
5. The method for recycling valuable metals from waste ternary lithium battery black powder as described in claim 3, characterized in that, The specific process for comparing based on the aforementioned significance amplification standard is as follows: Calculate the product of the preset amplification factor and the obtained significance level, multiply the sum of the product of the value 1 and the product by a preset standard, and obtain the adjusted comparison.
6. The method for recycling valuable metals from waste ternary lithium battery black powder as described in claim 3, characterized in that, The process of amplifying the standard extraction order based on the significance level includes: The adjusted extraction level is obtained by multiplying the calculated significance level by the range of the preset extraction level interval, and adding the preset lower limit of the extraction level.
7. The method for recycling and processing valuable metals from waste ternary lithium battery black powder as described in claim 1, characterized in that, The step of performing 984 extraction on the mixture according to the adjusted ratio and extraction stage to complete the copper-manganese separation and obtain the manganese-containing raffinate is as follows: First, the pH of the mixture is adjusted using an alkaline neutralizing agent; the organic phase of the 984 extractant is a mixture of 30% 984 and sulfonated kerosene, the extraction ratio is set to the adjusted ratio, and the flow rate ratio of the pumped organic phase to the mixture is controlled to be equal to the adjusted ratio, and the countercurrent extraction stage is set to the adjusted extraction stage; after completing the countercurrent extraction, a copper-loaded organic phase and raffinate 2 are obtained, wherein raffinate 2 is a manganese-containing raffinate; The copper-loaded organic phase was back-extracted using a 1.5 mol / L sulfuric acid solution to obtain a copper sulfate solution.
8. The method for recycling valuable metals from waste ternary lithium battery black powder as described in claim 1, characterized in that, The specific steps for performing P507 semi-extraction are as follows: The raffinate 1 was subjected to countercurrent extraction using P507 extractant to obtain an organic phase loaded with cobalt and magnesium, as well as raffinate 3. The organic phase of the countercurrent extraction was a mixture of 25% P507, 5% TBP and sulfonated kerosene, with a nickel soap saponification rate of 60%. The extraction ratio was set to 1:1.5, and the number of countercurrent extraction stages was 11. The organic phase loaded with cobalt and magnesium was subjected to serial stepwise back-extraction: first, back-extraction was performed with a 1.5 mol / L sulfuric acid solution to obtain a magnesium sulfate solution, and then back-extraction was performed with a 2.6 mol / L sulfuric acid solution to obtain a cobalt sulfate solution.
9. A method for recycling valuable metals from waste ternary lithium battery black powder as described in claim 8, characterized in that, The specific process of the P507 whole extraction is as follows: The raffinate 3 was subjected to countercurrent extraction using P507 extractant to obtain a nickel-rich organic phase and raffinate 4. The organic phase for countercurrent extraction was a mixture of 25% P507, 5% TBP and sulfonated kerosene. The organic phase was subjected to saponification treatment to maintain the saponification rate at 60%~70%. The extraction ratio was set to 1.5:1 and the number of countercurrent extraction stages was 8. The nickel-rich organic phase was back-extracted using a 2.6 mol / L sulfuric acid solution to obtain a nickel sulfate solution.
10. A method for recycling valuable metals from waste ternary lithium battery black powder as described in claim 9, characterized in that, The specific operation of the lithium concentration treatment includes: evaporating and concentrating the raffinate 4 until the lithium mass concentration in the solution reaches 15~20g / L, to obtain a mixed concentrate containing lithium sulfate and sodium sulfate.