A method for preparing a locally machinable copper-diamond composite heat dissipation material
By designing local machinable and composite zones in copper-diamond composite materials, utilizing dispersed reinforced copper and a nonlinear transition layer, and combining them with a metallurgical interface, the contradiction between high thermal conductivity and machinability in copper-diamond composite materials was resolved, achieving efficient machining and material reliability.
Patent Information
- Application Number
- CN202611128454.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing copper-diamond composite materials are difficult to machine using conventional methods while maintaining high thermal conductivity, and the interface is prone to cracking, resulting in discontinuous heat flow and poor reliability.
By designing local machinable and composite zones in copper-diamond composite materials, utilizing dispersion-strengthened copper and nonlinear transition layers, combined with metallurgical bonding interfaces, the continuity and machinability of the copper matrix are achieved. Segmented sintering and active element intermediate layers are used to improve interfacial bonding.
This achieves effective separation between the high thermal conductivity zone and the machinable zone, avoiding interfacial thermal resistance and interfacial cracking, improving machining efficiency and material reliability, and reducing local hot spots and stress concentration.
Smart Images

Figure CN123108352A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor packaging and heat dissipation materials technology, specifically to a method for preparing a locally machinable copper-diamond composite heat dissipation material. Background Technology
[0002] The continuous development of third-generation semiconductor devices and high-power lasers, radars, and power electronic modules has led to a continuous increase in the local heat flux density of chips, with some hot spots reaching the kilowatt level per square centimeter. Although pure copper has good processability and low cost, its thermal conductivity is about 400 W / m·K and its coefficient of thermal expansion is about 17 ppm / K, which is far inferior to chip materials such as silicon, silicon carbide, and gallium nitride. As a heat dissipation substrate or heat sink for high-power devices, it is no longer sufficient.
[0003] In contrast, diamond has a thermal conductivity as high as 700~2000 W / m·K and a coefficient of thermal expansion as low as about 1 ppm / K. Dispersing diamond particles in a copper matrix to form copper-diamond composites allows for the adjustment of their thermophysical properties over a wide range. Therefore, copper-diamond composites are considered an important candidate for heat dissipation substrates and heat sinks for next-generation high-power devices.
[0004] However, a problem arises: diamond has a Mohs hardness of 10. While this characteristic provides high thermal conductivity, it also makes diamond-containing composite materials difficult to machine using conventional methods. Carbide drills and taps wear out extremely quickly during drilling and tapping, often failing to create holes; electrical discharge machining (EDM) has low efficiency and poor surface quality; laser processing results in a heat-affected zone and a recast layer. Furthermore, heat sinks often require features such as threaded holes, locating pin holes, fluid interfaces, and sealing grooves in actual assembly. How to achieve these machinable features while maintaining high thermal conductivity in the composite area has been a long-standing challenge in this field. Summary of the Invention
[0005] In order to overcome the shortcomings of the prior art, the present invention aims to provide a method for preparing a locally machinable copper-diamond composite heat dissipation material, so as to solve the technical problems in the prior art such as discontinuous heat conduction across regions, easy formation of local hot spots in the machinable region, and interface expansion mismatch cracking.
[0006] To address the above problems, a first aspect of the present invention provides a locally machinable copper-diamond composite heat dissipation material, comprising: The composite region is configured to be formed by diamond particles dispersed in a copper matrix; The machinable area is configured such that its position in the heat dissipation material corresponds to the position of subsequent machining, and is formed of pure copper or copper-based material with a diamond volume fraction of no more than 10%; The diamond volume fraction in the composite region is higher than that in the machinable region; A continuous metallurgical bonding interface of copper matrix is also formed between the composite zone and the machinable zone.
[0007] In some embodiments, the processable region is dispersion-strengthened copper, in which 0.2% to 3% by volume of rigid oxide or carbide dispersion particles are dispersed. The dispersion particles constrain the densification shrinkage of the processable region during sintering, so that its shrinkage is close to that of the composite region.
[0008] In some embodiments, the processable area is a blind column that does not penetrate the thickness of the heat dissipation material and is located on the side of the heat dissipation material away from the heat source; The composite area continuously covers the side of the blind zone column facing the heat source, and the thickness of the covered portion along the thickness direction is not less than half of the maximum transverse dimension of the blind zone column.
[0009] In some embodiments, a transition layer is provided between the composite region and the machinable region, wherein the diamond volume fraction in the transition layer decreases non-linearly from the composite region side to the machinable region side, and the rate of decrease of the volume fraction along the thickness is smaller on the side closer to the composite region than on the side closer to the machinable region.
[0010] In some embodiments, the average particle size of the diamond particles in the transition layer near the machinable region is smaller than the average particle size of the diamond particles in the composite region.
[0011] In some embodiments, the surface of the diamond particles in the composite region is coated with a carbide intermediate layer generated in situ by a carbide-forming element, wherein the carbide-forming element is selected from at least one of titanium, chromium, tungsten, and molybdenum, and the carbide intermediate layer continuously covers the diamond surface and has a thickness of 50 nm to 800 nm.
[0012] In some embodiments, the copper matrix contains an active element that reacts with the diamond interface to form carbides.
[0013] A second aspect of the present invention provides a method for preparing a locally machinable copper-diamond composite heat dissipation material as described above, comprising: The molding mold defines the molding space of the composite area and the machining area molding space of the corresponding subsequent machining position; The composite zone molding space is filled with a mixture of diamond and copper powder, and the machinable zone molding space is filled with pure copper material or copper-based material with a diamond volume fraction of no more than 10%. The material inside the mold is sintered as a whole, making the two zones dense and forming a continuous metallurgical bond of copper matrix at their interface.
[0014] In some embodiments, the integral sintering is uniaxial pressure sintering, with a temperature of 900℃~1050℃ and a pressure of 30MPa~80MPa; During sintering, a compressible buffer is provided between the forming space of the machinable zone and the pressure punch to make the pressure on the machinable zone lower than the pressure on the composite zone; Furthermore, before the integral sintering, the mixed powder in the composite zone is subjected to cold isostatic pre-pressing to make its green body density match the initial density of the material in the processable zone; The integral sintering adopts a segmented heating method. First, the composite region is formed into a skeleton at a first temperature, and then the temperature is raised to a second temperature higher than the first temperature to make the processable region dense.
[0015] In some embodiments, an intermediate layer containing active elements with a melting point lower than that of copper is laid at the junction of the forming space of the machinable zone and the forming space of the composite zone. The active elements belong to the same group as the carbide-forming elements on the diamond surface in the composite zone. The intermediate layer melts before the copper substrate to form a liquid phase during the integral sintering, and after capillary filling of the pores at the junction, it is isothermally solidified to form a metallurgical bond.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. The opposing goals of high thermal conductivity and machinability are spatially separated. The composite zone is responsible for thermal conductivity, while the machinable zone is responsible for machining. The composite zone can maintain a thermal conductivity of 600~800W / m·K, while the machinable zone can be efficiently machined with conventional tools without the tools touching the diamond. Furthermore, since the two zones are connected by a continuous metallurgical interface of copper matrix, rather than an adhesive layer or weld, the heat flow across the zones does not need to cross the additional interface, resulting in continuous thermal conductivity and mechanical reliability. 2. The machinable zone uses dispersion-strengthened copper, and the rigid dispersion phase constrains the densification shrinkage of the copper matrix. Its constraint method is isomorphic to the constraint of copper by diamond in the composite zone. Therefore, the shrinkage of the machinable zone is close to that of the composite zone, which suppresses the annular pores at the interface from the source. 3. The processable area is made into a blind column on the back heat source side and covered by the composite area. Before the heat flow reaches the column, it has already expanded laterally within the high thermal conductivity covering layer and travels around the column. As a result, the pure copper area is removed from the main heat flow path, and local hot spots are eliminated.
[0017] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments. Attached Figure Description
[0018] Figure 1 This is a cross-sectional view along the thickness direction of a partially machinable copper-diamond composite heat dissipation material according to an embodiment of this application, showing the relative positions of the composite region, the machinable region, the transition layer, and their metallurgical bonding interface.
[0019] Figure 2 for Figure 1A partially enlarged schematic diagram of the central blind zone column and the composite zone covering above it, with arrows indicating the path of the heat flow as it expands laterally within the covering layer and bypasses the blind zone column.
[0020] Figure 3 The curve shows the distribution of diamond volume fraction along the thickness direction in the transition layer. The solid line represents the nonlinear distribution of the present invention, and the dashed line represents the linear distribution, used to compare the location of the stress peak.
[0021] Figure 4 This is a schematic cross-sectional view of the machinable region that extends through the thickness, showing the central pure copper channel and its surrounding oriented, highly thermally conductive phase pointing towards the composite region.
[0022] Figure 5 This is a schematic diagram of a mold assembly using a removable placeholder and a compressible buffer in a method for preparing a partially machinable copper-diamond composite heat dissipation material according to another embodiment of this application.
[0023] The markings in the diagram are: 1—composite zone; 2—machinable zone; 3—transition layer; 4—metallurgical bonding interface; 5—blind zone column; 6—covered part; 7—pure copper channel; 8—directional high thermal conductivity phase; 9—placer; 10—compressible buffer. Detailed Implementation
[0024] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.
[0026] The following detailed description of some embodiments of the present invention is provided in conjunction with the accompanying drawings. Unless otherwise specified, the following embodiments and features can be combined with each other.
[0027] The applicant discovered: In order to obtain these machinable features while maintaining high thermal conductivity in the composite region, those skilled in the art shall at least employ the following practices: 1. First, the copper-diamond composite material is integrally molded, and then a piece of pure copper is mechanically inlaid or brazed into the area that needs to be processed. Although this approach provides a processable area, the pure copper block and the composite body are mechanically mating surfaces or brazed seams. The copper matrix is interrupted at the interface, and the heat flow across the region must pass through the adhesive layer or weld, resulting in significant interfacial thermal resistance. Mechanical reliability is also limited by the fitting accuracy and weld strength, and the interface is prone to loosening or cracking under thermal cycling. 2. Reduce the content of reinforcing phase in the areas requiring machining to make them closer to pure copper for easier cutting. However, as this approach is implemented in engineering, several subtle problems will gradually emerge. First, the thermal conductivity of pure copper is only about half that of the composite matrix. If this area happens to fall on the main heat flow path, it becomes a localized high thermal resistance zone, forming a hotspot. Second, the coefficient of thermal expansion of pure copper is approximately 17 ppm / K, while that of the composite zone is approximately 6-9 ppm / K, a difference of nearly three times. This leads to stress concentration at the interface during thermal cycling, making it prone to cracking. Third, pure copper is soft, with low recrystallization and creep temperatures. Under the combined effects of bolt preload and temperature cycling, pure copper threaded holes will experience creep and stress relaxation, resulting in loose connections and increased contact thermal resistance.
[0028] The above-mentioned phase-reduction approach still faces process-level obstacles in the integrated powder metallurgy molding process. During sintering, the unconstrained pure copper undergoes significantly greater densification shrinkage than the composite zone constrained by the diamond framework. The two zones shrink asynchronously, easily forming annular pore bands at the interface. If uniaxial pressure sintering is used, the soft pure copper zone will yield first, become excessively dense, and even laterally squeeze into the interface, while the more rigid composite zone will have residual pores due to insufficient pressure, resulting in overall warping and poor flatness after cooling. When a pure copper zone is pre-reserved using removable spacers and then backfilled with pure copper powder, a cold seam with a density abrupt change is formed between the loosely packed pure copper powder and the pre-compacted composite powder. The sintering neck formed by solid-state sintering is difficult to cross this abrupt change line.
[0029] 3. In addition, to improve the bonding between diamond and copper, it is known in the art to apply a metal layer to the diamond surface or to add alloying elements to the copper. However, such treatments usually focus on the thermal conductivity and strength of the entire composite material, without considering the partitioning requirements of "where to retain the machinable area and how to establish a reliable metallurgical bond between the machinable area and the composite area"; the thickness of the metallization layer is also mostly limited to meeting wetting requirements, without studying its effect on interfacial heat transfer.
[0030] In view of this, refer to Figure 1 One embodiment of this application provides a locally machinable copper-diamond composite heat dissipation material, comprising: Composite region 1 is configured to be formed by diamond particles dispersed in a copper matrix; Machinable area 2 is configured such that its position in the heat dissipation material corresponds to the position of subsequent machining. It should be noted that within the same heat dissipation material, there are composite area 1 and machinable area 2. Composite area 1 is responsible for heat conduction, and the position of machinable area 2 in the heat dissipation material corresponds to the position of subsequent machining. In other words, this heat dissipation material can be specifically designed according to different machining requirements, and the machinable area 2 can be designed in a specific position to meet the needs of various machining situations. Preferably, the subsequent machining situations include application scenarios such as threaded holes, locating pin holes, fluid interfaces, and sealing grooves. Furthermore, the machinable region 2 is formed of pure copper or copper-based material with a diamond volume fraction of no more than 10%; the diamond volume fraction of the composite region 1 is higher than that of the machinable region 2; and a continuous metallurgical bonding interface 4 of copper matrix is formed between the composite region 1 and the machinable region 2.
[0031] Specifically, the machinable region 2, as defined above, and the metallurgical bonding interface 4 are a pair of coupled technical features. Only through the coupling of these two features can the technical problem that this application aims to solve be addressed as a whole. If there is only a machinable zone 2 and the interface is mechanically inlaid or brazed, cross-zone heat conduction is interrupted through the additional interface, and reliability is limited by the fit or weld. If there is only metallurgical bonding but no low-hardness machinable zone 2, then machining will still be difficult.
[0032] Therefore, in this embodiment, the metallurgical bonding interface 4 is defined as a continuous copper matrix across the interface, which makes this embodiment deviate from the simple approach of embedding copper blocks in composite materials: the copper matrix is uninterrupted at the interface, the heat flow is conducted across the region without additional interfacial thermal resistance, and the two regions are connected as one at the atomic level.
[0033] In one implementation, when the machinable region 2 is made of pure copper, the pure copper shrinks freely during sintering, and the shrinkage amount is greater than that of the composite region 1, which is constrained by the diamond framework. The two regions shrink mismatch and annular pores are generated at the interface. In order to improve the shrinkage constraint, in this embodiment, the machinable region 2 is a dispersion-strengthened copper, which contains 0.2% to 3% by volume of rigid oxide or carbide dispersion particles. The dispersion particles constrain the densification shrinkage of the machinable region 2 during sintering, so that its shrinkage amount is close to that of the composite region 1.
[0034] Specifically, the rigid oxide or carbide particles dispersed in the copper matrix constrain the densification shrinkage of the copper matrix in a way that is mechanically isomorphic to the constraint of the copper by the diamond in composite zone 1. When the machinable zone 2 also contains this type of rigid constraint phase, its sintering shrinkage trajectory moves closer to that of composite zone 1, and the shrinkage of the two zones tends to be synchronized, thus suppressing the annular pores at the interface from the source.
[0035] In addition, the dispersed particles pin the grain boundaries and delay recrystallization, raising the recrystallization temperature of the machinable zone 2 above that of pure copper, thus suppressing creep and stress relaxation at the service temperature and maintaining the preload of the threaded connection for a long time.
[0036] As another implementation, when the machinable zone 2 is made of pure copper, the pure copper threaded hole will creep, relax stress, and loosen under the preload and temperature cycling due to the low recrystallization and creep temperature of pure copper. In order to solve this problem, in this embodiment, the machinable zone 2 is precipitation-strengthened copper, in which a second phase is precipitated, and the forming element includes at least one of chromium and zirconium. The recrystallization temperature of the machinable zone 2 is higher than that of pure copper.
[0037] Specifically, the chromium and zirconium used in the precipitation strengthening system are both elements that form the second phase and carbide-forming elements. They belong to the same group as the active elements used in the interface of this invention, so their introduction will not precipitate an embrittled phase at the metallurgical bonding interface 4.
[0038] Preferably, the volume fraction of the dispersed phase is limited to 0.2% to 3%. If it is below this range, the shrinkage constraint and grain boundary pinning are insufficient; if it is above this range, the cutting resistance of the machinable zone 2 will increase due to the excessive rigid phase, deviating from the intended machinability.
[0039] Preferably, in terms of recrystallization temperature, the recrystallization temperature of pure copper is usually on the order of about 200°C. After dispersion strengthening, it shifts significantly upward due to grain boundary pinning. This upward shift directly corresponds to the leap in creep resistance of threaded holes at service temperatures in the hundreds of degrees Celsius range.
[0040] refer to Figure 2 In one implementation, the processable area 2 is a blind column 5 that does not penetrate the thickness of the heat dissipation material and is located on the side of the heat dissipation material away from the heat source. The composite zone 1 continuously covers the side of the blind zone column 5 facing the heat source. The thickness of the covering portion 6 along the thickness direction is not less than half of the maximum transverse dimension of the blind zone column 5, so that the heat flow expands laterally within the composite zone 1 and bypasses the blind zone column 5.
[0041] Since the thermal conductivity of the processable region 2 is about half that of the composite body, if the processable region 2 is located on the main heat flow path, it is easy to form local hot spots. Therefore, in order to solve this problem, the processable region 2 is made into a blind zone pillar 5 that does not penetrate the thickness and is located on the side facing the heat source. The composite region 1 is continuously covered on the side facing the heat source, so that the heat flow lines are refracted at the interface where the thermal conductivity changes abruptly. Because the heat flow preferentially propagates along the high thermal conductivity path, when the side facing the heat source is a continuous high thermal conductivity composite layer, the heat flow injected by the chip first expands laterally in the covering layer and then bypasses the low thermal conductivity blind zone pillar 5. The pillar is thus relegated to the heat shadow area and only undertakes the mechanical connection of bolts or pins.
[0042] Furthermore, the thickness of the covering portion 6 is limited to not less than half of the maximum lateral dimension of the blind zone column 5, because the characteristic length required for the heat flow to fully expand laterally within the covering layer is on the same order of magnitude as the lateral dimension of the column. If the covering is too thin, the heat flow will not have enough time to bypass it, and the hot spot will reappear.
[0043] refer to Figure 3 Furthermore, a transition layer 3 is provided between the composite region 1 and the machinable region 2. The volume fraction of diamond in the transition layer 3 decreases non-linearly from the composite region 1 side to the machinable region 2 side. The rate of decrease of this volume fraction along the thickness is smaller on the side closer to the composite region 1 than on the side closer to the machinable region 2. Preferably, the average particle size of the diamond particles in the transition layer 3 near the machinable region 2 is smaller than the average particle size of the diamond particles in the composite region 1.
[0044] Because the coefficients of thermal expansion of pure copper and composite region 1 differ by nearly three times, interfacial cracking is easily caused during thermal cycling. This is because the interfacial thermal stress peak is concentrated at one end of the high-rigidity composite region 1. Since rigid materials cannot release stress through deformation, if the transition layer 3 is linearly decreasing, the stress singularity will remain there. To solve this problem, this embodiment makes the diamond volume fraction in the transition layer 3 nonlinearly distributed, so that the diamond volume fraction changes gradually on the rigid composite region 1 side and abruptly changes on the flexible machinable region 2 side, i.e., a nonlinear distribution that is gradual at the rigid end and abrupt at the flexible end. This actively migrates the stress peak to the copper side with good plasticity, where it is absorbed by the copper matrix through micro-plastic deformation.
[0045] Furthermore, according to fracture mechanics, the critical crack size is positively correlated with the particle size; by using smaller-diameter diamonds on the interface side, the potential crack initiation size can be reduced to below the critical value, while the equivalent modulus step corresponding to the change in unit volume fraction is reduced, the interface is more diffuse, and the modulus transition is smoother.
[0046] It should be noted that by designing the volume fraction of diamond in transition layer 3 to have a non-linear distribution, the stress distribution is controlled. Then, by refining the diamond on the interface side, crack initiation is suppressed. The combination of these two methods enables crack suppression to be achieved.
[0047] More specifically, the coefficient of thermal expansion of pure copper is approximately 17 ppm / K, while that of composite region 1 with 60% diamond volume fraction is approximately 6-9 ppm / K. If the temperature cycling span is considered to be 200℃, the accumulated mismatch strain along the interface is considerable. Finite element analysis in this embodiment shows that during the linear transition, the peak values of interfacial shear stress and normal stress are concentrated at the end of transition layer 3 on one side of composite region 1, where the material modulus is high and the plasticity reserve is low. When the nonlinear distribution of this embodiment is adopted, the stress peak position shifts towards the copper side, and the peak value decreases accordingly, allowing the copper matrix to absorb strain within its plasticity range. The effect of diamond refinement on the interface side is superimposed: after the particle size is reduced, the stress concentration factor at the particle-matrix interface decreases, and combined with the downward shift of the critical crack size, crack initiation and propagation are difficult.
[0048] refer to Figure 4 As one implementation, a pure copper channel 7, coaxial with the machining tool and with a lateral dimension not less than the diameter of the tool, is provided in the machinable area 2 that penetrates the thickness of the heat dissipation material; the area outside the pure copper channel 7 is filled with a directionally arranged high thermal conductivity phase 8, the orientation of the high thermal conductivity phase 8 pointing towards the composite area 1.
[0049] If the high thermal conductivity phase 8 is randomly distributed, its guiding effect on heat flow is averaged out. When its orientation points towards the composite region 1, the heat flow can pass through the machinable region 2 and converge into the composite region 1 along the orientation with a shorter path, which is equivalent to building several thermal bridges around the through hole. The lateral dimension of the pure copper channel 7 is not less than the tool diameter, ensuring that the tool is wrapped in pure copper throughout the machining process and does not touch the high thermal conductivity phase 8 outside the channel.
[0050] In one embodiment, the surface of the diamond particles in composite region 1 is coated with a carbide intermediate layer generated in situ by a carbide-forming element. The carbide-forming element is selected from at least one of titanium, chromium, tungsten, and molybdenum. The carbide intermediate layer continuously covers the diamond surface and has a thickness of 50 nm to 800 nm.
[0051] A continuous carbide interlayer is generated in situ on the diamond surface. This interlayer is chemically bonded to the diamond and wettable by copper. Furthermore, the phonon spectrum and acoustic impedance of the carbide lie between those of diamond (which has a high Debye temperature) and copper (which is primarily thermally conductive by electrons). This allows the interlayer to act as a bridge for acoustic impedance matching, improving the interfacial phonon transmission coefficient and reducing the interfacial thermal resistance. More specifically, the thickness of the interlayer is limited to 50–800 nm. Too thin an interlayer results in incomplete coverage and discontinuous bridging; too thick an interlayer, on the other hand, results in low thermal conductivity of the carbide itself (approximately 20 W / m·K), creating a new bottleneck.
[0052] Preferably, the copper matrix contains an active element that reacts with the diamond interface to form carbides.
[0053] Another embodiment of this application provides a method for preparing a locally machinable copper-diamond composite heat dissipation material as described above, comprising: In the molding die, the molding space of composite area 1 and the molding space of machinable area 2 corresponding to the subsequent machining position are defined; A mixture of diamond and copper powder is filled into the molding space of the composite zone 1, and pure copper material or copper-based material with a diamond volume fraction of no more than 10% is configured in the molding space of the machinable zone 2. The material inside the mold is sintered as a whole, making the two zones dense and forming a continuous metallurgical bond of copper matrix at their interface.
[0054] It should be noted that defining the forming space is a prerequisite for subsequent filling and configuration, and must be completed before loading. Filling the composite zone 1 with mixed powder and configuring the machinable zone 2 with pure copper or copper-based material can be done in parallel or sequentially, but both must be in place before integral sintering. Integral sintering is a converging step, in which the two zones become dense in the same thermal process and merge at the interface to form a metallurgical bond. refer to Figure 5 As one implementation method, integral sintering is uniaxial pressure sintering at a temperature of 900℃~1050℃ and a pressure of 30MPa~80MPa; During sintering, a compressible buffer 10 is set between the forming space of the machinable zone 2 and the pressure punch so that the pressure on the machinable zone 2 is lower than the pressure on the composite zone 1. Furthermore, before integral sintering, the mixed powder in composite zone 1 is subjected to cold isostatic pre-pressing to make its green density match the initial density of the material in processable zone 2. The integral sintering adopts segmented heating. First, the composite zone 1 is formed into a skeleton at the first temperature, and then the temperature is raised to a second temperature higher than the first temperature to make the processable zone 2 dense.
[0055] Due to the yielding, excessive densification, and even lateral extrusion into the interface of soft pure copper under uniaxial pressure sintering, the composite zone 1 is under-pressured and leaves pores. The shrinkage trajectories of the two zones diverge, resulting in interface porosity and overall warping. Therefore, in this embodiment, a compressible buffer 10 is provided between the forming space of the processable zone 2 and the pressure punch, so that the pressure on the processable zone 2 is lower than that on the composite zone 1, and the two zones fall into their own densification windows. Before sintering, the mixed powder of the composite zone 1 is cold isostatically pre-pressed so that its green density is comparable to the initial density of the material in the processable zone 2. During sintering, the temperature is raised in stages. First, the composite zone 1 is formed into a skeleton at the first temperature, and then the temperature is raised to the second temperature to densify the processable zone 2, thereby staggering the shrinkage peaks of the two zones.
[0056] As one implementation method, an intermediate layer containing active elements with a melting point lower than that of copper is laid at the junction of the forming space of the machinable zone 2 and the forming space of the composite zone 1. The active elements belong to the same group as the carbide forming elements on the diamond surface in the composite zone 1. During the integral sintering, the intermediate layer melts before the copper substrate to form a liquid phase, and after capillary filling of the pores at the junction, it is isothermally solidified to form a metallurgical bond.
[0057] It should be noted that when reserving a machinable area using the removable occupier 9 and then backfilling with loosely packed pure copper powder, there is a cold joint with a density abrupt change between the backfill powder and the pre-pressed composite powder. The solid-phase sintering neck only grows within each zone and cannot cross this abrupt change line. Therefore, in this embodiment, an intermediate layer containing active elements with a melting point lower than copper is laid at the interface. This layer melts before the copper matrix during sintering to form a liquid phase, which wets both sides and fills the joint pores through capillary action. The active elements simultaneously reduce the interface oxide film and bond both sides. Subsequently, the liquid phase is isothermally solidified through diffusion of solute into the base material, solidifying into a metallurgical bond. The capillary filling and isothermal solidification of the liquid phase precisely cross the density breakpoint that solid-phase diffusion cannot overcome. The active elements used are in the same group as the carbide-forming elements on the diamond surface of composite zone 1, and will not introduce an embrittlement phase.
[0058] The present invention will be further described in detail below with reference to specific embodiments: To verify the technical effect of the present invention, the heat dissipation substrate prepared in this embodiment has two M3 threaded hole mounting positions, as detailed below: In this embodiment, a 50mm × 50mm × 6mm heat dissipation substrate is fabricated. Dispersion-strengthened copper blind zone pillars are positioned on the back side corresponding to the two M3 mounting holes. These pillars are cylindrical, 5mm in diameter, and 3mm deep from the back side without penetrating. The side of the pillar facing the heat source is continuously covered by a composite zone with a thickness of 3mm, not less than half the 5mm pillar diameter. The composite zone uses 60% diamond by volume, with diamond particle size of 100-150μm. The particle surface is pre-chromium-plated by magnetron sputtering and subsequently transformed into a carbide intermediate layer in situ during sintering, with a thickness of approximately 300nm. The machinable zone uses dispersion-strengthened copper containing 1.0 vol% nano-alumina dispersed particles. A 1.0mm wide transition layer is provided between the two zones. The diamond volume fraction decreases non-linearly from 60% to 0, with a gentle decrease near the composite zone and a steep decrease near the machinable zone. The diamond particle size on the machinable zone side of the transition layer is 30-50μm, smaller than the 100-150μm in the composite zone.
[0059] Mold and Material Preparation: A graphite mold with an inner cavity of 50mm × 50mm was designed, with 5.2mm diameter removable graphite placeholders embedded in two machinable areas. Chromium-plated diamond (60 vol%) and electrolytic copper powder (approximately 10 μm particle size) were mixed in a three-dimensional mixer for 2 hours to prepare the composite zone mixed powder. The transition layer micro-layer powders were separately prepared according to a non-linear distribution, with the difference in diamond volume fraction between adjacent layers controlled within 5%. Dispersion-strengthening copper powder was prepared separately. Before filling the composite zone forming space with the mixed powder, a 200MPa cold isostatic pressing was applied to pre-press the mixed powder into a blank, ensuring that its green blank density matched the initial density of the subsequently backfilled dispersion-strengthening copper powder—this step was completed before mold assembly to ensure that the initial densities of the two zones were similar upon sintering. Subsequently, the pre-pressed composite blank, along with the transition layer micro-layers, was sequentially placed into the cavity, excluding the placeholders, and gently pressed together.
[0060] After removing the graphite placer, fill the two cavities with dispersed reinforced copper powder. Place a flexible graphite buffer pad approximately 0.5 mm thick between the top surface of the powder in the machinable area and the upper punch, so that the effective pressure in this area is lower than that in the composite area during sintering. Move the mold into the spark plasma sintering furnace, apply an axial pressure of 50 MPa, and heat at 100 °C / min, with segmented holding: first heat to 850 °C and hold for 5 min to allow the diamond-copper framework to form in the composite area, then heat to 980 °C and hold for 10 min to densify the dispersed reinforced copper area, and then cool and demold with the furnace.
[0061] Post-processing was relatively standard: the upper and lower surfaces of the demolded blank were ground smooth to a thickness tolerance of ±0.02mm. A φ2.5mm pilot hole was drilled in the machinable area on the back side, followed by tapping with an M3 tap. No abnormal wear was observed on the tool during tapping, and the hole walls were smooth. Tests showed that the thermal conductivity of the composite zone was approximately 720W / m·K (laser flash method), and approximately 340W / m·K in the machinable area of the dispersion-strengthened copper. The annular porosity at the interface was statistically less than 0.5% according to metallographic analysis. Room temperature tensile fracture occurred on one side of the composite zone, and no debonding was observed at the interface. After 500 temperature cycles from 55℃ to 150℃, there are no cracks at the interface, and the overall thermal resistance change is less than 2.5%. When two M3 bolts are pre-tightened to 0.6 N·m and subjected to the above temperature cycles, the pre-tightening force retention rate of the dispersion-reinforced copper threaded hole is higher than 92%.
[0062] Furthermore, the diamond particle size in the composite zone can be selected between 80 and 180 μm, and the volume fraction can be adjusted between 50% and 65%. The volume fraction of dispersed particles can be selected between 0.5% and 2.0%. If it is too low, the shrinkage constraint and grain boundary pinning will be insufficient; if it is too high, the tapping resistance will increase. The cold isostatic pressing pressure can be adjusted between 150 and 250 MPa to match the initial density of the backfill powder. The first of the two insulation temperature stages can be selected between 820 and 880℃, and the second stage can be selected between 960 and 1000℃. It should be noted that the thickness of the flexible graphite buffer pad is directly related to the reduction in pressure in the machinable area. If the pad is too thick, the machinable area will not be sufficiently densified; if it is too thin, the regional differential pressure effect will be ineffective. In this embodiment, 0.5 mm is appropriate.
[0063] The above embodiments are merely preferred embodiments of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-substantial changes and substitutions made by those skilled in the art based on the present invention shall fall within the scope of protection claimed by the present invention.
Claims
1. A locally machinable copper-diamond composite heat dissipation material, characterized in that, include: The composite region is configured to be formed by diamond particles dispersed in a copper matrix; The machinable area is configured such that its position in the heat dissipation material corresponds to the position of subsequent machining, and is formed of pure copper or copper-based material with a diamond volume fraction of no more than 10%; The diamond volume fraction in the composite region is higher than that in the machinable region; A continuous metallurgical bonding interface of copper matrix is also formed between the composite zone and the machinable zone.
2. The heat dissipation material as described in claim 1, characterized in that, The processable region is a dispersion-strengthened copper, in which 0.2% to 3% by volume of rigid oxide or carbide dispersion particles are dispersed. The dispersion particles constrain the densification shrinkage of the processable region during sintering, so that its shrinkage is close to that of the composite region.
3. The heat dissipation material as described in claim 2, characterized in that, The processable area is a blind column that does not penetrate the thickness of the heat dissipation material and is located on the side of the heat dissipation material away from the heat source; The composite area continuously covers the side of the blind zone column facing the heat source, and the thickness of the covered portion along the thickness direction is not less than half of the maximum transverse dimension of the blind zone column.
4. The heat dissipation material as described in claim 3, characterized in that, A transition layer is provided between the composite region and the machinable region. The diamond volume fraction in the transition layer decreases non-linearly from the composite region side to the machinable region side. The rate of decrease of the volume fraction along the thickness is smaller on the side closer to the composite region than on the side closer to the machinable region.
5. The heat dissipation material as described in claim 4, characterized in that, The average particle size of the diamond particles in the transition layer near the machinable region is smaller than the average particle size of the diamond particles in the composite region.
6. The heat dissipation material as described in claim 5, characterized in that, The surface of the diamond particles in the composite region is coated with a carbide intermediate layer generated in situ by a carbide-forming element. The carbide-forming element is selected from at least one of titanium, chromium, tungsten, and molybdenum. The carbide intermediate layer continuously covers the diamond surface and has a thickness of 50 nm to 800 nm.
7. The heat dissipation material as described in claim 5, characterized in that, The copper matrix contains an active element that reacts with the diamond interface to form carbides.
8. A method for preparing a locally machinable copper-diamond composite heat dissipation material as described in any one of claims 1 to 7, characterized in that, include: The molding mold defines the molding space of the composite area and the machining area molding space of the corresponding subsequent machining position; The composite zone molding space is filled with a mixture of diamond and copper powder, and the machinable zone molding space is filled with pure copper material or copper-based material with a diamond volume fraction of no more than 10%. The material inside the mold is sintered as a whole, making the two zones dense and forming a continuous metallurgical bond of copper matrix at their interface.
9. The preparation method according to claim 8, characterized in that, The integral sintering is uniaxial pressure sintering, with a temperature of 900℃~1050℃ and a pressure of 30MPa~80MPa; During sintering, a compressible buffer is provided between the forming space of the machinable zone and the pressure punch to make the pressure on the machinable zone lower than the pressure on the composite zone; Furthermore, before the integral sintering, the mixed powder in the composite zone is subjected to cold isostatic pressing pre-pressing to make its green body density match the initial density of the material in the processable zone; The integral sintering adopts a segmented heating method. First, the composite region is formed into a skeleton at a first temperature, and then the temperature is raised to a second temperature higher than the first temperature to make the processable region dense.
10. The preparation method according to claim 9, characterized in that, At the junction of the processing zone forming space and the composite zone forming space, an intermediate layer containing active elements with a melting point lower than that of copper is laid. The active elements belong to the same group as the carbide forming elements on the diamond surface in the composite zone. The intermediate layer melts before the copper matrix to form a liquid phase during the integral sintering. After capillary filling of the pores at the junction, it is isothermally solidified to form a metallurgical bond.