A wide-temperature-range high-strength and high-toughness TaWRu alloy that is easy to cold work, its preparation process and applications
By introducing Ru into the Ta-W alloy and employing cold rolling and vacuum heat treatment, the problem of insufficient strength and plasticity of the Ta-W alloy in a wide temperature range is solved, achieving high strength and high plasticity in extreme temperature ranges, making it suitable for structural materials in aerospace and other fields.
Patent Information
- Application Number
- CN202611440330.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing Ta-W alloys struggle to balance high strength and high plasticity across a wide temperature range, especially at extreme low and high temperatures, and have poor processing properties, making it difficult to meet the stringent requirements of aerospace and other fields.
By introducing Ru, the composition design of the Ta-W alloy is optimized. The preparation process includes induction melting, cold rolling and vacuum heat treatment to form a homogeneous microstructure, ensuring that the alloy has high strength and good plasticity over a wide temperature range.
The TaWRu alloy achieves a high strength and high plasticity balance within the temperature range of -196℃ to 1300℃, exhibiting excellent creep resistance and making it suitable for structural material applications in extreme environments.
Smart Images

Figure CN123108381A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal structural materials technology, and particularly relates to a wide-temperature-range high-strength and high-toughness TaWRu alloy that is easy to cold work, its preparation process and application. Background Technology
[0002] Humanity's pursuit of changing the world and exploring the universe has never ceased, and increasingly complex and demanding application environments pose enormous challenges to existing structural materials. The rapid development of the aerospace industry requires more powerful jet engines, necessitating the use of new materials that are less prone to softening at higher temperatures. Deep-sea exploration and cryogenic superconductivity, on the other hand, require structural materials with high cryogenic fracture toughness to ensure they do not easily fracture under low or even extremely low temperatures. To realize the dreams of manned lunar landings and reaching the depths of space, structural materials used in space exploration must remain stable and withstand shocks in the extreme temperature variations of the space environment. As industrial progresses, the loads in service environments will become increasingly complex and extreme, urgently requiring stronger and higher-performance materials to meet these challenges.
[0003] With the development of aerospace, nuclear energy, and high-end equipment manufacturing, the demand for structural materials capable of long-term service under extreme high temperatures (>1300℃), high stress, and complex atmospheres is becoming increasingly urgent. For example, turbine blades and combustion chamber liners for next-generation aero-engines, as well as the thermal protection systems of hypersonic vehicles, all require materials that maintain excellent high-temperature strength while possessing good resistance to oxidation, creep, and thermal shock. Ultra-high temperature materials refer to special alloy systems that can maintain structural stability and functional integrity under extreme service conditions such as high temperature, oxidation, and corrosion. Their typical operating temperature is usually above 1300℃, and they are widely used in aerospace, energy, and power fields. For example, when hypersonic vehicles traverse the atmosphere, the surface temperature of leading-edge components can reach 1300℃ or higher; and aero-engine turbine blades, when achieving a thrust-to-weight ratio of 15-20, operate at temperatures close to 1900℃. Traditional nickel-based single-crystal high-temperature alloys, with melting points of only 1300-1400℃, can no longer meet the requirements of such extreme environments.
[0004] Besides ultra-high temperature service environments, extreme low temperature conditions are also a significant challenge for high-performance structural materials. Liquid nitrogen temperature (77 K, or -196 °C) is a typical operating temperature for critical components in aerospace propulsion systems, such as liquid nitrogen tanks, cryogenic fuel delivery pipelines, and superconducting magnet support structures. At this temperature, the plastic deformation mechanism of materials undergoes a fundamental transformation: dislocation movement is severely hindered, slip system activation becomes difficult, and most body-centered cubic (bcc) metals and alloys exhibit a pronounced tendency towards low-temperature brittleness, manifested as a sharp increase in yield strength, a drastic drop in fracture elongation, and even complete loss of macroscopic plasticity. For example, the fracture elongation of the traditional refractory alloy Ta-10W at 77 K is often less than 5%, far from meeting the safety margin requirements for cryogenic structural components. Structural materials designed for liquid nitrogen temperature service scenarios must meet the following performance requirements: high cryogenic plasticity reserve (elongation at break at cryogenic temperatures not less than 10%) to avoid sudden brittle fracture; stable high strength level (yield strength at cryogenic temperatures not less than 800 MPa) to withstand cryogenic high-pressure loads; low plastic-brittle transition temperature should be below -196℃ to ensure that the material maintains ductile fracture mode throughout the cryogenic range; good fatigue and impact resistance to adapt to transient impact loads such as rocket ignition and interstage separation.
[0005] Currently, alloys suitable for liquid nitrogen temperatures mainly include austenitic stainless steels (such as 304L and 316LN), Invar alloys, and some low-temperature titanium alloys. However, these materials have limited high-temperature performance, making it difficult to meet the service requirements across the entire temperature range from low to high. For example, 304L stainless steel can achieve an elongation of over 30% at 77 K, but its strength rapidly decreases to less than 100 MPa above 800 °C, making it unsuitable for the extreme conditions of the same component undergoing a wide temperature range cycle from low temperature to room temperature to high temperature during ascent. In contrast, Ta-W alloys, due to their high melting point and good low-temperature plasticity potential due to their bcc matrix, exhibit unique advantages in wide-temperature applications. However, traditional Ta-W alloys still face the problem of balancing strength and plasticity at liquid nitrogen temperatures: high W content increases room temperature strength but significantly raises the ductile-brittle transition temperature, leading to low-temperature embrittlement; low W content retains low-temperature plasticity but sacrifices high-temperature load-bearing capacity. The rapid development of aerospace technology has placed increasingly stringent demands on the comprehensive strength and toughness of high-temperature structural materials across a wide temperature range. This requires not only sufficient room-temperature ductility but also higher room-temperature and high-temperature strength. Simultaneously, the need for low-carbon and environmentally friendly mass production necessitates new alloy systems that are easier to cold-work at room temperature. Currently, most alloys designed for extreme high-temperature applications have poor room-temperature workability and are prone to ductile-brittle transitions at low temperatures, requiring cumbersome and easily oxidized thermomechanical processing methods. Although many TaW series alloys have shown potential for high-temperature applications and have been widely industrialized in numerous fields, maintaining excellent ductility and workability while strengthening alloys across a wide temperature range remains a significant challenge. Recent studies have found that appropriate Ru doping can uniformly replace Ta atoms in the crystal lattice, resulting in solid solution strengthening. Trace amounts of Ru (≤1%) hinder dislocation movement and increase strength, but generally have little effect on grain boundary movement and the initiation of slip systems; therefore, plasticity does not decrease significantly, and room-temperature workability is maintained or even optimized. However, when the Ru content is too high (>1%), the excess Ru will form brittle intermetallic compounds (such as TaRu2) with Ta or other elements (such as W). These hard and brittle phases precipitate at grain boundaries, severely disrupting the matrix and becoming stress concentration points. During cold working, these phases will preferentially crack or become crack initiations, leading to a sharp decrease in material plasticity and a severe deterioration in processing performance. Therefore, conducting research on Ru-containing easily machinable TaW alloys, and designing alloy composition and controlling microstructure, can improve the strength and toughness of the alloy over a wide temperature range without compromising its room temperature cold deformation capability. Summary of the Invention
[0006] To address the aforementioned technical problems, this invention provides a wide-temperature-range high-strength and high-toughness TaWRu alloy that is easily cold-workable, along with its preparation process and applications. This TaWRu alloy exhibits high strength and toughness and excellent creep resistance over a wide temperature range (from -196℃ to 1300℃).
[0007] To achieve the above purpose, the present invention adopts the following technical solution:
[0008] A TaWRu alloy with easy cold workability, wide temperature range, high strength and high toughness, the composition of which satisfies the general formula Ta a W b Ru c , wherein a, b and c respectively represent the atomic percentages of the corresponding alloy elements, 90≤a≤95, 5≤b≤10, 0<c≤1, and a+b+c=100;
[0009] The TaWRu alloy has a homogenized microstructure in the as-cast state; inside the fractured TaWRu alloy, there exist grain orientation differences and deformation bands generated by high-density dislocation slip, and no obvious transgranular propagation or intergranular crack propagation is observed.
[0010] Wherein, in the general formula, 91≤a≤94, 6≤b≤9, 0.25≤c≤0.75.
[0011] Wherein, the TaWRu alloy is a single BCC phase with equiaxed grains, and is substantially free of intermetallic compounds and other micro-nano scale precipitated phases.
[0012] Wherein, the yield strength of the TaWRu alloy at room temperature is 500 MPa or more, the tensile strength is 590 MPa or more, and the elongation after fracture is 20% or more;
[0013] The yield strength of the TaWRu alloy at -196 °C is 900 MPa or more, the tensile strength is 1000 MPa or more, and the elongation after fracture is 30% or more;
[0014] The yield strength of the TaWRu alloy at 1300 °C is 95 MPa or more, the tensile strength is 150 MPa or more, and the elongation after fracture is 30% or more.
[0015] The preparation process of the above-mentioned TaWRu alloy with easy cold workability, wide temperature range, high strength and high toughness comprises the following steps:
[0016] a. Weigh and prepare alloy raw materials containing Ta, W and Ru according to the above general formula for batching;
[0017] b. Subject the alloy raw material obtained in step a to smelting treatment to obtain an alloy ingot;
[0018] c. Subject the alloy ingot to cold rolling treatment to obtain a rolled alloy sheet; the total rolling reduction of the cold rolling treatment is 80-90%;
[0019] d. The alloy rolled sheet is subjected to vacuum heat treatment at 1400~1800 ℃, and the holding time of the vacuum heat treatment is at least 2 h. After the holding time is completed, it is cooled to obtain a wide temperature range high strength and toughness TaWRu alloy.
[0020] In step b, the smelting process is induction melting, electric arc melting, or suspension melting.
[0021] Specifically, the melting process in step b involves placing the alloy raw material in a melting furnace, evacuating it, and then filling it with inert gas to 0.05~0.1 MPa. The material is then melted at a temperature of 3000℃ or higher and held for 15~30 min before being transferred to a mold for cooling.
[0022] In step c, the single rolling amount of cold rolling is 2-3%, and the number of rolling cycles is more than 10.
[0023] In step d, the cooling rate is ≥20 °C / min.
[0024] Applications of the aforementioned easy-to-cold-work, wide-temperature-range, high-strength and high-toughness TaWRu alloy in extreme load environments.
[0025] The beneficial effects of this invention are as follows:
[0026] (1) The present invention significantly improves the room temperature cold working performance and comprehensive mechanical properties of TaW alloy by introducing Ru (ruthenium) element. The strength and toughness matching from low temperature of -196℃ to high temperature of 1300℃ is improved to a certain extent.
[0027] (2) The present invention greatly improves the room temperature cold working capability of the alloy through optimized composition design (especially the control of Ru content). The TaWRu alloy of the present invention can obtain excellent properties through simple room temperature rolling and heat treatment steps, realizing fine control of the alloy microstructure and obtaining excellent strength and plasticity matching.
[0028] (3) The preparation process of the present invention has a wide window and the equipment is conventional equipment, which is suitable for low-carbon industrial mass production and provides a new option for structural materials for extreme high temperature environments. Attached Figure Description
[0029] Figure 1 This is the ternary phase diagram of the TaWRu alloy, which is easy to cold work, has a wide temperature range, and is high in strength and toughness.
[0030] Figure 2 The image shows the EDS chemical element distribution of the as-cast TaWRu alloy ingot prepared in Example 1.
[0031] Figure 3 EBSD micrograph of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy prepared in Example 1.
[0032] Figure 4 The tensile curve is shown for the TaWRu alloy with wide temperature range that is easy to cold work and has high strength and toughness, prepared in Example 1.
[0033] Figure 5 EBSD images of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy prepared in Example 1 after fracture at different temperatures.
[0034] Figure 6 The TEM microstructures of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy prepared in Example 1 after fracture at different temperatures are shown; wherein... Figure 6 (a) shows the TEM microstructure at 500 nm after fracture at -196℃. Figure 6 (b) shows the TEM microstructure at 500 nm after fracture at 25℃. Figure 6 (c) shows the TEM microstructure at 500 nm after fracture at 1300℃. Figure 6 (d) in the figure represents the TEM microstructure at 200 nm after fracture at -196℃. Figure 6 (e) in the figure represents the TEM microstructure at 200 nm after fracture at 25 °C. Figure 6 (f) in the figure represents the TEM micro-deformation characteristics at 200 nm after fracture at 1300℃.
[0035] Figure 7 Comparative photographs of ingots cast at room temperature using different embodiments. Detailed Implementation
[0036] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.
[0037] Experimental methods not specified in the following examples are generally performed under standard conditions or as recommended by the manufacturer.
[0038] Unless otherwise specified, the raw materials and test materials used in the embodiments of this application were all purchased commercially.
[0039] The analytical measuring instruments used in the embodiments of this application are as follows:
[0040] Ternary alloy phase diagrams were constructed using Thermo-Calc 2025 software and corresponding data.
[0041] The alloy sample surface was ground using a Truly VP-430 and a Hitachi IM4000Ⅱ standard ion mill to prepare samples for microstructure observation and characterization.
[0042] The microstructure of the TaWRu alloy sample was characterized using a ZEISS EVO 18 scanning electron microscope.
[0043] Electron backscatter diffraction (EBSD) tests were performed on the alloy samples using an Apreo S LoVac thermal field emission scanning electron microscope.
[0044] Microscopic tissue observation was performed using a FEI Tecnai G2 F20 transmission electron microscope (TEM) and selected area electron diffraction (SAED) techniques, and chemical element distribution maps were obtained using the energy dispersive spectroscopy (EDS) function.
[0045] Dog-bone shaped tensile specimens of TaWRu alloy were prepared using a Ching Hung G43S immersion-type slow wire EDM machine from Taiwan, China.
[0046] The low-temperature and room-temperature mechanical properties of the alloy were measured using an AGS-X 10KN mechanical testing machine and an RVX-112B video extensometer.
[0047] The high-temperature mechanical properties of alloys were measured using an Instron 45582 twin-column electronic universal testing machine.
[0048] This application proposes a novel alloy design approach that introduces Ru into a Ta-W matrix. Ru, as a platinum group metal, has attracted attention in recent years for its unique physical and metallurgical properties in the modification of refractory alloys. Ru has a melting point of 2334℃ and an atomic radius similar to Ta and W. It exhibits high solid solubility in the Ta-W matrix, effectively hindering dislocation movement through solid solution strengthening, thereby enhancing the alloy's strength. Appropriate amounts of Ru can suppress W segregation at grain boundaries and avoid the formation of hard and brittle TaRu2 intermetallic compounds, ultimately purifying the grain boundaries and improving their strength. This lowers the ductile-brittle transition temperature, resulting in excellent cold workability at room temperature. Constructing a novel TaWRu-based alloy that combines high strength over a wide temperature range with good formability can overcome the "strength-ductility inversion" bottleneck of traditional refractory alloys and is expected to meet the application requirements of next-generation ultra-high temperature structural materials.
[0049] The readily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy of this application possesses two significant novel features: excellent room-temperature cold workability and high strength and toughness mechanical properties over a wide temperature range. In the alloy system of this application, Ta serves as the matrix element, providing good low-temperature plasticity and a solid solution matrix; W is the main solid solution strengthening element, significantly improving the high-temperature strength and creep resistance of the alloy; the addition of Ru is the core innovation of this application, and its mechanism of action includes: 1) a strong solid solution strengthening effect, as its atomic size differs significantly from Ta and W, effectively hindering dislocation movement; 2) reducing the stacking fault energy of the alloy, promoting the formation of twins during deformation, thereby improving plasticity while maintaining strength; 3) inhibiting the segregation of W at grain boundaries, purifying grain boundaries, improving grain boundary strength, and lowering the ductile-brittle transition temperature; 4) delaying recrystallization and coarsening of precipitated phases, improving the recrystallization temperature and high-temperature stability of the alloy.
[0050] The TaWRu alloy of this application, characterized by its easy cold workability and high strength and toughness over a wide temperature range, does not require cumbersome thermomechanical processing methods. It exhibits sufficient room-temperature ductility across a wide temperature range and simultaneously achieves higher room-temperature and high-temperature strength through only room-temperature cold rolling and a single heat treatment step. This unique and excellent room-temperature cold workability facilitates cold deformation processes such as room-temperature rolling and die cold pressing, making it highly suitable for rapid industrial application.
[0051] Example 1:
[0052] The wide-temperature-range high-strength and high-toughness TaWRu alloy of this embodiment has the following composition: Ta 92 W 7.5 Ru 0.5 at%.
[0053] Its preparation process includes the following steps:
[0054] a. Weigh the alloy raw materials containing Ta, W and Ru according to the above general formula and prepare the ingredients;
[0055] b. Place the alloy raw material in a melting furnace, evacuate it, and then fill it with inert gas to 0.05~0.1 MPa. Melt it at a temperature above 3000℃ and hold it for 15~30 min. Then transfer it to a mold and cool it for 20~30 min to obtain an alloy ingot.
[0056] c. The alloy ingot is cold rolled at room temperature, with a single rolling reduction of 2-3%, and more than 10 rolling passes, with a total rolling reduction of about 90%, to obtain alloy rolled sheet.
[0057] d. The alloy rolled plate was subjected to vacuum heat treatment at 1500 ℃ for 10 h, and then cooled in the furnace at a cooling rate of not less than 30 ℃ / min to obtain a uniform microstructure and a wide temperature range high strength and toughness TaWRu alloy.
[0058] Figure 1 This is the ternary phase diagram of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy of the present invention. Figure 1 As can be seen, the alloys prepared in the relevant embodiments of the present invention are all single BCC phases, with virtually no intermetallic compounds or other micro- or nano-scale precipitates.
[0059] Figure 2 This is an EDS chemical element distribution diagram of the as-cast TaWRu alloy ingot prepared in Example 1. Figure 2 It is evident that the as-cast TaWRu alloy ingot does not exhibit the chemical element segregation, shrinkage cavities, or porosity defects commonly found in traditionally melted and cast ingots. In this embodiment, the alloy exhibits a homogeneous microstructure immediately after melting, which helps prevent rapid fracture caused by microcracks and other defects during room temperature cold deformation.
[0060] Figure 3 EBSD micrograph of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy prepared in Example 1. Figure 3 It can be seen that the grain boundary of the wide-temperature-range high-strength and high-toughness TaWRu alloy obtained after melting, room temperature rolling and heat treatment is relatively uniform, and all of them are equiaxed grains.
[0061] Figure 4 Tensile curves of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy prepared in Example 1. Figure 4 It can be seen that the room temperature (25℃) yield strength of this alloy Tensile strength reaching over 500 MPa Reaching over 600 MPa, elongation at break The yield strength at -196℃ reaches over 30%. Tensile strength reaching over 900 MPa Reaching over 1000 MPa, elongation at break The yield strength of this alloy reaches over 30%. Tensile strength reaching over 100 MPa Reaching over 150 MPa, elongation at break It has reached over 30%.
[0062] Figure 5 EBSD images of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy prepared in Example 1 after fracture at different temperatures, with the fracture sites treated by mechanical polishing and ion polishing. Figure 5 It can be clearly observed that the alloy underwent varying degrees of deformation at different temperatures. Analysis of parameters such as grain reference orientation deviation and average grain orientation difference (KAM) reveals that, compared to... Figure 2The microstructure of the undeformed alloy is shown, while the deformed alloy exhibits deformation bands resulting from grain orientation differences and high-density dislocation slip. No significant transgranular or intergranular crack propagation is observed. This information preliminarily indicates that the alloy possesses strong and tough properties over a wide temperature range.
[0063] Figure 6 The TEM microstructures of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy prepared in Example 1 after fracture at different temperatures are shown; wherein... Figure 6 (a) shows the TEM microstructure at 500 nm after fracture at -196℃. Figure 6 (b) shows the TEM microstructure at 500 nm after fracture at 25℃. Figure 6 (c) shows the TEM microstructure at 500 nm after fracture at 1300℃. Figure 6 (d) in the figure represents the TEM microstructure at 200 nm after fracture at -196℃. Figure 6 (e) in the figure represents the TEM microstructure at 200 nm after fracture at 25 °C. Figure 6 (f) in the figure represents the TEM microstructure at 200 nm after fracture at 1300℃. Figure 6 As can be seen in (a) and (d), and (b) and (e), at lower temperatures, multiple slip systems (with different crystal planes and orientations) must be activated simultaneously to coordinate deformation in different grain directions. When dislocations from different slip systems meet during their motion, they cannot avoid each other by climbing; instead, they undergo dislocation reactions, "knotting" and intertwining to form dislocation entanglements. These entangled dislocations form dislocation walls, while the interior is a dislocation-free region, collectively forming dislocation cells. This creates a honeycomb-like dislocation cell structure. Essentially, this is a minimum energy configuration adopted by materials to accommodate large amounts of plastic deformation when recovery is impossible.
[0064] from Figure 6 As can be seen in (c) and (f), at high temperatures, atoms acquire sufficient diffusion energy, and this high energy facilitates dislocation climb and cross-slip. Dislocations spontaneously rearrange from a disordered tangled state, forming low-energy, ordered two-dimensional or three-dimensional network structures. The entire alloy transforms a disordered high-energy state into an ordered low-energy state. Initially, quadrilateral dislocation networks form, which then gradually transform into hexagonal and near-quadrilateral networks. This unique dislocation movement at different temperatures allows the alloy to exhibit superior strength and toughness compared to traditional TaW alloys.
[0065] Example 2:
[0066] The wide-temperature-range high-strength and high-toughness TaWRu alloy of this embodiment has the following composition: Ta 92 W 7.5 Ru 0.5 at%.
[0067] Its preparation process includes the following steps:
[0068] a. Weigh the alloy raw materials containing Ta, W and Ru according to the above general formula and prepare the ingredients;
[0069] b. Place the alloy raw material in a melting furnace, evacuate it, and then fill it with inert gas to 0.05~0.1 MPa. Melt it at a temperature above 3000℃ and hold it for 15~30 min. Then transfer it to a mold and cool it for 20~30 min to obtain an alloy ingot.
[0070] c. The alloy ingot is cold rolled at room temperature, with a single rolling reduction of 2-3%, and more than 10 rolling passes, with a total rolling reduction of about 90%, to obtain alloy rolled sheet.
[0071] d. The alloy rolled plate was subjected to vacuum heat treatment at 1800 ℃ for 10 h, and then cooled in the furnace at a cooling rate of not less than 30 ℃ / min to obtain a uniform microstructure and a wide temperature range high strength and toughness TaWRu alloy.
[0072] Example 3:
[0073] The wide-temperature-range high-strength and high-toughness TaWRu alloy of this embodiment has the following composition: Ta 92 W 7.5 Ru 0.5 at%.
[0074] Its preparation process includes the following steps:
[0075] a. Weigh the alloy raw materials containing Ta, W and Ru according to the above general formula and prepare the ingredients;
[0076] b. Place the alloy raw material in a melting furnace, evacuate it, and then fill it with inert gas to 0.05~0.1 MPa. Melt it at a temperature above 3000℃ and hold it for 15~30 min. Then transfer it to a mold and cool it for 20~30 min to obtain an alloy ingot.
[0077] c. The alloy ingot is cold rolled at room temperature, with a single rolling reduction of 2-3%, and more than 10 rolling passes, with a total rolling reduction of about 90%, to obtain alloy rolled sheet.
[0078] d. The alloy rolled plate was subjected to vacuum heat treatment at 1500 ℃ for 2 h, and then cooled in the furnace at a cooling rate of not less than 30 ℃ / min to obtain a uniform microstructure and a wide temperature range high strength and toughness TaWRu alloy.
[0079] Example 4:
[0080] The wide-temperature-range high-strength and high-toughness TaWRu alloy of this embodiment has the following composition: Ta 92 W 7.5 Ru 0.5 at%.
[0081] Its preparation process includes the following steps:
[0082] a. Weigh the alloy raw materials containing Ta, W and Ru according to the above general formula and prepare the ingredients;
[0083] b. Place the alloy raw material in a melting furnace, evacuate it, and then fill it with inert gas to 0.05~0.1 MPa. Melt it at a temperature above 3000℃ and hold it for 15~30 min. Then transfer it to a mold and cool it for 20~30 min to obtain an alloy ingot.
[0084] c. The alloy ingot is cold rolled at room temperature, with a single rolling reduction of 2-3%, and more than 10 rolling passes, with a total rolling reduction of about 90%, to obtain alloy rolled sheet.
[0085] d. The alloy rolled plate was subjected to vacuum heat treatment at 1500 ℃ for 12 h, and then cooled in the furnace at a cooling rate of not less than 30 ℃ / min to obtain a uniform microstructure and a wide temperature range high strength and toughness TaWRu alloy.
[0086] Example 5:
[0087] The wide-temperature-range high-strength and high-toughness TaWRu alloy of this embodiment has the following composition: Ta 92 W 7.5 Ru 0.5 at%.
[0088] Its preparation process includes the following steps:
[0089] a. Weigh the alloy raw materials containing Ta, W and Ru according to the above general formula and prepare the ingredients;
[0090] b. Place the alloy raw material in a melting furnace, evacuate it, and then fill it with inert gas to 0.05~0.1 MPa. Melt it at a temperature above 3000℃ and hold it for 15~30 min. Then transfer it to a mold and cool it for 20~30 min to obtain an alloy ingot.
[0091] c. The alloy ingot is cold rolled at room temperature, with a single rolling reduction of 2-3%, and more than 10 rolling passes, with a total rolling reduction of about 90%, to obtain alloy rolled sheet.
[0092] d. The alloy rolled plate was subjected to vacuum heat treatment at 1800 ℃ for 2 h, and then cooled in the furnace at a cooling rate of not less than 30 ℃ / min to obtain a uniform microstructure and a wide temperature range high strength and toughness TaWRu alloy.
[0093] Example 6:
[0094] The wide-temperature-range high-strength and high-toughness TaWRu alloy of this embodiment has the following composition: Ta 92 W 7.75 Ru 0.25 at%.
[0095] Its preparation process includes the following steps:
[0096] a. Weigh the alloy raw materials containing Ta, W and Ru according to the above general formula and prepare the ingredients;
[0097] b. Place the alloy raw material in a melting furnace, evacuate it, and then fill it with inert gas to 0.05~0.1 MPa. Melt it at a temperature above 3000℃ and hold it for 15~30 min. Then transfer it to a mold and cool it for 20~30 min to obtain an alloy ingot.
[0098] c. The alloy ingot is cold rolled at room temperature, with a single rolling reduction of 2-3%, and more than 10 rolling passes, with a total rolling reduction of about 90%, to obtain alloy rolled sheet.
[0099] d. The alloy rolled plate is subjected to vacuum heat treatment at 1500 ℃ for 10 h, and then cooled in the furnace at a cooling rate of not less than 30 ℃ / min to obtain a uniform microstructure and a wide temperature range high strength and toughness TaWRu alloy.
[0100] Example 7:
[0101] The wide-temperature-range high-strength and high-toughness TaWRu alloy of this embodiment has the following composition: Ta 92 W 7.5 Ru 0.5 at%.
[0102] Its preparation process includes the following steps:
[0103] a. Weigh the alloy raw materials containing Ta, W and Ru according to the above general formula and prepare the ingredients;
[0104] b. Place the alloy raw material in a melting furnace, evacuate it, and then fill it with inert gas to 0.05~0.1 MPa. Melt it at a temperature above 3000℃ and hold it for 15~30 min. Then transfer it to a mold and cool it for 20~30 min to obtain an alloy ingot.
[0105] c. The alloy ingot is cold rolled at room temperature, with a single rolling reduction of 2-3%, and more than 10 rolling passes, with a total rolling reduction of about 90%, to obtain alloy rolled sheet.
[0106] d. The alloy rolled plate was subjected to vacuum heat treatment at 1800 ℃ for 2 h, and then cooled in the furnace at a cooling rate of not less than 30 ℃ / min to obtain a uniform microstructure and a wide temperature range high strength and toughness TaWRu alloy.
[0107] Example 8:
[0108] The wide-temperature-range high-strength and high-toughness TaWRu alloy of this embodiment has the following composition: Ta 92 W 7.25 Ru 0.75 at%.
[0109] Its preparation process includes the following steps:
[0110] a. Weigh the alloy raw materials containing Ta, W and Ru according to the above general formula and prepare the ingredients;
[0111] b. Place the alloy raw material in a melting furnace, evacuate it, and then fill it with inert gas to 0.05~0.1 MPa. Melt it at a temperature above 3000℃ and hold it for 15~30 min. Then transfer it to a mold and cool it for 20~30 min to obtain an alloy ingot.
[0112] c. The alloy ingot is cold rolled at room temperature, with a single rolling reduction of 2-3%, and more than 10 rolling passes, with a total rolling reduction of about 90%, to obtain alloy rolled sheet.
[0113] d. The alloy rolled plate is subjected to vacuum heat treatment at 1500 ℃ for 10 h, and then cooled in the furnace at a cooling rate of not less than 30 ℃ / min to obtain a uniform microstructure and a wide temperature range high strength and toughness TaWRu alloy.
[0114] Example 9:
[0115] The wide-temperature-range high-strength and high-toughness TaWRu alloy of this embodiment has the following composition: Ta 92 W 7.25 Ru 0.75 at%.
[0116] Its preparation process includes the following steps:
[0117] a. Weigh the alloy raw materials containing Ta, W and Ru according to the above general formula and prepare the ingredients;
[0118] b. Place the alloy raw material in a melting furnace, evacuate it, and then fill it with inert gas to 0.05~0.1 MPa. Melt it at a temperature above 3000℃ and hold it for 15~30 min. Then transfer it to a mold and cool it for 20~30 min to obtain an alloy ingot.
[0119] c. The alloy ingot is cold rolled at room temperature, with a single rolling reduction of 2-3%, and more than 10 rolling passes, with a total rolling reduction of about 90%, to obtain alloy rolled sheet.
[0120] d. The alloy rolled plate was subjected to vacuum heat treatment at 1800 ℃ for 2 h, and then cooled in the furnace at a cooling rate of not less than 30 ℃ / min to obtain a uniform microstructure and a wide temperature range high strength and toughness TaWRu alloy.
[0121] Example 10:
[0122] The wide-temperature-range high-strength and high-toughness TaWRu alloy of this embodiment has the following composition: Ta 92 W7Ru1 at%.
[0123] Its preparation process includes the following steps:
[0124] a. Weigh the alloy raw materials containing Ta, W and Ru according to the above general formula and prepare the ingredients;
[0125] b. Place the alloy raw material in a melting furnace, evacuate it, and then fill it with inert gas to 0.05~0.1 MPa. Melt it at a temperature above 3000℃ and hold it for 15~30 min. Then transfer it to a mold and cool it for 20~30 min to obtain an alloy ingot.
[0126] c. The alloy ingot is cold rolled at room temperature, with a single rolling reduction of 2-3%, and more than 10 rolling passes, with a total rolling reduction of about 80%, to obtain alloy rolled sheet.
[0127] d. The alloy rolled plate is subjected to vacuum heat treatment at 1500 ℃ for 10 h, and then cooled in the furnace at a cooling rate of not less than 30 ℃ / min to obtain a uniform microstructure and a wide temperature range high strength and toughness TaWRu alloy.
[0128] Comparative Example 1:
[0129] Comparative Example 1: Preparation of Ta 93 The W7 (at.%) binary alloy was prepared using the same process as in Example 1.
[0130] Comparative Example 2:
[0131] Comparative Example 2 Preparation of Ta 93 The preparation process of the W7 (at.%) binary alloy differs from that of Example 1 in that vacuum heat treatment is performed at 1800 °C in step d, and the holding time is 10 h.
[0132] Comparative Example 3:
[0133] Preparation of Ta in Comparative Example 3 93The preparation process of the W7 (at.%) binary alloy differs from that of Example 1 in that vacuum heat treatment is performed at 1800 °C in step d, and the holding time is 2 h.
[0134] Comparative Example 4:
[0135] The technical solution comes from patent application CN113319292A, and the alloy composition is Ta. 88 W 12 Specifically, the TaW alloy is prepared based on laser selective melting and then subjected to vacuum heat treatment at 900 ℃ for 2 hours.
[0136] Comparative Example 5:
[0137] The technical solution comes from patent application CN113319292A, and the alloy composition is Ta. 88 W 12 Specifically, the TaW alloy is prepared based on laser selective melting and then subjected to vacuum heat treatment at 1500 ℃ for 2 hours.
[0138] Comparative Example 6:
[0139] The technical solution is derived from the high-temperature mechanical properties of Ta-10W alloy in the literature "Rare Metals Materials and Engineering 2006 Volume 35, Suppl.2". The alloy composition is Ta 90 W 10 The specific process is hot forging + cold working + recrystallization vacuum annealing.
[0140] The mechanical properties of the alloys obtained in Examples 1 to 5 and Comparative Examples 1 to 6 are shown in Table 1.
[0141] Table 1 Mechanical properties of the alloys obtained in Examples 1 to 5 and Comparative Examples 1 to 6
[0142]
[0143] As can be seen from Table 1, the wide-temperature-range high-strength and high-toughness TaWRu alloy prepared in this application has a yield strength at room temperature (25℃). Tensile strength of 500 MPa or more With an elongation of over 590 MPa, the elongation is... It is above 30%; yield strength at -196 ℃ Tensile strength is above 900 MPa. For a strength of 1000 MPa or higher, the elongation at break is It is over 30%; yield strength at 1300 ℃ Tensile strength is above 95 MPa. The strength is 150 MPa, and the elongation at break is... It is over 30%.
[0144] Depend on Figure 4 Tensile test data and Figure 5 The microstructure of the fractured structure after tensile testing shows that the addition of an appropriate amount of Ru results in excellent low-temperature toughness of the alloy, with no brittle fracture morphology observed. This indicates that the DBTT (ductile-brittle transition temperature) of the alloy can be lowered to below -196℃, while simultaneously achieving yield strength at -196℃. ≥900 MPa, elongation at break The optimal combination of ≥12% meets the stringent requirements of structural materials for alternating extreme low-temperature and ultra-high-temperature service scenarios.
[0145] The performance data from Examples 1 to 5 and Comparative Examples 1 to 3 show that the addition of trace amounts of Ru, combined with appropriate heat treatment, improves both the strength and toughness of the alloy. Across the entire temperature range, compared to the Ru-free TaW alloy, the tensile strength increases by approximately 8-14.8%, while the elongation remains above approximately 30%. The Ru doping not only ensures good plasticity at room temperature, allowing for 90% crack-free rolling at room temperature, but also utilizes solid solution strengthening and grain refinement mechanisms to synergistically enhance the alloy's strength and toughness over a wide temperature range.
[0146] As can be seen from the performance data of Examples 1 and Comparative Examples 4 to 5, the wide-temperature-range high-toughness alloy designed in this invention maintains an elongation of over 30% from liquid nitrogen service temperature to ultra-high temperature environments, which is several times higher than that of alloys disclosed in other inventions. This indicates that the alloy possesses excellent formability and processability (good processability), superior fracture safety and energy absorption buffering capacity (high safety), and effective stress relaxation and load redistribution (strong overload resistance) across a wide temperature range, making it better suited for high-safety-margin applications such as aerospace and nuclear industries.
[0147] The performance data from Example 1 and Comparative Example 6 show that the high-temperature strength is enhanced after adding trace amounts of Ru and undergoing appropriate heat treatment. The tensile strength of the alloy at 1300°C is approximately 201 MPa, which is close to the high-temperature strength of the Ru-free alloy at 1000°C. This indicates that the alloy can withstand harsher service environments at higher temperatures.
[0148] Figure 7 Comparative photographs of ingots cast at room temperature using different embodiments. From Figure 7 It can be seen that Ta in Examples 1 and 2 92 W 7.5 Ru 0.5The alloy ingots of Example 6 and Example 8 showed few edge cracks after rolling, indicating excellent room temperature cold working performance. The alloys of Example 6 and Example 8 showed a few edge cracks after rolling, and the surface of the alloy of Example 8 had a distinct metallic luster after rolling; while the alloy of Comparative Example 1 had a rough surface and was generally dark black. This indicates that excessive or insufficient Ru doping drastically reduces the room temperature working ability of the alloy, which is detrimental to cold deformation processing.
[0149] This application achieves excellent mechanical properties across a full temperature range from -196 °C to 1300 °C by simultaneously enhancing strength and plasticity at liquid nitrogen temperature through alloying while maintaining a low ductile-brittle transition temperature. The wide-temperature-range, high-strength and high-toughness TaWRu alloy of this application exhibits a homogeneous microstructure in its as-cast state, free from common melting defects such as segregation and shrinkage cavities, allowing for direct cold deformation processing. The TaWRu alloy maintains high strength and uniform, coordinated deformation at different temperatures, without significant transgranular or intergranular crack propagation. The TaWRu alloy of this application, after simple room-temperature cold deformation processing and a single-step heat treatment, exhibits high yield strength, high tensile strength, and high elongation from liquid nitrogen temperature (-196 °C) to ultra-high temperatures (1300 °C), making it suitable for industrial-scale production. The wide-temperature-range high-strength and high-toughness TaWRu alloy of this application exhibits high yield strength, high tensile strength, and high elongation from liquid nitrogen temperature (-196℃) to ultra-high temperature (1300℃), and maintains good mechanical property stability under extreme service environment temperatures from low to high temperatures. It has good room temperature plastic processing capability and is simple to process. The preparation process of this application is simple and has low requirements, making it suitable for promotion and application in extreme application environments such as aerospace and nuclear industry.
[0150] In summary, the TaWRu alloy of this application exhibits a good balance of strength and toughness over a wide temperature range, meeting the application requirements in extremely harsh service environments. This application is of great significance for expanding the types of metallic structural materials and their application research in extreme load environments.
[0151] Those skilled in the art will readily understand that the above description is merely a preferred embodiment of the present invention. The above embodiments are provided only for the purpose of describing the present invention and are not intended to limit the present invention. Parts not described in detail in this specification are well-known in the art and are not intended to limit the scope of the present invention. The scope of the present invention is defined by the appended claims. All equivalent substitutions and modifications made without departing from the spirit and principle of the present invention should be covered within the scope of the present invention.
Claims
1. A wide-temperature-range high-strength and high-toughness TaWRu alloy that is easy to cold work, characterized in that, The composition of this TaWRu alloy satisfies the general formula Ta a W b Ru c , where a, b and c respectively represent the atomic percentages of the corresponding alloying elements, 90≤a≤95, 5≤b≤10, 0<c≤1, and a+b+c=100; The TaWRu alloy exhibits a homogeneous microstructure in the as-cast state; after fracture, the TaWRu alloy contains deformation bands caused by grain orientation differences and high-density dislocation slip, but there is no obvious transgranular propagation or intergranular crack propagation.
2. The easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy according to claim 1, characterized in that, In the general formula, 91≤a≤94, 6≤b≤9, and 0.25≤c≤0.
75.
3. The easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy according to claim 1, characterized in that, The TaWRu alloy is a single BCC phase with equiaxed grains and virtually no intermetallic compounds or other micro / nano-scale precipitates.
4. The easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy according to claim 1, characterized in that, The TaWRu alloy has a yield strength of over 500 MPa, a tensile strength of over 590 MPa, and an elongation at break of over 20% at room temperature. The TaWRu alloy has a yield strength of over 900 MPa, a tensile strength of over 1000 MPa, and a fracture elongation of over 30% at -196 ℃. The TaWRu alloy has a yield strength of ≥95 MPa, a tensile strength of ≥150 MPa, and an elongation at break of ≥30% at 1300 ℃.
5. The preparation process of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy according to any one of claims 1 to 4, characterized in that, Includes the following steps: a. Weigh the alloy raw materials containing Ta, W and Ru according to the above general formula and prepare the ingredients; b. The alloy raw material obtained in step a is smelted to obtain an alloy ingot; c. The alloy ingot is cold-rolled to obtain an alloy rolled sheet; the total reduction during cold rolling is 80-90%. d. The alloy rolled sheet is subjected to vacuum heat treatment at 1400~1800 ℃, and the holding time of the vacuum heat treatment is at least 2 h. After the holding time is completed, it is cooled to obtain a wide temperature range high strength and toughness TaWRu alloy.
6. The preparation process of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy according to claim 5, characterized in that, The smelting process in step b is induction melting, electric arc melting, or suspension melting.
7. The preparation process of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy according to claim 6, characterized in that, The melting process in step b is as follows: the alloy raw material is placed in a melting furnace, vacuumed and then filled with inert gas to 0.05~0.1 MPa, melted at 3000℃ or above and held for 15~30 min, and then transferred to a mold to cool.
8. The preparation process of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy according to claim 5, characterized in that, In step c, the single rolling amount of cold rolling is 2-3%, and the number of rolling cycles is more than 10.
9. The preparation process of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy according to claim 5, characterized in that, The cooling rate in step d is ≥20 °C / min.
10. The application of the easily cold-workable, wide-temperature-range, high-strength and high-toughness TaWRu alloy according to any one of claims 1 to 4 in extreme load environments.
Citation Information
Patent Citations
Tantalum-tungsten alloy preparation process based on selective laser melting forming and tantalum-tungsten alloy
CN113319292A