A method and component for ultrasonic shot peening and hydrothermal corrosion protection of AZ80 magnesium alloy
By forming a surface plastic deformation defect layer on the surface of forged T6 AZ80 magnesium alloy components and performing hydrothermal treatment, the nucleation and growth of Mg(OH)2 are regulated, solving the problems of microgalvanic corrosion and insufficient density of the protective coating in forged T6 AZ80 magnesium alloy components, and achieving better corrosion resistance and component service performance.
Patent Information
- Application Number
- CN202611482741.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing forged T6 state AZ80 magnesium alloy components are prone to microgalvanic corrosion in corrosive environments. The Mg(OH)2 nanosheets formed after hydrothermal treatment are large in size and have high inter-sheet porosity, resulting in insufficient density and long-term corrosion protection performance of the protective coating.
Ultrasonic shot peening was used to form a surface plastic deformation defect layer on the surface of forged T6 AZ80 magnesium alloy components. Then, hydrothermal treatment was performed without grinding or polishing. The surface plastic deformation defect layer was used as a heterogeneous nucleation site to regulate the nucleation and growth of Mg(OH)2 and form a dense Mg(OH)2 protective coating.
It significantly reduces the size of Mg(OH)2 nanosheets, decreases inter-sheet porosity, improves the density and scratch resistance of the protective coating, enhances long-term corrosion resistance, and does not damage the original matrix structure and mechanical properties of the component.
Smart Images

Figure CN123108448A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of magnesium alloy surface treatment and corrosion protection technology, and in particular to an ultrasonic shot peening hydrothermal corrosion protection method and component for AZ80 magnesium alloy. Background Technology
[0002] Magnesium alloys possess advantages such as low density and high specific strength, making them promising candidates for applications in new energy vehicles and lightweight load-bearing components. AZ80 magnesium alloy, after forging and T6 heat treatment, achieves good strength and plasticity, making it suitable for manufacturing forged load-bearing components such as vehicle crankshafts.
[0003] However, Mg precipitates inside the forged T6 state AZ80 magnesium alloy. 17 Al 12 The second phase consists of an α-Mg matrix and Mg. 17 Al 12 A significant Voltaic potential difference exists between the second phase and the Mg phase. In corrosive environments such as rainwater, sweat, and salt spray, the α-Mg matrix and Mg... 17 Al 12 Microgalvanic corrosion can easily form between the second phases, leading to localized pitting corrosion in the component. As corrosion time increases, the localized corrosion area may continue to expand, affecting the component's service performance and service life.
[0004] Hydrothermal corrosion protection of magnesium alloys is an environmentally friendly surface modification technology. In an alkaline hydrothermal environment, a protective coating with Mg(OH)₂ as the main phase can be formed in situ on the magnesium alloy surface, thus preventing corrosive media from contacting the magnesium alloy substrate. Current hydrothermal treatment methods typically involve first grinding or polishing the magnesium alloy surface with sandpaper, followed by direct hydrothermal treatment. Because the number of nucleation sites available for hydrothermal reactions on the ground or polished surface is limited, the Mg(OH)₂ nanosheets formed during hydrothermal treatment tend to grow laterally, resulting in large nanosheet sizes and high inter-sheet porosity. Corrosive media such as chloride ions and water molecules can easily penetrate into the magnesium alloy substrate through these inter-sheet pores. Therefore, the resulting protective coating still has insufficient corrosion protection performance under long-term immersion conditions, making it difficult to meet the corrosion protection requirements for long-term service of forged load-bearing components.
[0005] Ultrasonic shot peening is a mechanical surface modification method that uses ultrasonic vibration to drive shot at high speed to impact the workpiece surface, causing plastic deformation of the substrate surface layer and introducing residual compressive stress and crystal defects. Current ultrasonic shot peening treatments are mainly used to refine the surface grains of the substrate, introduce residual compressive stress, and improve the fatigue properties of the substrate. To reduce surface undulations caused by ultrasonic shot peening or to remove the plastically deformed surface layer formed by ultrasonic shot peening, existing processes typically involve grinding or polishing after ultrasonic shot peening.
[0006] After ultrasonic shot peening, subsequent grinding or polishing can partially or completely remove the high-density dislocations, surface defects, and surface plastic deformation layer introduced by ultrasonic shot peening on the workpiece surface. Currently, ultrasonic shot peening and hydrothermal corrosion protection are usually used separately. There is still a lack of a complete set of processing technology suitable for forging T6 state AZ80 magnesium alloy components, which utilizes the surface plastic deformation defect layer formed after ultrasonic shot peening to control the nucleation and growth process of Mg(OH)2 in the subsequent hydrothermal reaction.
[0007] Furthermore, existing research on hydrothermal corrosion protection of magnesium alloys primarily focuses on cast or extruded flat plate specimens, with relatively insufficient research on its applicability to actual forged T6-temper AZ80 magnesium alloy components. Flat plate specimens differ from forged load-bearing components such as vehicle cranks in terms of material state, microstructure, and surface shape. Therefore, hydrothermal corrosion protection processes developed for flat plate specimens may not be directly applicable to actual forged T6-temper AZ80 magnesium alloy components.
[0008] Therefore, how to regulate the nucleation and growth of Mg(OH)2 during hydrothermal treatment, reduce the size of Mg(OH)2 nanosheets, decrease inter-sheet porosity, and improve the density of the protective coating, thereby improving the scratch resistance and long-term corrosion resistance of the components, without damaging the original matrix structure and mechanical properties of the forged T6 state AZ80 magnesium alloy components, is a technical problem to be solved in this field. Summary of the Invention
[0009] The purpose of this invention is to solve the problem of existing forged T6 state AZ80 magnesium alloy components due to the α-Mg matrix and Mg... 17 Al 12 To address the issues of insufficient corrosion resistance due to micro-galvanic corrosion between the second phases, as well as the problems of large size, high inter-plate porosity, insufficient density of protective coatings, and insufficient long-term corrosion resistance of Mg(OH)2 nanosheets obtained by existing hydrothermal treatment, this paper provides a hydrothermal anti-corrosion method and component for ultrasonic shot peening of AZ80 magnesium alloy.
[0010] To achieve the above objectives, the embodiments of the present invention provide the following technical solutions:
[0011] A hydrothermal ultrasonic shot peening method for corrosion protection of AZ80 magnesium alloy includes the following steps:
[0012] The surface of the forged T6 state AZ80 magnesium alloy component to be treated is subjected to ultrasonic shot peening to form a surface plastic deformation defect layer on the surface to be treated.
[0013] After ultrasonic shot peening, the surface to be treated is not ground or polished, but the component is cleaned so that the surface plastic deformation defect layer is retained on the surface to be treated.
[0014] The component, after cleaning and retaining the surface plastic deformation defect layer, is placed in an aqueous sodium hydroxide solution for hydrothermal treatment, thereby forming a protective coating with Mg(OH)2 as the main phase in situ on the surface to be treated.
[0015] Furthermore, the ultrasonic shot peening process uses zirconia shot with a diameter of 2.5~3.5mm, an ultrasonic vibration frequency of 18~22 kHz, and a shot peening time of 15~25 min.
[0016] Furthermore, the ultrasonic shot peening process uses zirconia shot with a diameter of 2.8~3.2mm, an ultrasonic vibration frequency of 19~21 kHz, and a shot peening time of 18~22 min.
[0017] Furthermore, the ultrasonic peening equipment used in the ultrasonic shot peening process has an adjustable ultrasonic amplitude range of 20~60 μm and an adjustable ultrasonic output power range of 400~1000 W; the shot peening chamber of the ultrasonic shot peening equipment is a closed cavity, and the shot is placed in the shot peening chamber and moves back and forth at high speed under the drive of ultrasonic vibration to impact the surface of the component to be treated; during the ultrasonic shot peening process, the component is rotated at regular intervals so that the surface of the component to be treated receives the shot impact evenly.
[0018] Furthermore, the diameter of the zirconia shot is 3 mm, the ultrasonic vibration frequency is 20 kHz, and the shot peening time is 20 min.
[0019] Furthermore, after ultrasonic shot peening, the component is ultrasonically cleaned with deionized water and anhydrous ethanol in sequence, and then dried with cold air to remove shot fragments and contaminants.
[0020] Further, the molar concentration of NaOH in the sodium hydroxide aqueous solution is 0.8~1.2 mol / L; further, the molar concentration of NaOH in the sodium hydroxide aqueous solution is 0.9~1.1 mol / L; preferably, the molar concentration of NaOH in the sodium hydroxide aqueous solution is 1 mol / L.
[0021] Furthermore, the temperature of the hydrothermal treatment is 115~135 ℃, and the holding time is 5~7 h; further, the holding time is 5.5~6.5 h; preferably, the temperature of the hydrothermal treatment is 125 ℃, and the holding time is 6 h.
[0022] Furthermore, before the ultrasonic shot peening treatment, the surface to be treated is polished step by step with SiC sandpaper, and then ultrasonically cleaned with anhydrous ethanol and dried with cold air.
[0023] Furthermore, the AZ80 magnesium alloy comprises, by mass fraction, 7.8%~9.2% Al, 0.2%~0.8% Zn, and 0.15%~0.50% Mn, with the balance being Mg and unavoidable impurities.
[0024] Furthermore, the forged T6 state AZ80 magnesium alloy component is obtained through the following process: forging after preheating at 400 ℃ for 2 h, solution treatment at 420 ℃ for 2 h followed by water quenching, artificial aging at 180 ℃ for 24 h, and air cooling.
[0025] Another objective of this invention is to provide an AZ80 magnesium alloy component, wherein the component is a forged T6 state AZ80 magnesium alloy component obtained by the above-mentioned ultrasonic shot peening hydrothermal anti-corrosion method for AZ80 magnesium alloy; the component includes a forged T6 state AZ80 magnesium alloy substrate and a protective coating formed in situ on the surface of the forged T6 state AZ80 magnesium alloy substrate, wherein the main phase of the protective coating is Mg(OH)2.
[0026] Furthermore, the Mg(OH)2 in the protective coating is in the form of nanosheets.
[0027] Furthermore, the average lateral dimension of the Mg(OH)2 nanosheets in the protective coating is 28~38 nm, the inter-sheet porosity is ≤0.6%, and the thickness of the protective coating is 7.5~9.5 μm.
[0028] Furthermore, the Mg(OH)2 nanosheets in the protective coating have an average lateral dimension of 31.8 nm, an inter-sheet porosity of 0.4%, and a thickness of 8.7 μm.
[0029] Furthermore, the component is a lightweight forged load-bearing component similar to a vehicle crank.
[0030] In this invention, during ultrasonic shot peening, high-speed projectiles impact the surface of a forged T6-state AZ80 magnesium alloy component, causing surface plastic deformation and introducing high-density dislocations and surface irregularities. After ultrasonic shot peening, the surface is not ground or polished, thus preserving the surface plastic deformation defect layer formed by the ultrasonic shot peening.
[0031] In the alkaline environment created by subsequent hydrothermal treatment, the high-energy defect sites in the surface plastic deformation defect layer provide a large number of heterogeneous nucleation sites, significantly increasing the nucleation density of Mg(OH)₂ and regulating its nucleation and growth kinetics. This results in the in-situ formation of a protective coating with Mg(OH)₂ as the main phase on the surface of the component to be treated. The solute in the reaction system is distributed by a large number of crystal nuclei, thus limiting the excessive lateral growth of Mg(OH)₂ nanosheets. Simultaneously, the surface undulations created by ultrasonic shot peening on the surface to be treated facilitate the multi-oriented growth and interlocking stacking of Mg(OH)₂ nanosheets, resulting in a Mg(OH)₂ protective coating with smaller nanosheet size, denser structure, and increased thickness.
[0032] The dense protective coating forms a physical barrier, preventing corrosive media from penetrating into the forged T6 state AZ80 magnesium alloy matrix and blocking the interaction between the α-Mg matrix and Mg. 17 Al 12 The ultrasonic shot peening process creates micro-galvanic corrosion channels between the second phases, thereby inhibiting micro-galvanic corrosion. Ultrasonic shot peening itself does not generate new phases; the main phase of the resulting protective coating remains Mg(OH)2. Ultrasonic shot peening primarily regulates the nucleation and growth kinetics of Mg(OH)2 in subsequent hydrothermal reactions by preserving a surface plastic deformation defect layer on the surface of the component to be treated.
[0033] The beneficial effects of this invention are as follows:
[0034] 1. This invention is not a simple sequential combination of ultrasonic shot peening and hydrothermal treatment. Instead, it avoids grinding or polishing the surface of the component after ultrasonic shot peening, thus preserving the surface plastic deformation defect layer formed by the ultrasonic shot peening. The high dislocations and crystal defects in this surface plastic deformation defect layer can serve as heterogeneous nucleation sites for subsequent hydrothermal reactions, increasing the nucleation density of Mg(OH)₂ and inhibiting excessive lateral growth of Mg(OH)₂ nanosheets, thereby achieving control over the nucleation and growth process of the protective coating.
[0035] Compared with the AZ80-H sample that underwent hydrothermal treatment without ultrasonic shot peening, the average lateral size of the Mg(OH)2 nanosheets in the AZ80-SH sample obtained by this invention decreased from 51.7 nm to 31.8 nm, a reduction of 38.5%; the inter-sheet porosity decreased from 2.3% to 0.4%, a reduction of over 80%; and the protective coating thickness increased from 6.1 μm to 8.7 μm, an increase of 42.6%. The main phase of the obtained protective coating is still Mg(OH)2. Ultrasonic shot peening did not change the main chemical composition of the protective coating, but rather regulated the nucleation and growth kinetics of Mg(OH)2 by retaining the surface plastic deformation defect layer. Therefore, the microstructure regulation effect of the coating obtained is not a simple superposition of the effects of ultrasonic shot peening and hydrothermal treatment.
[0036] 2. This invention can significantly improve the density of the protective coating, prolong the path for chloride ions and water molecules to penetrate into the substrate through the protective coating, and effectively block the electrolyte from reaching the forged T6 state AZ80 magnesium alloy substrate, thereby inhibiting the interaction between the α-Mg matrix and Mg. 17 Al 12 Micro-galvanic corrosion between the second phases. Electrochemical test results show that the charge transfer impedance of the AZ80-SH sample obtained in this invention reaches 67370 Ω·cm. 2 The value was significantly higher than that of the AZ80-H sample, which underwent hydrothermal treatment directly without ultrasonic shot peening (2605 Ω·cm). 2 This indicates that the obtained protective coating has better electrochemical corrosion protection performance.
[0037] 3. The surface undulations created by ultrasonic shot peening on the surface of the component to be treated are conducive to the multi-oriented growth and interlocking stacking of Mg(OH)2 nanosheets, thereby enhancing the mechanical interlocking between the protective coating and the substrate and improving the scratch resistance of the protective coating. The maximum scratch indentation depth of the AZ80-SH sample obtained by this invention was reduced from 49.3 μm for the AZ80-H sample that was directly hydrothermally treated without ultrasonic shot peening to 38.8 μm.
[0038] 4. The protective coating obtained by this invention exhibits excellent long-term corrosion resistance. After immersion in a 5 wt.% NaCl solution for 250 h, the cumulative hydrogen evolution of the AZ80-SH sample obtained by this invention is less than 0.5 mL / cm³. 2 The cumulative hydrogen evolution of the AZ80-H sample, which underwent hydrothermal treatment directly without ultrasonic shot peening, was 4.7 mL / cm³. 2 The cumulative hydrogen evolution of the bare AZ80 substrate without ultrasonic shot peening and hydrothermal treatment was 12 mL / cm³. 2 The maximum corrosion depth of the AZ80-SH sample obtained by this invention is 50 μm, which is 96% lower than that of the bare AZ80 substrate and 69% lower than that of the AZ80-H sample. This indicates that the present invention can significantly improve the long-term chloride ion corrosion resistance of forged T6 state AZ80 magnesium alloy components.
[0039] 5. The hydrothermal reaction of this invention uses a water-based system, making the overall process environmentally friendly. This method forms a protective coating on the surface of forged T6-state AZ80 magnesium alloy components without altering the original microstructure of the forged T6-state AZ80 magnesium alloy matrix, and without damaging the original strength and plasticity obtained by forging and T6 heat treatment of the components. It is suitable for corrosion protection of lightweight forged load-bearing components such as vehicle cranks. Attached Figure Description
[0040] Figure 1The image shows an actual AZ80 magnesium alloy crankshaft and a temperature-time flow chart of the forging and T6 heat treatment processes.
[0041] Figure 2 EBSD inverse pole figure, grain diameter statistics, and pole figure of AZ80 magnesium alloy substrate;
[0042] Figure 3 To observe the Mg content in AZ80 magnesium alloy substrate using SEM and TEM 17 Al 12 Image of the second phase;
[0043] Figure 4 The tensile stress-strain curve of AZ80 magnesium alloy substrate;
[0044] Figure 5 This is a schematic diagram of the process flow of the ultrasonic shot peening hydrothermal corrosion protection method for AZ80 magnesium alloy of the present invention.
[0045] Figure 6 SEM images of the protective coating surface of AZ80-H and AZ80-SH samples and schematic diagram of Mg(OH)2 nanosheet growth.
[0046] Figure 7 The graph shows the statistical distribution of Mg(OH)2 nanosheet size and the bar chart of inter-sheet porosity.
[0047] Figure 8 SEM images of the protective coating section and surface distribution diagrams of Mg, O, and C elements;
[0048] Figure 9 FTIR spectra of the protective coating and XPS spectra of Mg 1s and O 1s;
[0049] Figure 10 This includes a macroscopic scratch morphology diagram and a scratch indentation depth curve.
[0050] Figure 11 EIS Nyquist plot, Bode plot, potentiodynamic polarization curve, and equivalent circuit diagram;
[0051] Figure 12 The cumulative hydrogen evolution curves of each sample after soaking in 5 wt.% NaCl solution for 250 h and macroscopic photographs after soaking are shown.
[0052] Figure 13 The α-Mg and Mg content in the AZ80 magnesium alloy matrix as measured by KPFM 17 Al 12 Voltaic potential difference diagram between the second phases;
[0053] Figure 14Three-dimensional contour map and corrosion depth line scan map after removal of corrosion products;
[0054] Figure 15 A schematic diagram of the corrosion protection mechanism of a bare AZ80 substrate sample that has undergone hydrothermal treatment without ultrasonic shot peening and a sample treated with the ultrasonic shot peening hydrothermal corrosion protection method of the present invention. Detailed Implementation
[0055] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0056] The specific implementation of the present invention will be described in detail below with reference to specific embodiments.
[0057] Example 1: This example provides a hydrothermal ultrasonic shot peening method for corrosion protection of AZ80 magnesium alloy, specifically including the following steps:
[0058] S1. A forged T6-state AZ80 magnesium alloy vehicle crankshaft is selected as the component to be processed. The preparation process of the forged T6-state AZ80 magnesium alloy component is as follows: the AZ80 magnesium alloy is preheated at 400 ℃ for 2 h and then forged; after forging, it is solution treated at 420 ℃, held for 2 h and then water quenched; subsequently, it is artificially aged at 180 ℃, held for 24 h and then air-cooled to obtain the forged T6-state AZ80 magnesium alloy component.
[0059] To characterize the room temperature mechanical properties of the forged T6 state AZ80 magnesium alloy substrate used in this embodiment, three parallel specimens were selected for room temperature tensile tests to measure their tensile yield strength, tensile strength, and elongation after fracture. The test results are shown in Table 1.
[0060] Table 1. Room temperature tensile properties of forged T6 AZ80 magnesium alloy substrates
[0061] sample Tensile yield strength (MPa) Tensile strength (MPa) Elongation after fracture (%) AZ80-1# 220 326 8.0 AZ80-2# 220 330 8.7 AZ80-3# 220 325 6.4
[0062] S2. The surface of the forged T6-state AZ80 magnesium alloy component to be treated is progressively polished using SiC sandpaper, ultrasonically cleaned with anhydrous ethanol, and dried with cold air. Subsequently, the surface to be treated is subjected to ultrasonic shot peening using 3 mm diameter zirconium oxide shot at an ultrasonic vibration frequency of 20 kHz for 20 minutes. During the treatment, the component is rotated periodically to ensure that the surface to be treated receives uniform impact from the shot.
[0063] After ultrasonic shot peening, the surface to be treated is not ground or polished. Instead, the component is ultrasonically cleaned with deionized water and anhydrous ethanol in sequence, and then dried with cold air to remove shot debris and contaminants, so that the surface plastic deformation defect layer formed by ultrasonic shot peening on the surface to be treated is retained.
[0064] S3. The component treated in step S2 is placed in a polytetrafluoroethylene-lined high-pressure reactor, and a 1 mol / L NaOH aqueous solution is added. The reactor is sealed, and hydrothermal treatment is performed at 125 °C for 6 h. After hydrothermal treatment, the component is allowed to cool naturally to room temperature. The component is then removed, rinsed sequentially with deionized water and anhydrous ethanol, and dried at 30 °C for 2 h. A protective coating with Mg(OH)2 as the main phase is formed in situ on the surface of the component to be treated, resulting in the AZ80-SH sample.
[0065] Comparative Example 1: This comparative example provides an AZ80-H sample that has undergone hydrothermal treatment directly without ultrasonic shot peening.
[0066] The forged T6 state AZ80 magnesium alloy component used in this comparative example, as well as its forging and T6 heat treatment processes, are exactly the same as those in Example 1. The surface of the component to be treated is progressively ground and polished using SiC sandpaper, and then cleaned with anhydrous ethanol. After cleaning, ultrasonic shot peening is not performed; instead, hydrothermal treatment, the same as step S3 in Example 1, is directly applied.
[0067] Specifically, the component was placed in a polytetrafluoroethylene-lined high-pressure reactor, and a 1 mol / L NaOH aqueous solution was added. The reactor was sealed and kept at 125 °C for 6 h. After the hydrothermal treatment, the component was allowed to cool naturally to room temperature, removed, and rinsed sequentially with deionized water and anhydrous ethanol. It was then dried at 30 °C for 2 h to obtain an AZ80-H sample that underwent hydrothermal treatment directly without ultrasonic shot peening.
[0068] Comparative Example 2: This comparative example provides a bare AZ80 substrate sample that has not undergone ultrasonic shot peening and hydrothermal treatment.
[0069] This comparative example uses the same forged T6-state AZ80 magnesium alloy component as in Example 1. The surface of the component to be treated was ground and cleaned, without ultrasonic shot peening or hydrothermal treatment, to obtain a bare AZ80 substrate sample.
[0070] Comparative Example 3: This comparative example provides an AZ80-SP-PH sample that underwent shot peening to remove the surface plastic deformation defect layer and then hydrothermal treatment, specifically including the following steps:
[0071] S1. The same forged T6 state AZ80 magnesium alloy bicycle crank as in Example 1 is used as the component to be processed. The forged T6 state AZ80 magnesium alloy bicycle crank belongs to the category of forged load-bearing components for vehicle cranks.
[0072] S2. The surface of the component to be treated is treated using the same ultrasonic shot peening process as in Example 1, that is, using zirconia shot with a diameter of 3 mm, ultrasonic vibration frequency of 20 kHz, and shot peening time of 20 min.
[0073] After ultrasonic shot peening, the surface to be treated is ground and polished step by step using SiC sandpaper to mechanically remove the surface plastic deformation defect layer formed by ultrasonic shot peening on the surface to be treated. Then the component is cleaned and dried.
[0074] S3. The same hydrothermal treatment process as in Example 1 was adopted, that is, the component was placed in a NaOH aqueous solution with a molar concentration of 1 mol / L, and hydrothermally treated at 125 °C for 6 h. After the hydrothermal treatment, the component was cooled, rinsed and dried to obtain the AZ80-SP-PH sample.
[0075] To evaluate the effect of different treatment methods on the corrosion resistance of forged T6-state AZ80 magnesium alloy, electrochemical impedance spectroscopy was performed on the bare AZ80 substrate sample, the AZ80-H sample obtained in Comparative Example 1, and the AZ80-SH sample obtained in Example 1. Figure 11 The equivalent circuit shown is used to fit the obtained electrochemical impedance spectrum, and the fitting parameters are shown in Table 2:
[0076] Table 2. EIS impedance spectral fitting parameters for AZ80, AZ80-H, and AZ80-SH samples.
[0077] parameter AZ80 AZ80-H AZ80-SH <![CDATA[ (Ω·cm 2 )]]> 15.58 44.53 <![CDATA[6.85×10 -7 ]]> <![CDATA[ (S·s n ·cm -2 )]]> <![CDATA[1.079×10 -5 ]]> <![CDATA[1.467×10 -5 ]]> <![CDATA[1.224×10 -7 ]]> 0.8711 0.6112 0.7451 <![CDATA[ (Ω·cm 2 )]]> 910 2605 67370 <![CDATA[ (S·s n ·cm -2 )]]> - <![CDATA[1.191×10 -5 ]]> <![CDATA[7.815×10 -6 ]]> - 0.7889 0.5759 <![CDATA[ (Ω·cm 2 )]]> - <![CDATA[4.64×10 5 ]]> <![CDATA[6.01×10 5 ]]> <![CDATA[ (Ω·cm 2 )]]> 2363 - - <![CDATA[L (H·cm 2 )]]> 369.6 - - <![CDATA[1.976×10 -3 ]]> <![CDATA[2.068×10 -3 ]]> <![CDATA[1.622×10 -3 ]]>
[0078] In Table 2, Indicates the resistance of the solution. Indicates a double-layer constant phase angle element. The index represents the constant phase angle of a double-layer element. Indicates charge transfer impedance, This indicates a constant phase angle element for the protective coating. The index of the constant phase angle element representing the protective coating. Indicates the resistance of the protective coating. Indicates the resistance of the inductive branch. Indicates inductance. This represents the fitting error.
[0079] As shown in Table 2, the charge transfer impedance Rct of the AZ80 bare substrate sample is 910 Ω·cm.2 The charge transfer impedance Rct of the AZ80-H sample obtained in Comparative Example 1 was 2605 Ω·cm. 2 The charge transfer impedance Rct of the AZ80-SH sample obtained in Example 1 reached 67370 Ω·cm. 2 The charge transfer impedance of the AZ80-SH sample was significantly higher than that of the bare AZ80 substrate sample and the AZ80-H sample, indicating that the protective coating formed by the method of the present invention can effectively inhibit charge transfer during the corrosion reaction process and improve the corrosion resistance of forged T6 state AZ80 magnesium alloy components.
[0080] The protective coating resistance Rf of the AZ80-SH sample is 6.01 × 10⁻⁶. 5 Ω·cm 2 The value is higher than that of the AZ80-H sample, which is 4.64 × 10⁻⁶. 5 Ω·cm 2 Meanwhile, the AZ80-SH sample The lower values of the AZ80 bare substrate sample and the AZ80-H sample indicate that the protective coating obtained by this invention has a better barrier effect and can reduce the effective contact between the electrolyte and the substrate interface. The values of each sample... All are at 10 -3 The magnitude indicates that the equivalent circuit used has a good fit with the electrochemical impedance spectroscopy test results.
[0081] To further evaluate the corrosion electrochemical behavior of each sample under different treatment methods, potentiodynamic polarization tests were performed on the AZ80 bare substrate sample, the AZ80-H sample obtained in Comparative Example 1, and the AZ80-SH sample obtained in Example 1. The obtained potentiodynamic polarization curves were fitted using Tafel fitting to obtain the corrosion potential. and corrosion current density The fitting results are shown in Table 3:
[0082] Table 3. Fitted corrosion electrochemical parameters of Tafel
[0083] sample (V relative to SCE) <![CDATA[ (A / cm 2 )]]> AZ80 -1.53 AZ80-H -1.34 AZ80-SH -1.38
[0084] Table 3 shows the corrosion current density of the AZ80 bare substrate sample. 1.21×10 -5 A / cm 2 The corrosion current density of the AZ80-H sample obtained in Comparative Example 1 Reduced to 8.95×10 -7 A / cm 2 The corrosion current density of the AZ80-SH sample obtained in Example 1 Further reduced to 2.86×10 -7 A / cm2 The corrosion current density of the AZ80-SH sample is approximately 1 / 42 of that of the bare AZ80 substrate sample and 1 / 3 of that of the AZ80-H sample, indicating that the protective coating obtained in this invention can significantly reduce the corrosion reaction rate of the forged T6 state AZ80 magnesium alloy substrate.
[0085] Corrosion potentials of AZ80 bare substrate specimens, AZ80-H specimens and AZ80-SH specimens The values were -1.53 V, -1.34 V, and -1.38 V, respectively. Compared with the bare AZ80 substrate sample, the corrosion potentials of both the AZ80-H and AZ80-SH samples showed a positive shift. Combined with the corrosion current density and electrochemical impedance spectroscopy test results, it can be seen that the AZ80-SH sample obtained in this invention has better corrosion protection performance.
[0086] To evaluate the microstructure and corrosion resistance of the protective coating obtained in this invention, and to further clarify the essential factors influencing the growth of the hydrothermal protective coating by ultrasonic shot peening, tests were conducted on the AZ80-SH sample obtained in Example 1, the AZ80-H sample obtained in Comparative Example 1, the AZ80 bare substrate sample obtained in Comparative Example 2, and the AZ80-SP-PH sample obtained in Comparative Example 3. The process, coating microstructure, and corrosion resistance test results for each sample are shown in Table 4.
[0087] Table 4. Test results of coating microstructure and corrosion resistance
[0088] Sample number Process Overview Average lateral size of nanosheets (nm) interlaminar porosity Coating thickness (μm) <![CDATA[Rct(Ω·cm 2 )]]> <![CDATA[250 h cumulative hydrogen evolution amount (mL / cm 2 )]]> Maximum corrosion depth (μm) Example 1 AZ80-SH Ultrasonic shot peening followed by cleaning and preservation of the surface plastic deformation defect layer → hydrothermal treatment 31.8 0.40% 8.7 67370 <0.5 50 Comparative Example 1 AZ80-H Raw polished substrate, without ultrasonic shot peening, directly hydrothermal treatment 51.7 2.30% 6.1 2605 4.7 160 Comparative Example 3 AZ80-SP-PH Ultrasonic shot peening → Grinding and polishing to remove the shot peening deformation layer → Same hydrothermal treatment 49.2 2.10% 6.3 2940 4.3 148 Comparative Example 2: AZ80 bare substrate Only grinding and cleaning were performed; ultrasonic shot peening and hydrothermal treatment were not carried out. - - - 910 12 1300
[0089] As shown in Table 4, the Mg(OH)₂ nanosheets of the AZ80-SP-PH sample obtained in Comparative Example 3 have an average lateral dimension of 49.2 nm, an inter-sheet porosity of 2.1%, and a protective coating thickness of 6.3 μm. These microstructural parameters of the coating are quite similar to those of the AZ80-H sample obtained in Comparative Example 1, which underwent hydrothermal treatment directly without ultrasonic shot peening; the AZ80-H sample has an average lateral dimension of 51.7 nm for the Mg(OH)₂ nanosheets, an inter-sheet porosity of 2.3%, and a protective coating thickness of 6.1 μm.
[0090] The charge transfer impedance Rct of the AZ80-SP-PH sample obtained in Comparative Example 3 was 2940 Ω·cm. 2 The cumulative hydrogen evolution amount after soaking in 5 wt.% NaCl solution for 250 h was 4.3 mL / cm³. 2 The maximum corrosion depth was 148 μm. Although its corrosion resistance was better than that of the AZ80 bare substrate sample obtained in Comparative Example 2, it was significantly lower than that of the AZ80-SH sample obtained in Example 1, and was at a similar level to that of the AZ80-H sample obtained in Comparative Example 1.
[0091] The above comparative results show that ultrasonic shot peening itself cannot directly achieve the microstructure control effect of the hydrothermal protective coating described in this invention. Only by retaining the high dislocation and surface plastic deformation defect layer on the surface of the component after ultrasonic shot peening can a large number of high-energy heterogeneous nucleation sites be provided for the subsequent hydrothermal reaction, thereby achieving the effects of refining Mg(OH)2 nanosheets, reducing inter-sheet porosity, and thickening the protective coating. Once the surface plastic deformation defect layer formed by ultrasonic shot peening is removed by grinding and polishing, the above-mentioned control effect basically disappears.
[0092] Therefore, the crystal defects induced and retained on the surface of the component to be treated by ultrasonic shot peening are the core factor in regulating the nucleation and growth kinetics of Mg(OH)2, rather than the surface roughness formed by ultrasonic shot peening or other secondary factors. This result further illustrates that the key to the coating microstructure regulation and corrosion resistance improvement effects of this invention lies in the continuous technical process of "ultrasonic shot peening to form a surface plastic deformation defect layer – without grinding or polishing – retaining the surface plastic deformation defect layer after cleaning – performing hydrothermal treatment."
[0093] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A method for ultrasonic shot peening and hydrothermal corrosion protection of AZ80 magnesium alloy, characterized in that, The method includes the following steps: The surface of the forged T6 state AZ80 magnesium alloy component to be treated is subjected to ultrasonic shot peening to form a surface plastic deformation defect layer on the surface to be treated. After ultrasonic shot peening, the surface to be treated is not ground or polished, but the component is cleaned so that the surface plastic deformation defect layer is retained on the surface to be treated. The component, after cleaning and retaining the surface plastic deformation defect layer, is placed in an aqueous sodium hydroxide solution for hydrothermal treatment, thereby forming a protective coating with Mg(OH)2 as the main phase in situ on the surface to be treated.
2. The ultrasonic shot peening hydrothermal corrosion protection method for AZ80 magnesium alloy according to claim 1, characterized in that, The ultrasonic shot peening process uses zirconia shot with a diameter of 2.5~3.5 mm, an ultrasonic vibration frequency of 18~22 kHz, and a shot peening time of 15~25 min.
3. The ultrasonic shot peening hydrothermal corrosion protection method for AZ80 magnesium alloy according to claim 1, characterized in that, After ultrasonic shot peening, the component is ultrasonically cleaned with deionized water and anhydrous ethanol in sequence, and then dried with cold air to remove shot fragments and contaminants.
4. The ultrasonic shot peening hydrothermal corrosion protection method for AZ80 magnesium alloy according to claim 1, characterized in that, The molar concentration of NaOH in the sodium hydroxide aqueous solution is 0.8~1.2 mol / L.
5. The ultrasonic shot peening hydrothermal corrosion protection method for AZ80 magnesium alloy according to claim 1, characterized in that, The hydrothermal treatment temperature is 115~135 ℃, and the holding time is 5~7 h.
6. The ultrasonic shot peening hydrothermal corrosion protection method for AZ80 magnesium alloy according to claim 1, characterized in that, Before the ultrasonic shot peening treatment, the surface to be treated was polished step by step with SiC sandpaper, and then ultrasonically cleaned with anhydrous ethanol and dried with cold air.
7. The ultrasonic shot peening hydrothermal corrosion protection method for AZ80 magnesium alloy according to claim 1, characterized in that, The AZ80 magnesium alloy comprises, by mass fraction, 7.8%~9.2% Al, 0.2%~0.8% Zn, and 0.15%~0.50% Mn, with the balance being Mg and unavoidable impurities.
8. An AZ80 magnesium alloy component, characterized in that, The component is a forged T6 state AZ80 magnesium alloy component obtained by ultrasonic shot peening and hydrothermal corrosion protection method according to any one of claims 1 to 7; the component includes a forged T6 state AZ80 magnesium alloy substrate and a protective coating formed in situ on the surface of the forged T6 state AZ80 magnesium alloy substrate, wherein the main phase of the protective coating is Mg(OH)2.
9. The AZ80 magnesium alloy component according to claim 8, characterized in that, The Mg(OH)2 in the protective coating is in the form of nanosheets.
10. The AZ80 magnesium alloy component according to claim 8, characterized in that, The component is a forged load-bearing component similar to a vehicle crank.