A production process for shortening the abnormal management period of a fully graphitized cathode aluminum electrolytic cell
By employing a fully graphitized cathode aluminum electrolytic cell production process, and through gradual adjustments to voltage, temperature, and molecular ratio, the problem of long abnormal management periods in aluminum electrolytic cells has been solved, achieving the effects of short high-voltage time, high production efficiency, and low energy consumption.
Patent Information
- Application Number
- CN202611263035.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, the abnormal management period of aluminum electrolytic cells is long, resulting in problems such as long high-voltage time, low production efficiency and high energy consumption.
The production process using a fully graphitized cathode aluminum electrolytic cell includes a plateau period, a rapid decay period, a slow decay period, and a transition period. By gradually adjusting the electrolytic cell voltage, cell temperature, molecular ratio, and fluoride salt addition, the abnormal management period is shortened.
It effectively shortens the abnormal management period, reduces the high voltage maintenance time of the electrolytic cell, improves production efficiency and reduces energy consumption, thereby enhancing the economic benefits of electrolytic production.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of aluminum electrolysis production processes, specifically to a production process for shortening the abnormal management period of a fully graphitized cathode aluminum electrolysis cell. Background Technology
[0002] After the electrolytic cell starts up, managing the abnormal period is an essential step in transitioning it to normal production and a crucial control point for stable and efficient production in the later stages. A well-defined furnace chamber is established under conditions such as high voltage, high cell temperature, high electrolyte level, and high molecular weight ratio. In the initial startup phase, the cell temperature, voltage, electrolyte level, and molecular weight ratio are significantly higher than normal values. Management measures are needed to control the rate of cooling and resistance reduction to prevent thermal shock that could cause lining cracking or aluminum melt seepage into the cathode. This period is also a critical window for the formation of the cell's internal shape. Preventing the formation of deformed furnace walls requires proactive intervention using effect coefficients and feeding strategies; otherwise, the electrolytic cell will experience low current efficiency in subsequent operation, significantly shortening its lifespan and increasing the cost per ton of aluminum.
[0003] Chinese invention patent application CN118727064A discloses a process control method for abnormal periods and a fully graphitized cathode aluminum electrolytic cell, relating to the field of aluminum electrolysis. The method includes: obtaining the current duration of the abnormal period in the fully graphitized cathode aluminum electrolytic cell; determining a process parameter control strategy for the time period corresponding to the duration of the abnormal period, wherein the process parameter control strategy includes a voltage control strategy, an electrolyte temperature control strategy, an aluminum melt level control strategy, an electrolyte level level control strategy, a molecular ratio control strategy, and an anode replacement control strategy; and controlling the production process of the fully graphitized cathode aluminum electrolytic cell based on the process parameter control strategy.
[0004] Currently, the typical duration of abnormal management periods is approximately 90-120 days. Maintaining high voltage and high cell temperature during these periods requires significant electrical energy consumption. Prolonged high voltage also delays the time it takes for the electrolytic cell to reach full-capacity, high-efficiency production, thus reducing the electrolytic aluminum production efficiency during abnormal management periods. Therefore, existing technologies for electrolytic cell production during abnormal management periods suffer from technical problems such as prolonged high-voltage periods, low production efficiency, and high energy consumption. Summary of the Invention
[0005] To address the aforementioned technical problems, the present invention aims to provide a production process for shortening the abnormal management period of a fully graphitized cathode aluminum electrolytic cell, which includes a plateau period, a rapid decay period, and a slow decay period. This production process for shortening the abnormal management period of a fully graphitized cathode aluminum electrolytic cell has the advantages of shorter high-voltage time, higher production efficiency, and lower energy consumption.
[0006] To achieve the above-mentioned objectives, the technical solution adopted by the present invention is as follows:
[0007] A production process for shortening the abnormal management period of a fully graphitized cathode aluminum electrolytic cell includes the following steps:
[0008] S1. Plateau period: After adding electrolyte to the electrolytic cell, adjust the electrolytic cell voltage to 4.7V. After the electrolytic cell temperature stabilizes at 975℃-985℃, add molten aluminum. Maintain the electrolytic cell voltage at 4.7V and the electrolyte molecular ratio at 2.9-3.0 until the second day after adding aluminum.
[0009] S2. Rapid decay period: The electrolytic cell voltage is reduced by 0.05V-0.1V per day, the electrolytic cell temperature is maintained at 975℃-985℃, and the electrolyte molecular ratio is maintained at 2.9-3.0, continuing until the 7th-8th day after aluminum filling, when the electrolytic cell voltage is reduced to 4.3V-4.1V.
[0010] S3. Slow decay period: The electrolytic cell voltage is reduced by 0.005V-0.03V per day, the electrolytic cell temperature is maintained at 975℃-985℃, and the electrolyte molecular ratio is maintained at 2.9-3.0. This continues until the 55th day after aluminum filling, when the electrolytic cell voltage is reduced to 3.9V.
[0011] Preferably, step S3 further includes the following step:
[0012] Fluoride salts were added after the electrolytic cell voltage dropped to 3.95V.
[0013] Preferably, step S3 further includes the following step:
[0014] Gradually increase the amount of fluoride added.
[0015] Preferably, step S3 further includes the following step:
[0016] The fluoride salt is made of aluminum fluoride.
[0017] Preferably, step S2 further includes the following step:
[0018] Eleven days after aluminum injection, electrolyte levels remained between 26 cm and 30 cm.
[0019] Preferably, step S3 further includes the following step:
[0020] On day 31 after aluminum filling, the electrolyte level was adjusted to 19-21 cm.
[0021] Preferably, after step S3, the following step is also included:
[0022] S4. Transition period: The electrolytic cell voltage is maintained at 3.9V, the electrolytic cell temperature is maintained at 955℃-975℃, the electrolyte molecular ratio is maintained at 2.5-2.6, the aluminum level is maintained at 18cm-20cm, and the electrolyte level is maintained at 19cm-21cm, continuing until the 90th day after aluminum is poured.
[0023] Preferably, after step S4, the following step is also included:
[0024] S5. Normal period: Increase the electrolytic cell voltage to 3.92V, maintain the electrolytic cell temperature at 955℃-965℃, maintain the electrolyte molecular ratio at 2.3-2.35, maintain the aluminum level at 18cm-20cm, and maintain the electrolyte level at 19cm-21cm.
[0025] Preferably, step S4 further includes the following step:
[0026] Gradually increase the amount of fluoride added.
[0027] Compared with the prior art, the present invention has achieved beneficial technical effects:
[0028] The initial voltage of the electrolytic cell during the plateau phase is only 4.7V, decreasing to 4.2V and 3.9V after rapid and slow decay periods, respectively. While maintaining the cell temperature and ensuring proper furnace wall formation, this process significantly reduces the high-voltage maintenance time compared to existing processes, effectively reducing unnecessary energy consumption and improving production efficiency. By gradually adding aluminum fluoride to smoothly reduce the molecular ratio, instability caused by large fluctuations in the molecular ratio is avoided. This ensures smooth furnace wall formation during the early stages of abnormal management and a stable transition to the normal production molecular ratio parameter range. A relatively stable transition production phase can be entered 55 days after aluminum filling, during which the electrolytic cell voltage is maintained at only 3.9V. At this point, the electrolytic cell already exhibits high electrical efficiency, further reducing overall energy consumption and effectively improving the economic benefits of aluminum electrolysis production. This achieves the advantages of shorter high-voltage time, higher production efficiency, and lower energy consumption. Detailed Implementation
[0029] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the embodiments. However, the scope of protection of this invention is not limited to the specific embodiments described below.
[0030] A production process for shortening the abnormal management period of a fully graphitized cathode aluminum electrolytic cell includes the following steps:
[0031] S1. Plateau period: When electrolyte is poured into the electrolytic cell, the voltage of the electrolytic cell is 5.3V; after electrolyte is poured into the electrolytic cell, molten aluminum is poured in, and the voltage of the electrolytic cell is gradually adjusted to 4.7V. After the temperature of the electrolytic cell stabilizes at 975℃-985℃, the voltage of the electrolytic cell is maintained at 4.7V, and the electrolyte molecular ratio is maintained at 2.9-3.0, which continues until the second day after aluminum is poured in.
[0032] S2. Rapid Decay Period: The electrolytic cell voltage is reduced by 0.05V-0.1V per day, the electrolytic cell temperature is maintained at 975℃-985℃, and the electrolyte molecular ratio is maintained at 2.9-3.0. This continues until the 7th-8th day after aluminum filling, when the electrolytic cell voltage is reduced to 4.2V. After the 11th day after aluminum filling, the electrolyte level is maintained at 26cm-30cm.
[0033] S3. Slow Decline Period: The electrolytic cell voltage is reduced by 0.005V-0.03V daily, the cell temperature is maintained at 975℃-985℃, and the electrolyte molecular ratio is maintained at 2.9-3.0, continuing until day 55 after aluminum filling, at which point the electrolytic cell voltage is reduced to 3.9V. Because it is a newly started electrolytic cell, the electrolyte molecular ratio is high, and the volatilization of aluminum fluoride is low, resulting in low fluorine loading in the alumina. Within 50 days of startup, the molecular ratio does not decrease, and the cell temperature remains at 975-985℃ until the set voltage drops below 3.95V, at which point the furnace lining thickness reaches approximately 18cm, forming a relatively good furnace lining. After the electrolytic cell voltage is reduced to 3.95V, the amount of fluoride salt added is gradually increased. Aluminum fluoride is used as the fluoride salt. On day 31 after aluminum filling, the electrolyte level is adjusted to 19cm-21cm.
[0034] S4. Transition period: The electrolytic cell voltage is maintained at 3.9V, the electrolytic cell temperature is maintained at 955℃-975℃, the electrolyte molecular ratio is maintained at 2.5-2.6, the aluminum level is maintained at 18cm-20cm, and the electrolyte level is maintained at 19cm-21cm. This continues until the 90th day after aluminum filling, and the amount of fluoride added is gradually increased until the amount of fluoride added meets the requirements of normal fluoride addition.
[0035] S5. Normal period: Increase the electrolytic cell voltage to 3.92V, maintain the electrolytic cell temperature at 955℃-965℃, maintain the electrolyte molecular ratio at 2.3-2.35, maintain the aluminum level at 18cm-20cm, and maintain the electrolyte level at 19cm-21cm.
[0036] The specific process flow is shown in Table 1.
[0037] Table 1. Production process flow chart for shortening the abnormal management period of a fully graphitized cathode aluminum electrolytic cell in this embodiment.
[0038]
[0039] This embodiment has the following advantages:
[0040] The initial voltage of the electrolytic cell during the plateau phase is only 4.7V, decreasing to 4.2V and 3.9V after rapid and slow decay periods, respectively. While maintaining the cell temperature and ensuring proper furnace wall formation, this process significantly reduces the high-voltage maintenance time compared to existing processes, effectively reducing unnecessary energy consumption and improving production efficiency. By gradually adding aluminum fluoride to smoothly reduce the molecular ratio, instability caused by large fluctuations in the molecular ratio is avoided. This ensures smooth furnace wall formation during the early stages of abnormal management and a stable transition to the normal production molecular ratio parameter range. A relatively stable transition period begins 55 days after aluminum is poured, during which the electrolytic cell voltage is maintained at only 3.9V. At this point, the electrolytic cell already exhibits high electrical efficiency, further reducing overall energy consumption and effectively improving the economic benefits of aluminum electrolysis production. This achieves the advantages of shorter high-voltage time, higher production efficiency, and lower energy consumption.
[0041] In traditional non-period management models, high voltage, high cell temperature, and high molecular weight ratios are required to form a robust and stable furnace wall. Therefore, in later management, the initial molecular weight ratio of the electrolytic cell is artificially increased through technical means. Later, aluminum fluoride needs to be added to reduce the molecular weight ratio to a normal and controllable range. Consequently, this adjustment transition period is relatively long, requiring three months to complete. After the production process of the fully graphitized cathode aluminum electrolytic cell shortens the non-period management period, newly started electrolytic cells possess the parameter characteristics for normal production in less than 60 days.
[0042] Taking a 350kA electrolytic cell as an example, the production process of shortening the abnormal management period by adopting this fully graphitized cathode aluminum electrolytic cell effectively reduces energy consumption in aluminum liquid production and lowers the financial cost per ton of aluminum produced. After the entire series of 280 units were started up, the direct electricity cost savings during the abnormal management period were approximately 7 million yuan. The current efficiency of the electrolytic cell was significantly improved, increasing benefits by approximately 6 million yuan, with a total increase in benefits of approximately 13 million yuan, and carbon emissions were reduced by approximately 6,000 tons. Moreover, this technology enables the electrolytic cell to establish a regular furnace, promoting efficient and stable operation after the electrolytic cell enters the normal production cycle. At the same time, it can be directly promoted and applied to other 420kA electrolytic cells, continuously achieving cost reduction and efficiency improvement.
[0043] Within 55 days after aluminum filling, the electrolytic cell temperature is maintained at 975-985℃. This ensures the electrolyte is superheated, maintains good fluidity, enhances its ability to dissolve alumina, and reduces sediment buildup at the bottom of the cell. It also helps dissolve alumina promptly, preventing a rapid drop in local concentration that could trigger the anodic effect. Simultaneously, it improves the electrolyte's conductivity, reduces resistance fluctuations between electrodes, increases the uniformity of current distribution, stabilizes partial discharge at the anolyte, and smooths the airflow and melt agitation within the cell, thereby reducing noise and vibration.
[0044] The plateau voltage is 4.7V, which, through the Joule effect, enhances the heat generation within the electrolytic cell, offsetting the heat loss caused by the large heat dissipation of the cell after aluminum pouring and the low heat capacity of the molten aluminum. This prevents the electrolyte from overcooling and solidifying, quickly establishing the stable thermal environment required after aluminum pouring. The higher voltage corresponds to a larger electrode gap, which weakens the molten aluminum surge caused by the unstable magnetofluid field after aluminum pouring, preventing short circuits caused by direct contact between the molten aluminum and the anode. This allows the newly poured molten aluminum to quickly form a base and ensures uniform current distribution. Sufficient electrode gap and heat allow the incomplete cell surface after aluminum pouring to quickly melt and flatten, promoting the initial formation of the furnace lining. This lays the foundation for gradually reducing the voltage and smoothly transitioning the cell conditions to the normal range over the following days.
[0045] During the rapid decay period, the electrolytic cell voltage is rapidly reduced, thereby rapidly reducing the heat input of the electrolytic cell and decreasing the superheat of the electrolyte. This allows cryolite solids to precipitate on the side of the electrolytic cell, forming a furnace wall and creating a regular and uniform furnace wall.
[0046] During the slow decay period, the excess heat gain in the electrolyzer has been reduced, and the overheating of the electrolyte has lessened. Therefore, the electrolyzer voltage is gradually reduced to near normal voltage. As the electrode spacing of the electrolyzer approaches its limit, adjustments need to be made slowly. Adjusting too quickly can cause problems such as unstable magnetofluid field, disruption of thermal balance, and excessive cooling of the electrolyzer.
[0047] Molecular ratio, cell temperature, aluminum level, and electrolyte level gradually return to normal during the transition period. The voltage bottoms out at 3.9V. When the technical conditions return to normal values, the voltage is appropriately increased to ensure that the electrolytic cell's magnetofluid field is stable, the electrode spacing is appropriate, and the thermal balance is stable.
[0048] Maintaining a high electrolyte molecular weight ratio of 2.9–3.0 during the slow decay period can significantly increase the electrolyte's freezing point and accelerate the solidification rate of the electrolyte crust on the side. The furnace lining crystal structure formed by the high molecular weight ratio solidification is dense, hard, and extremely resistant to electrolyte erosion. It can quickly form a uniform and complete protective furnace lining on the side of the electrolytic cell, completely avoiding the problems caused by the high-temperature electrolyte directly eroding the inner lining of the cell side when there is no formed furnace lining protection in the early stage, which leads to lining damage, furnace deformity, and increased risk of leakage. This lays the structural foundation for the subsequent fine and regularized furnace lining. Furthermore, during abnormal periods, the electrolytic cell system is not yet balanced, with significant fluctuations in cell temperature, material distribution, and electric field state. High-polymer ratio conditions can comprehensively optimize the electrolyte's overall performance: First, they significantly improve electrolyte fluidity, preventing low-temperature blockage and material accumulation, ensuring uniform electrolyte circulation within the cell; second, they significantly increase the alumina dissolution rate and saturation, eliminating alumina precipitation and furnace bottom crusting caused by uneven initial feeding, and avoiding frequent triggering of the anode effect; third, they improve electrolyte conductivity, reduce inter-electrode resistance and cell voltage fluctuations, stabilize the electric field distribution within the cell, effectively suppressing abnormal conditions such as initial flow deviation, aluminum rolling, and voltage fluctuations, and quickly achieving initial balance in the electrolytic cell production system.
[0049] Maintaining a high molecular weight ratio of 2.9–3.0, a dense and hardened sidewall is rapidly formed by the rapid precipitation of high-freezing-point electrolytes, constructing a protective layer for the furnace body. As the furnace lining continuously adsorbs sodium, the molecular weight ratio naturally decreases. When the lining approaches sodium saturation, the natural decrease in molecular weight ratio disappears, and a rebound occurs. After two rebounds, the molecular weight ratio is gradually and smoothly reduced by adding aluminum fluoride, achieving a gradient transition from 2.9–3.0 to 2.30. Gradually adding small amounts of aluminum fluoride avoids large fluctuations in the molecular weight ratio, achieving a smooth transition curve.
[0050] Comparative example:
[0051] The traditional production process flow during abnormal management periods is shown in Table 2.
[0052] Table 2 Production Process Flow Chart during Abnormal Management Period
[0053]
[0054] By comparing this comparative example with the production process for shortening the abnormal management period of a fully graphitized cathode aluminum electrolytic cell in this application, it can be seen that this process can shorten the abnormal management period of the graphite cathode aluminum electrolytic cell by 30 days compared with the traditional process, and can reduce the voltage to near the normal production range more than 40 days earlier. The molecular ratio also completes the transition to the normal production parameter range nearly 2 months earlier, significantly reducing the inefficient production time of high voltage and low power efficiency, and reducing the overall power consumption during the abnormal management period. This achieves a significant reduction in energy consumption per ton of aluminum and a significant improvement in current efficiency, thus achieving the effects of cost reduction, efficiency improvement, energy saving, and emission reduction.
[0055] Based on the disclosure and teachings of the foregoing specification, those skilled in the art can make changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some modifications and changes to the invention should also fall within the protection scope of the claims of the present invention. Furthermore, although some specific terms are used in this specification, these terms are only for convenience of explanation and do not constitute any limitation on the invention.
Claims
1. A production process for shortening the abnormal management period of a fully graphitized cathode aluminum electrolytic cell, characterized in that, Includes the following steps: S1. Plateau period: After adding electrolyte to the electrolytic cell, adjust the electrolytic cell voltage to 4.7V. After the electrolytic cell temperature stabilizes at 975℃-985℃, add molten aluminum. Maintain the electrolytic cell voltage at 4.7V and the electrolyte molecular ratio at 2.9-3.0 until the second day after adding aluminum. S2. Rapid decay period: The electrolytic cell voltage is reduced by 0.05V-0.1V per day, the electrolytic cell temperature is maintained at 975℃-985℃, and the electrolyte molecular ratio is maintained at 2.9-3.0, continuing until the 7th-8th day after aluminum filling, when the electrolytic cell voltage is reduced to 4.3V-4.1V. S3. Slow decay period: The electrolytic cell voltage is reduced by 0.005V-0.03V per day, the electrolytic cell temperature is maintained at 975℃-985℃, and the electrolyte molecular ratio is maintained at 2.9-3.
0. This continues until the 55th day after aluminum filling, when the electrolytic cell voltage is reduced to 3.9V.
2. The production process for shortening the abnormal management period of the fully graphitized cathode aluminum electrolytic cell according to claim 1, characterized in that, Step S3 further includes the following steps: Fluoride salts were added after the electrolytic cell voltage dropped to 3.95V.
3. The production process for shortening the abnormal management period of the fully graphitized cathode aluminum electrolytic cell according to claim 2, characterized in that, Step S3 further includes the following steps: Gradually increase the amount of fluoride added.
4. The production process for shortening the abnormal management period of the fully graphitized cathode aluminum electrolytic cell according to claim 2, characterized in that, Step S3 further includes the following steps: The fluoride salt is made of aluminum fluoride.
5. The production process for shortening the abnormal management period of the fully graphitized cathode aluminum electrolytic cell according to claim 1, characterized in that, Step S2 further includes the following steps: Eleven days after aluminum injection, electrolyte levels remained between 26 cm and 30 cm.
6. The production process for shortening the abnormal management period of the fully graphitized cathode aluminum electrolytic cell according to claim 5, characterized in that, Step S3 further includes the following steps: On day 31 after aluminum filling, the electrolyte level was adjusted to 19-21 cm.
7. The production process for shortening the abnormal management period of the fully graphitized cathode aluminum electrolytic cell according to claim 1, characterized in that, Following step S3, the following steps are also included: S4. Transition period: The electrolytic cell voltage is maintained at 3.9V, the electrolytic cell temperature is maintained at 955℃-975℃, the electrolyte molecular ratio is maintained at 2.5-2.6, the aluminum level is maintained at 18cm-20cm, and the electrolyte level is maintained at 19cm-21cm, continuing until the 90th day after aluminum is poured.
8. The production process for shortening the abnormal management period of the fully graphitized cathode aluminum electrolytic cell according to claim 7, characterized in that, Following step S4, the following steps are also included: S5. Normal period: Increase the electrolytic cell voltage to 3.92V, maintain the electrolytic cell temperature at 955℃-965℃, maintain the electrolyte molecular ratio at 2.3-2.35, maintain the aluminum level at 18cm-20cm, and maintain the electrolyte level at 19cm-21cm.
9. The production process for shortening the abnormal management period of the fully graphitized cathode aluminum electrolytic cell according to claim 7, characterized in that, Step S4 also includes the following steps: Gradually increase the amount of fluoride added.
Citation Information
Patent Citations
Abnormal-period process control method and fully-graphitized cathode aluminum electrolysis cell
CN118727064A