A method for surface electroplating of isolated conductive blocks
By using a rotating conductive brush for simultaneous electroplating and stripping, the problem of continuous and automated electroplating of isolated conductive blocks is solved, improving coating uniformity and production efficiency, simplifying the process and improving environmental and wastewater treatment.
Patent Information
- Application Number
- CN202611509894.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional electroplating methods require connecting conductive leads to each isolated conductive block, which is complex, inefficient, and difficult to achieve continuous and automated production. Furthermore, existing PCB surface treatment processes suffer from poor plating functionality, harsh production environments, and high difficulty in wastewater treatment.
The conductive brush bristles of the rotating conductive brush are in direct contact with the isolated conductive block to be plated. Through the synchronous electroplating and deplating design of the rotating conductive brush, continuous and automated electroplating of the conductive block is achieved. Hydrogen-resistant and highly elastic materials such as nickel-chromium alloy are used and coated with an insulating layer to ensure uniform current distribution and uniformity of the metal layer.
It simplifies the process, improves production efficiency, ensures uniform coating thickness and surface smoothness, reduces equipment maintenance frequency and wastewater treatment pressure, and enhances the cleanliness and safety of the working environment.
Smart Images

Figure CN123108679A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electroplating and coating technology, specifically a method for surface electroplating of isolated conductive blocks. Background Technology
[0002] In the field of electroplating, it is often necessary to electroplat a metal layer on the surface of isolated conductive blocks on insulating materials. Since the isolated conductive blocks are insulated from each other, the traditional method requires connecting conductive leads to each conductive block, then connecting them to the negative terminal of the power supply, immersing them in the plating solution, and electroplating them facing the anode. After electroplating, the leads need to be removed by mechanical cutting or chemical etching. This process is complex, inefficient, and costly, making it difficult to meet the needs of continuous and automated production.
[0003] Currently, approximately 99% of PCB final surface treatments utilize electroless tin plating, electroless silver plating, electroless nickel-gold plating, or other chemical plating processes. For example, Chinese invention patent application CN107058930A discloses a method for tin plating a thick PCB board, including steps such as router trimming the long edges of the thick PCB board, pre-plating baking, and tin plating. Another example of electroless tin plating is Chinese invention patent application CN109652828A, which discloses a PCB board tin plating-removal system and its application method. The copper-plated PCB board is tin-plated using a SnCl2-HCl solution system. After film stripping and circuit etching, the tin-plated board undergoes two-stage tin removal using SnCl4-HCl and H2SO4-Fe2(SO4)3 solution systems, respectively. The tin removal waste liquid is recycled via diaphragm electrowinning.
[0004] However, the above-mentioned tin-plating process has problems such as poor surface flatness, easy bridging / cold soldering of fine-pitch QFN / BGA / CSP, PCB board warping caused by high temperature of nearly 300℃, large difference in plating thickness (3-50μm), poor operating environment and safety hazards such as flammable flux; while chemical tin plating has problems such as thin tin layer (maximum only about 1.5μm), poor solderability after multiple reflows, easy to produce tin whiskers, easy to gray and discolor the surface, sensitive to the cleanliness of PCB copper surface, narrow process control window, high chemical cost and difficulty in wastewater treatment.
[0005] More importantly, for surface metallization of isolated conductive blocks on insulating materials (such as PCB copper pads), traditional electroplating methods require connecting conductive leads to each block because these blocks are insulated from each other. After electroplating, the leads must be removed by mechanical cutting or chemical etching. This process is complex, inefficient, and costly, making continuous and automated production difficult. While the aforementioned tin spraying and chemical plating processes can be used for PCB surface treatment, neither can directly perform continuous electroplating on isolated conductive blocks without laying conductive leads, and it is difficult to balance coating uniformity, solderability, and production efficiency. Summary of the Invention
[0006] The purpose of this invention is to provide a method for surface electroplating of isolated conductive blocks. By rotating the conductive brush and directly contacting the end of the conductive bristles of the conductive brush with the isolated conductive block to be plated, the current is conducted and electroplating and deplating are achieved simultaneously. This solves many problems of traditional electroplating, such as the need to connect and remove conductive leads, which leads to complex processes, low efficiency, poor functionality of the plating layer in existing PCB final surface treatment processes, harsh production environment, and high difficulty in wastewater treatment.
[0007] The objective of this invention can be achieved through the following technical solutions: A method for surface electroplating of an isolated conductive block includes the following steps: Step 1: Add electroplating solution to the long electroplating tank of the electroplating equipment, immerse the product to be plated with the isolated conductive block to be plated into the electroplating solution, and position the product to be plated in the middle of the A rotating conductive brush and the B rotating conductive brush, so that the conductive brush filaments are in elastic contact with the isolated conductive block to be plated, and the outer surface of the conductive brush filaments is covered with an insulating layer, with only the end exposed metal cross-section. Step 2: Start the electroplating equipment. The rotation direction of the A rotating conductive brush and the B rotating conductive brush is the same, both clockwise or counterclockwise. When the conductive brush bristles are on the side of the product to be plated, turn on the power. In the electroplating area of the rotating conductive brush, a constant current power supply is used, with the plating metal material as the electroplating anode and the end face of the conductive brush bristles contacting the isolated conductive block to be plated as the cathode, and surface electroplating is performed on the isolated conductive block to be plated. Step 3: After the conductive brush filaments brush over the product to be plated and rotate to the side away from the product to be plated, the constant voltage power supply is turned on. In the rotating conductive brush stripping area, the conductive brush filaments are used as anodes to electrolytically remove the plating layer at the end of the conductive brush filaments. Then, rotate to the side closer to the product to be plated, and simultaneously and continuously electroplate the surface of the product to be plated and remove the plating from the conductive brush filaments.
[0008] Furthermore, the conductive brush filaments of both the A and B rotary conductive brushes are made of either nickel-chromium alloy or nickel-titanium alloy.
[0009] Furthermore, the nickel-chromium alloy material is any one of NS3304, NS3308, and NS3405.
[0010] Furthermore, the density of the conductive brush filaments is 800-1200 filaments / cm². 2 The diameter of the conductive brush bristles is 0.05-0.2mm.
[0011] Furthermore, the diameter of the conductive brush bristles is 0.08-0.15 mm.
[0012] Furthermore, the length of the conductive brush bristles is 20-50mm, and the bending amount of the conductive brush bristles during operation is 0.5-5mm.
[0013] Furthermore, the length of the conductive brush bristles is 35-45mm.
[0014] Furthermore, the bending amount is 0.5-1mm when the length of the conductive brush bristle is 20mm, 1-2mm when the length is 30mm, 2-3mm when the length is 40mm, and 3-5mm when the length is 50mm.
[0015] Furthermore, the moving speed of the A rotating conductive brush and the B rotating conductive brush relative to the isolated conductive block to be plated is 20-50 m / min.
[0016] Furthermore, the morphology of the coated metal material is spherical, sheet-like, or rod-like.
[0017] Furthermore, for tin plating, the material of the electroplating anode is any one of soluble pure tin balls, tin plates, tin rods, or insoluble iridium-titanium and platinum-titanium anodes.
[0018] Furthermore, when the plating metal material is tin, the electroplating solution can be either a methanesulfonic acid system or a sulfuric acid system tin plating solution.
[0019] Furthermore, when the plating metal material is tin, the thickness of the electroplated coating on the surface is 2-15 μm.
[0020] Furthermore, the voltage of the constant voltage power supply is set to 0.5-5V.
[0021] The beneficial effects of this invention are: 1. This invention enables current conduction by having the cross-section of the conductive bristles at the end of a rotating conductive brush directly contact the isolated conductive block to be plated, eliminating the need for pre-laying conductive leads and subsequent removal processes, thus fundamentally simplifying the process. At the same time, the product to be plated is placed vertically on the center line of the electroplating tank, and the A rotating conductive brush and B rotating conductive brush operate synchronously. Combined with the continuous movement or fixed position of the product to be plated, continuous and automated electroplating of the surface of the isolated conductive block is achieved, greatly improving production efficiency.
[0022] In addition, by using a rotating conductive brush to continuously move and contact the plated surface, the conductive brush filaments are arranged at a certain density and a suitable bending pressure is applied, so that the current can be evenly conducted to each isolated conductive block, effectively avoiding the problem of uneven current distribution caused by traditional fixed-point electroplating or fixed contact.
[0023] The constant current power supply outputs a constant current based on the sum of the plated area and the cross-sectional area of the brush tip, ensuring a stable current density during the electroplating process. This results in a uniform plating thickness and a smooth, dense surface, further improving the consistency of the plating distribution across the entire board surface. In the PCB manufacturing industry, when this application is set as the final surface treatment electroplating tin process, it can effectively replace the traditional spray tin process, overcoming the defects of poor surface smoothness and large thickness differences in the traditional spray tin process. At the same time, the surface electroplating tin process can also replace traditional chemical plating processes such as chemical tin plating, chemical silver plating, and chemical nickel-gold plating.
[0024] 2. In this invention, the conductive brush bristles act as cathodes in the rotating conductive brush electroplating zone, simultaneously depositing metal with the plated product. They then rotate to the rotating conductive brush stripping zone, where a constant voltage power supply switches to anode, electrolytically stripping the deposited metal layer from their ends. The brushes then recycle back into the electroplating zone to continue operation. This simultaneous electroplating-stripping design ensures that the ends of the conductive brush bristles do not adhere to each other or form metal plates due to the accumulation and thickening of the metal layer, maintaining an independent bristle shape and good elastic contact capability. In constant voltage stripping mode, the current automatically drops to zero after the metal at the bristle end is completely stripped, effectively preventing excessive electrolytic corrosion of the conductive brush bristle body, thus significantly extending the brush bristle's service life and ensuring the stability of long-term continuous operation of the equipment.
[0025] 3. This invention uses hydrogen-resistant and highly elastic materials such as nickel-chromium alloy to make conductive brush filaments, and coats them with an insulating layer. Only the end cross-section is exposed to participate in conduction and deposition, which effectively reduces metal deposition and impurity generation in non-target areas. The synchronous deplating mechanism prevents metal particles at the brush tip from falling into the plating solution, maintaining the cleanliness of the electroplating solution, reducing the risk of plate surface contamination and hole blockage caused by suspended particles, lowering the frequency of plating solution maintenance and wastewater treatment pressure, and improving the cleanliness and safety of the working environment. Attached Figure Description
[0026] Figure 1 This is a photograph of the PCB (Printed Circuit Board) surface before electroplating, according to the present invention. Figure 2 This is a photograph of the PCB (Printed Circuit Board) after electroplating. Figure 3 This is a photograph of the PCB (Printed Circuit Board) after soldering testing. Figure 4 This is a photograph of the PCB (PCB board) being plated according to the present invention after an aging solder test. Figure 5 This is a cross-sectional schematic diagram of the long electroplating tank of the present invention; Figure 6 This is a top view schematic diagram of the long electroplating tank of the present invention.
[0027] Figure label: 1. Conductive brush bristles; 2. Conductive brush holder; 3. Electroplating anode; 4. Constant current power supply; 5. Constant voltage power supply; 6. Electroplating solution level; 7. Insulating substrate of the product to be plated; 8. Isolated conductive block to be plated; 9. Cathode conductive copper busbar; 10. Anode conductive copper busbar; 11. Rotating conductive brush electroplating area; 12. Rotating conductive brush stripping area; 13. Conductive slider. Detailed Implementation
[0028] To further illustrate the technical means and effects of the present invention in achieving the intended purpose, the following detailed description of the specific implementation methods, features and effects of the present invention, in conjunction with preferred embodiments, is provided below.
[0029] Example 1: This example provides a method for surface electroplating of an isolated conductive block, including the following steps: S1: As Figure 5 , Figure 6 As shown, rotating conductive brush A and rotating conductive brush B each consist of a conductive brush holder and conductive brush filaments. The conductive brush holder and conductive brush filaments are connected by welding. Both are made of NS3304 nickel-chromium alloy. The conductive brush holder is 5mm thick, and the conductive brush filaments are 0.1mm diameter NS3304 nickel-chromium alloy wires. The outer surface of the conductive brush filaments is coated with a 10μm thick polyimide (PI) insulating varnish. The conductive brush holder is insulated by covering it with adhesive. The conductive brush filaments are arranged on the conductive brush holder at a density of 2 filaments every 0.6mm in the X direction and 1 filament every 0.4mm in the Y direction, i.e., 200 filaments / 60mm in the X direction and 100 filaments / 40mm in the Y direction, with a density of 833 filaments / cm². 2 The conductive brush bristles are 20mm long. After the conductive brush bristles are cut, the cross-section is exposed. When this cross-section comes into contact with the isolated conductive blocks to be plated on the A and B surfaces of the product to be plated, the isolated conductive blocks are energized to achieve electroplating on the surface of the isolated conductive blocks.
[0030] S2: Preparation of the electroplating solution; a methanesulfonic acid system is used. The composition of the electroplating solution is as follows: stannous methanesulfonate concentration of 51 g / L, methanesulfonic acid concentration of 105 g / L, 2205L additive concentration of 20 mL / L, 2205L wetting agent concentration of 50 mL / L, and DYAN-A0 antioxidant concentration of 15 mL / L. The electroplating solution level is as follows: Figure 5 As shown, the electroplating anode uses pure tin balls.
[0031] S3: Will be as follows Figure 1 The product to be plated (PCB) shown is placed vertically on the center line of a long electroplating tank. The product to be plated can move unidirectionally along the vertical direction or remain stationary (Note: the direction of movement of the product to be plated is not limited, because rotating conductive brush A and rotating conductive brush B move in opposite directions on the two surfaces). Rotating conductive brush A and rotating conductive brush B are symmetrically arranged about the center line of the long electroplating tank as the axis of symmetry, so that surface A and surface B of the product to be plated correspond to rotating conductive brush A and rotating conductive brush B, respectively. This is a top view of the long electroplating tank. Figure 6As can be seen, both rotating conductive brush A and rotating conductive brush B rotate clockwise (or both rotate counterclockwise). This causes the conductive filaments of rotating conductive brush A and rotating conductive brush B to move in opposite directions on the surface of the sample to be plated. The product to be plated will not be stretched or deformed. At the same time, by controlling the bending amount of the conductive filaments, the conductive filaments apply appropriate pressure to the surface of the isolated conductive block to be plated: when the length of the conductive filaments is 20mm, the bending amount is 1mm, and the moving speed of rotating conductive brush A and rotating conductive brush B relative to the isolated conductive block to be plated is set to 40m / min.
[0032] S4: In the rotating conductive brush electroplating area, set the constant current power supply (electroplating power supply) to constant current mode. Based on the plating area of surface A and surface B of the product being plated, and the sum of the cross-sectional areas of all conductive brush tips in the electroplating area, calculate the total current (e.g., 11A) according to the recommended current density of the plating solution to ensure a stable current density on the surface of the product being plated. The voltage is automatically adjusted during the electroplating process. Start the equipment, and rotating conductive brush A and rotating conductive brush B contact the surfaces of surface A and surface B of the product being plated (PCB), respectively. The constant current power supply supplies power to the isolated conductive blocks to be plated on surface A and surface B of the product being plated through the cathode conductive copper busbar, conductive brush holder, and conductive brush filaments. The electroplating anode (i.e., the plating metal material) is a pure tin ball, so that each isolated conductive block to be plated is connected to the cathode. In the electroplating solution, the isolated conductive blocks to be plated on surface A and surface B of the product being plated, as well as the cross-sectional areas of the conductive brush tips immersed in the electroplating solution, are simultaneously deposited with a tin metal layer, realizing the electroplating of the isolated conductive block surface in the rotating conductive brush electroplating area. The electroplating time is controlled to be 9 minutes.
[0033] S5: Rotary conductive brushes A and B continue to operate. When the conductive brush filaments rotate with the conductive brush holder to the stripping area of the rotating conductive brush away from the product to be plated, the conductive brush holder contacts the anode conductive copper busbar through the conductive slider (which contacts different positive and negative terminals of the power supply in different areas to achieve anode-cathode interchange). The conductive brush filaments contact the anode conductive copper busbar through the conductive brush holder. The anode conductive copper busbar is connected to the positive terminal of the constant voltage power supply, and the negative terminal of the constant voltage power supply is connected to the electroplating anode. At this time, the end of the conductive brush filaments switches to the anode of the constant voltage power supply, which is set to 2V. The tin layer plated at the end of the conductive brush filaments is electrolytically etched and stripped in the electroplating solution. When the tin layer at the head of the conductive brush filaments is completely stripped, the current automatically drops to 0, thereby avoiding electrolytic corrosion of the conductive brush filaments. After stripping, the conductive brush filaments re-enter the rotating conductive brush electroplating area with the A and B rotating conductive brushes, repeating the cycle to achieve synchronous and continuous electroplating of the product to be plated and stripping of the conductive brush filaments.
[0034] The actual product after surface electroplating is shown in the image below. Figure 2 As shown.
[0035] Example 2: This example provides a method for surface electroplating of an isolated conductive block. The difference from Example 1 is that in step S1, the thickness of the conductive brush holder is 50 mm, the outer surface of the conductive brush filaments is coated with a 15 μm thick polyimide (PI) insulating varnish, and the density of the conductive brush filaments is 1000 filaments / cm². 2 .
[0036] Example 3: This example provides a method for surface electroplating of an isolated conductive block. The difference from Example 1 is that the length of the conductive brush bristles in step S1 is 50mm, and the distance between the surfaces of the plated product A and the plated product B and the conductive brush holder surfaces of the A and B rotating conductive brushes in step S3 is 45mm, respectively, with a bending amount of 5mm.
[0037] Example 4: This example provides a method for surface electroplating of an isolated conductive block. The difference from Example 1 is that the composition of the electroplating solution in step S2 is as follows: the concentration of stannous methanesulfonate is 53 g / L, the concentration of methanesulfonic acid is 109 g / L, the concentration of 2205L additive is 22 mL / L, the concentration of 2205L wetting agent is 54 mL / L, and the concentration of DYAN-A0 antioxidant is 17 mL / L (the electroplating tin additive solution is provided by Shenzhen Fulit Technology Co., Ltd.). The electroplating anode is a pure tin plate.
[0038] Example 5: This example provides a method for surface electroplating of an isolated conductive block. The difference from Example 1 is that in step S3, the moving speed of the rotating conductive brush A and the rotating conductive brush B relative to the isolated conductive block to be plated is set to 45 m / min.
[0039] Example 6: This example provides a method for surface electroplating of an isolated conductive block. The difference from Example 1 is that the electroplating time in step S4 is set to 11 minutes.
[0040] The electroplating anode used in the above embodiments is a pure tin ball, but a pure tin plate can also be used; Nickel balls or pure nickel plates can also be used as the anode for nickel plating.
[0041] Comparative Example 1: This comparative example provides a method for surface electroplating of an isolated conductive block, using a first-generation horizontal single-sided brush plating line.
[0042] Electroplating method: A toothed filament is etched on the edge of a 0.1mm titanium sheet to serve as a brush filament. The conductive brush holder is fixed in place. The electroplating anode is set only on one side of the B-side of the PCB to be plated and is directly opposite the B-side. DC power supply is used. The electroplating solution is the same tin plating solution of methanesulfonic acid system as in Example 1 (stannous methanesulfonate 51g / L, methanesulfonic acid 105g / L, 2205L additive 20mL / L, 2205L wetting agent 50mL / L, DYAN-A0 antioxidant 15mL / L). The product to be plated is a PCB with isolated copper pads exposed after the solder resist ink process. The single-sided brush plating time is 10min.
[0043] Performance tests were conducted on Examples 1-6 and Comparative Example 1. Test items included plating thickness (X-ray measurement) (referencing the Chinese National Standard GB / T 39807-2021 "Specification for Lead-Free Tin Plating and Tin Alloy Processes," which specifies a plating thickness of 1-30 μm), plating uniformity, solder resist ink integrity (no obvious scratches under 10x magnification), tin surface appearance (smooth, particle-free, uniformly white, no exposed copper, no particles blocking holes, etc.), solderability (tinning at 245℃ for 5 seconds, tinning area greater than 95%), brush condition, solution cleanliness, and plating defects. Solderability tests included tests on fresh boards and tests after aging at 155℃ for 4 hours. Test results are shown in Table 1. Figure 3 , Figure 4 As shown: Table 1 Performance Test Overview
[0044] As shown in Table 1, Examples 1-6 use NS3304 nickel-chromium alloy conductive brushes, a rotary synchronous stripping design, and a vertical double-sided brush plating structure. The resulting plating thickness is uniform, the solder resist ink is undamaged, the tin surface is smooth, and the solderability of both fresh and aged boards reaches 100%. Furthermore, the brushes maintain normal conductivity after long-term operation, and the solution is clean and free of particulate contamination.
[0045] In contrast, Comparative Example 1 uses a first-generation horizontal single-sided brush plating line and titanium metal brushes. Due to inherent defects of titanium brushes, such as poor coating adhesion, insufficient elasticity, hydrogen embrittlement fracture, improper anode arrangement, and inability to remove plating from the brushes, the coating is extremely thin and uneven, with serious missed plating, particle contamination on the board surface, broken and stuck brushes, and turbid solution. The solderability is far below the process requirements. The above comparison fully demonstrates that the improvements of this invention in the selection of conductive brush material, the rotary synchronous deplating mechanism, and the vertical double-sided electroplating structure significantly improve the quality, efficiency, and continuity of electroplating on the surface of isolated conductive blocks.
[0046] It should be noted that, in this document, terms such as “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0047] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention.
Claims
1. A method for surface electroplating of an isolated conductive block, characterized in that, Includes the following steps: Step 1: Add electroplating solution to the long electroplating tank of the electroplating equipment, immerse the product to be plated with the isolated conductive block to be plated into the electroplating solution, and position the product to be plated in the middle of the A rotating conductive brush and the B rotating conductive brush, so that the conductive brush filaments are in elastic contact with the isolated conductive block to be plated, and the outer surface of the conductive brush filaments is covered with an insulating layer, with only the end exposed metal cross-section. Step 2: Start the electroplating equipment. The rotation direction of the A rotating conductive brush and the B rotating conductive brush is the same, both clockwise or counterclockwise. When the conductive brush bristles are on the side of the product to be plated, turn on the power. In the electroplating area of the rotating conductive brush, a constant current power supply is used, with the plating metal material as the electroplating anode and the end face of the conductive brush bristles contacting the isolated conductive block to be plated as the cathode, and surface electroplating is performed on the isolated conductive block to be plated. Step 3: After the conductive brush filaments brush over the product to be plated and rotate to the side away from the product to be plated, the constant voltage power supply is turned on. In the rotating conductive brush stripping area, the conductive brush filaments are used as anodes to electrolytically remove the plating layer at the end of the conductive brush filaments. Then, rotate to the side closer to the product to be plated, and simultaneously and continuously electroplate the surface of the product to be plated and remove the plating from the conductive brush filaments.
2. The method for surface electroplating of an isolated conductive block according to claim 1, characterized in that, The conductive brush filaments of the A rotating conductive brush and the B rotating conductive brush mentioned in step one are made of either nickel-chromium alloy or nickel-titanium alloy. The density of the conductive brush filaments is 800-1200 filaments / cm². 2 The diameter of the conductive brush bristles is 0.05-0.2 mm.
3. The method for surface electroplating of an isolated conductive block according to claim 1, characterized in that, The length of the conductive brush bristles is 20-50mm, and the bending amount of the conductive brush bristles during operation is 0.5-5mm.
4. The method for surface electroplating of an isolated conductive block according to claim 3, characterized in that, The length of the conductive brush bristles is 35-45mm.
5. The method for surface electroplating of an isolated conductive block according to claim 3, characterized in that, The bending amount of the conductive brush filament is 0.5-1mm when the length is 20mm, 1-2mm when the length is 30mm, 2-3mm when the length is 40mm, and 3-5mm when the length is 50mm.
6. The method for surface electroplating of an isolated conductive block according to claim 1, characterized in that, In step two, the moving speed of the A rotating conductive brush and the B rotating conductive brush relative to the isolated conductive block to be plated is 20-50 m / min.
7. The method for surface electroplating of an isolated conductive block according to claim 1, characterized in that, The coating metal material described in step two is in the form of a sphere, sheet, or rod.
8. A method for surface electroplating of an isolated conductive block according to claim 1, characterized in that, When the plating metal material is tin, the electroplating solution is either a methanesulfonic acid system or a sulfuric acid system tin plating solution.
9. A method for surface electroplating of an isolated conductive block according to claim 1, characterized in that, When the plating metal material is tin, the thickness of the electroplated coating in step two is 2-15 μm.
10. A method for surface electroplating of an isolated conductive block according to claim 1, characterized in that, The voltage of the constant voltage power supply mentioned in step three is set to 0.5-5V.
Citation Information
Patent Citations
Thick printed circuit board (PCB) and solder coating method thereof
CN107058930A
PCB tin plating-tin stripping system and application method
CN109652828A