A method for preparing a modified coating for a PEM electrolytic cell bipolar plate and the resulting titanium alloy bipolar plate for the PEM electrolytic cell.

By preparing an indium tin oxide coating on the surface of a titanium alloy bipolar plate using molten salt electrodeposition, the problems of poor coating adhesion and preparation complexity were solved, achieving efficient and low-cost coating preparation and improving the service life and conductivity of the electrolytic cell.

CN123108688APending Publication Date: 2026-11-17SHANGHAI INSTITUTE OF APPLIED PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611380519.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, the coating of titanium alloy bipolar plates has poor adhesion to the substrate and is prone to peeling. The preparation of high-performance coatings depends on vacuum processes and cannot be carried out continuously, resulting in a shortened lifespan of the electrolytic cell and increased energy consumption.

Method used

A molten salt electrodeposition process was adopted, using NaCl and KCl as molten salt solvents and In2O3 and SnO2 as molten salt solutes, to prepare an indium tin oxide protective coating on the surface of a titanium alloy bipolar plate. By controlling the electrolysis temperature, current density and time, high adhesion between the coating and the substrate and continuous production were achieved.

Benefits of technology

It improves the adhesion between the coating and the substrate, reduces the risk of coating peeling, simplifies the preparation process, reduces processing costs, and improves the service life and conductivity of the electrolytic cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108688A_ABST
    Figure CN123108688A_ABST
Patent Text Reader

Abstract

This invention relates to a method for preparing a modified coating on a bipolar plate of a PEM electrolytic cell and the resulting titanium alloy bipolar plate for a PEM electrolytic cell. The method includes mixing a molten salt solvent and a molten salt solute to obtain a molten salt electrolyte; the molten salt solvent is prepared by mixing NaCl and KCl, and the molten salt solute is prepared by mixing In₂O₃ and SnO₂; the molten salt electrolyte is placed in an electrochemical deposition tank and heated; the bipolar plate workpiece to be treated is connected to the negative terminal of a power supply, and the counter electrode is connected to the positive terminal; molten salt electrodeposition is performed to prepare an indium tin oxide (ITO) protective coating on the workpiece surface; the electrodeposition workpiece is then removed, cleaned, and dried for later use. This invention uses molten salt electrodeposition to prepare the ITO protective coating, which promotes interdiffusion between the coating and the substrate elements, improves the coating adhesion, and reduces the risk of coating peeling during start-up and shutdown. This process does not require a vacuum environment, has the potential for continuous production, and is suitable for the use of bipolar plates in PEM electrolytic cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to surface coating preparation technology, and more specifically to a method for preparing a modified coating for a PEM electrolytic cell bipolar plate and the resulting titanium alloy bipolar plate for the PEM electrolytic cell. Background Technology

[0002] Proton exchange membrane electrolyzers (PEMWEs) are core equipment for efficient hydrogen production. Bipolar plates, as key components of the electrolyzer, play a crucial role in conducting current, distributing reactant gases, and supporting the membrane electrodes. Titanium alloys, due to their low initial resistivity, good thermal conductivity, low gas permeability, and excellent mechanical strength, are ideal candidate substrate materials for PEM water electrolyzer bipolar plates. However, the anode side of the electrolyzer operates in a highly corrosive environment, making the titanium alloy substrate prone to corrosion and degradation. Simultaneously, a high-resistivity oxide layer continuously forms on the substrate surface, significantly increasing the interfacial contact resistance (ICR) of the bipolar plates. This increases the energy consumption for hydrogen production through electrolysis, severely limiting the electrolyzer's efficiency and lifespan. Therefore, preparing a protective conductive coating on the surface of the titanium alloy bipolar plates is the mainstream technical approach to solving these problems.

[0003] Existing technologies have disclosed methods for surface protection of titanium alloy bipolar plates using TiN coatings. For example, CN202510359999.7 describes a method that prepares a TiN coating on the surface of a titanium alloy substrate, which can improve the substrate's corrosion resistance and conductivity to some extent. However, the adhesion between the coating prepared by this process and the titanium alloy substrate is poor. Under the actual operating conditions of frequent start-ups and shutdowns in PEM electrolytic cells, the coating is prone to peeling off and failure, significantly shortening the service life of the bipolar plates and even the entire electrolytic cell.

[0004] To improve coating adhesion, existing technologies have disclosed another bipolar plate coating preparation scheme, such as CN202311345827.1. First, the titanium-based bipolar plate is pretreated by ion nitriding to form a uniformly distributed first protective layer on the substrate surface, reconstructing the substrate surface morphology and microstructure. Then, a fine-grained and dense second protective layer is prepared using magnetron sputtering, thereby improving the preparation quality of the bipolar plate coating in the PEM electrolytic cell. However, this entire process needs to be completed under vacuum conditions, making continuous production of the workpiece impossible. The overall process is complex, with high equipment investment and processing costs, hindering large-scale industrial application. Summary of the Invention

[0005] To address the problems of poor adhesion between the coating and the substrate of titanium alloy bipolar plates in the existing technology, easy peeling, reliance on vacuum processes for high-performance coating preparation, complex processes, and inability to achieve continuous production, this invention aims to provide a method for preparing modified coatings for PEM electrolytic cell bipolar plates and the resulting PEM electrolytic cell titanium alloy bipolar plates.

[0006] The method for preparing a modified coating for a bipolar plate in a PEM electrolytic cell according to the present invention includes the following steps: S1, preparing a molten salt solvent and a molten salt solute, mixing the molten salt solvent and the molten salt solute to obtain a molten salt electrolyte; the molten salt solvent is prepared by mixing NaCl and KCl, and the molten salt solute is prepared by mixing In2O3 and SnO2; S2, placing the mixed molten salt electrolyte in an electrochemical deposition cell and heating it to a preset electrolysis temperature; connecting the bipolar plate workpiece to be treated to the negative terminal of the power supply and the counter electrode to the positive terminal of the power supply, and performing molten salt electrodeposition to prepare an indium tin oxide protective coating on the surface of the workpiece; S3, removing the workpiece after electrodeposition, cleaning and drying it for later use. This invention employs a molten salt electrodeposition process, using NaCl and KCl as molten salt solvents and In2O3 and SnO2 as molten salt solutes to construct a molten salt electrolyte system. This allows for the direct preparation of an indium tin oxide protective coating on the surface of a bipolar plate workpiece. This eliminates the reliance on vacuum coating equipment, enabling continuous production. Furthermore, it improves the adhesion between the coating and the substrate, reducing the risk of coating detachment during electrolytic cell start-up and shutdown.

[0007] In a preferred embodiment, the mass ratio of NaCl to KCl in the molten salt solvent is 1:1 to 9. By limiting the range of NaCl to KCl ratio within the molten salt solvent, this invention can obtain a molten salt system with stable physicochemical properties, ensuring a smooth electrodeposition process and providing a basic environment for the formation of a uniform indium tin oxide coating.

[0008] In a preferred embodiment, the mass ratio of In₂O₃ to SnO₂ in the molten salt solute is 5~10:1. By limiting the range of the In₂O₃ to SnO₂ ratio in the molten salt solute, this invention can control the composition of the precipitated indium tin oxide coating, ensuring that the coating possesses good electrical conductivity and corrosion resistance.

[0009] In a preferred embodiment, the electrodeposition temperature is 350°C to 750°C. By limiting the above-mentioned electrodeposition temperature range, the present invention can provide suitable reaction conditions for the molten salt system, promote elemental interdiffusion between the coating and the substrate, improve the coating adhesion, and at the same time avoid the problems of excessive molten salt volatilization due to excessively high temperature or insufficient molten salt melting due to excessively low temperature.

[0010] In a preferred embodiment, the current density is 0.01~0.2 A / dm². 2 By limiting the aforementioned current density range, this invention can control the deposition rate of indium tin oxide coatings, avoiding both excessive current causing coating powdering and insufficient current leading to low deposition efficiency.

[0011] In a preferred embodiment, the electrodeposition time is greater than 0 and does not exceed 300 seconds. By limiting the above-mentioned electrodeposition time range, the present invention can obtain an indium tin oxide protective coating of suitable thickness, balancing the coating's protective effect with processing efficiency, and avoiding the defects of insufficient protection due to excessively short deposition time and excessively thick coating that is prone to cracking.

[0012] In a preferred embodiment, the mass ratio of the molten salt solvent to the molten salt solute is 100:9~10. By limiting the ratio range of the molten salt solvent to the molten salt solute, the present invention can ensure that the solute is fully dispersed in the molten salt solvent, which is beneficial to forming a uniform indium tin oxide protective coating on the workpiece surface.

[0013] In a preferred embodiment, the bipolar plate workpiece is a titanium alloy bipolar plate. By selecting titanium alloy as the substrate for the bipolar plate workpiece, this invention enables the direct formation of an indium tin oxide protective coating with both conductive and corrosion-resistant capabilities on the surface of the titanium alloy substrate, specifically for PEM electrolytic cell conditions. This inhibits corrosion and degradation of the titanium alloy substrate and alleviates the problem of increased interfacial contact resistance.

[0014] According to the present invention, the titanium alloy bipolar plate for PEM electrolysis cell has an indium tin oxide protective coating on its surface prepared by the above-described method. The titanium alloy bipolar plate with an indium tin oxide protective coating prepared by the present invention can be directly adapted to the operating conditions inside a PEM electrolysis cell, while maintaining good conductivity and corrosion resistance.

[0015] In a preferred embodiment, the indium tin oxide protective coating on the surface of the titanium alloy bipolar plate has a resistivity of 3.9~9.3×10⁻⁶ at 25°C. -4 Ω·cm. By limiting the resistivity range of the coating, this invention can ensure that the bipolar plate has excellent conductivity and reduce the energy loss during the electrolysis process.

[0016] This invention employs a molten salt electrodeposition process to prepare an indium tin oxide (ITO) protective coating on the surface of a bipolar plate workpiece. This method eliminates the dependence on a vacuum preparation environment while ensuring a high bonding strength between the coating and the substrate, simplifying the overall preparation process and reducing processing costs. By combining the molten salt solvent and solute with the electrodeposition process parameters, an ITO protective coating with uniform composition and good conductivity can be obtained, effectively improving the corrosion resistance of the workpiece, reducing coating peeling and failure, and meeting the actual application requirements of bipolar plates in proton exchange membrane water electrolyzers. Attached Figure Description

[0017] Figure 1 This is a schematic flowchart of the method for preparing the modified coating of the bipolar plate in the PEM electrolytic cell according to Embodiment 1 of the present invention.

[0018] Figure 2This is a schematic flowchart of the method for preparing the modified coating of the bipolar plate in the PEM electrolytic cell according to Embodiment 2 of the present invention. Detailed Implementation

[0019] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0020] The following embodiments are merely illustrative examples, and some conventional process steps are not described in detail. Those skilled in the art can complete the corresponding operations based on common knowledge.

[0021] This invention provides a method for preparing a modified coating for a PEM electrolytic cell bipolar plate. The method uses molten salt electrodeposition to prepare an indium tin oxide (ITO) protective coating, which is used to prepare an ITO protective coating with both conductivity and corrosion resistance on the surface of a titanium alloy bipolar plate workpiece.

[0022] This invention employs molten salt electrodeposition technology. The process temperature conditions of the molten salt system can promote elemental interdiffusion between the coating and the substrate, significantly improving the adhesion between the coating and the substrate and reducing the risk of coating detachment under repeated start-up and shutdown conditions of the electrolytic cell. At the same time, this process does not require a vacuum environment and has the potential for continuous production.

[0023] The preparation method of the present invention first includes step S1: preparing molten salt solvent and molten salt solute, and mixing the molten salt solvent and molten salt solute to obtain molten salt electrolyte.

[0024] In a preferred embodiment, the molten salt solvent is obtained by mixing NaCl and KCl. In a preferred embodiment, the mass ratio of NaCl to KCl is 1:1 to 9. In a specific embodiment, the molten salt solvent is prepared by mixing equal masses of NaCl and KCl.

[0025] In a preferred embodiment, the molten salt solute is obtained by mixing In₂O₃ and SnO₂. In a preferred embodiment, the mass ratio of In₂O₃ to SnO₂ is 5~10:1. In a more preferred embodiment, the mass ratio of In₂O₃ to SnO₂ is 8~9:1.

[0026] In a preferred embodiment, the mass ratio of molten salt solvent to molten salt solute is 100:9~10.

[0027] The method of the present invention then includes step S2: placing the molten salt electrolyte after mixing in an electrochemical deposition tank, heating it to a preset electrolysis temperature, connecting the bipolar plate workpiece to be treated to the negative terminal of the power supply, connecting the counter electrode to the positive terminal of the power supply, and performing electrodeposition by applying current to prepare an ITO protective coating on the surface of the workpiece.

[0028] In a preferred embodiment, the electrodeposition process is carried out at a temperature of 350°C to 750°C. In a more preferred embodiment, the electrodeposition temperature is 500°C to 560°C.

[0029] In a preferred embodiment, the current density during the electrodeposition process is 0.01~0.2 A / dm³. 2 In a more preferred embodiment, the current density is 0.1~0.2 A / dm³. 2 .

[0030] In a preferred embodiment, the electrodeposition time is set to be greater than 0 and not more than 300 seconds. In a more preferred embodiment, the electrodeposition time is 100-120 seconds.

[0031] The method of the present invention then includes step S3: taking out the workpiece after electrodeposition, cleaning and drying it for later use, and conducting subsequent performance tests.

[0032] In a preferred embodiment, after cleaning the workpiece, the coating-related performance indicators are tested.

[0033] Example 1

[0034] See Figure 1 The following steps were performed sequentially: S101 molten salt electrolyte solution preparation, S102 molten salt electrodeposition treatment, and S103 sample cleaning and performance testing.

[0035] Step S101: Prepare a molten salt electrolyte solution with a molten salt solvent: molten salt solute ratio of 100:10 (unless otherwise specified, all ratios are by mass); wherein, molten salt solvent: 1000g, wherein NaCl:KCl = 1:1; molten salt solute: 100g, wherein In2O3:SnO2 = 9:1.

[0036] Step S102: Place the above molten salt electrolyte solution in an alumina crucible, connect the negative terminal of the power supply to the pre-plated workpiece, and connect the positive terminal of the power supply to the graphite rod, both of which are placed in the crucible; the temperature is preset to 560℃, the power supply is turned on, and the current is adjusted to a current density of 0.1A / dm³. 2 The electroplating process takes 120 seconds to complete the preparation of the protective coating.

[0037] Step S103: Remove the workpiece after electrodeposition, clean the sample, dry it, and then perform performance testing.

[0038] The coating prepared in this embodiment has a thickness of approximately 2.5 micrometers. The coating exhibits good adhesion to the substrate, with no porosity defects, and a resistivity of 3.9 × 10⁻⁶ at 25°C. -4 The coating has good electrical conductivity (Ω·cm).

[0039] Example 2

[0040] See Figure 2 The following steps were performed sequentially: S201 molten salt electrolyte solution preparation, S202 molten salt electrodeposition treatment, and S203 sample cleaning and performance testing.

[0041] Step S201: Prepare a molten salt electrolyte solution with a molten salt solvent: molten salt solute ratio of 100:9 (unless otherwise specified, all ratios are by mass); wherein, molten salt solvent: 1000g, wherein NaCl:KCl = 1:1; molten salt solute: 90g, wherein In2O3:SnO2 = 8:1.

[0042] Step S202: Place the above molten salt electrolyte solution in an alumina crucible, connect the negative terminal of the power supply to the pre-plated workpiece, and connect the positive terminal of the power supply to the graphite rod, both of which are placed in the crucible; the temperature is preset to 500℃, the power supply is turned on, and the current is adjusted to a current density of 0.2A / dm³. 2 Electroplating time is 100 seconds to complete the preparation of the protective coating.

[0043] Step S203: Remove the workpiece, clean it, dry it, and wait for performance testing.

[0044] The coating prepared in this embodiment has a thickness of approximately 3.8 micrometers. The coating exhibits good adhesion to the substrate, with no porosity defects, and a resistivity of 9.3 × 10⁻⁶ at 25°C. -4 Ω·cm.

[0045] Comparison table of sample performance from different implementation cases:

[0046] Implementation Cases Thickness / micrometer Coating adhesion to substrate <![CDATA[Resistivity / ×10 -4 Ω·cm]]> Case 1 2.5 good 3.9 Case 2 3.8 good 9.3

[0047] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of the invention. Various variations can be made to the above embodiments of the present invention. That is, all simple and equivalent changes and modifications made based on the claims and description of this invention fall within the protection scope of the claims. All aspects not described in detail in this invention are conventional technical content.

Claims

1. A method for producing a modified coating for PEM electrolyser bipolar plates, characterized in that, Includes the following steps: S1. Prepare molten salt solvent and molten salt solute by mixing the molten salt solvent and the molten salt solute to obtain molten salt electrolyte; the molten salt solvent is prepared by mixing NaCl and KCl, and the molten salt solute is prepared by mixing In2O3 and SnO2; S2. Place the mixed molten salt electrolyte in an electrochemical deposition tank and heat it to the preset electrolysis temperature. Connect the bipolar plate workpiece to be treated to the negative terminal of the power supply and the counter electrode to the positive terminal of the power supply. Apply current to perform molten salt electrodeposition and prepare an indium tin oxide protective coating on the surface of the workpiece. S3. Remove the workpiece after electrodeposition, clean and dry it for later use.

2. The method for producing a modified coating for bipolar plates of PEM electrolysis cells according to claim 1, characterized in that, The mass ratio of NaCl to KCl in the molten salt solvent is 1:1 to 9.

3. The method for preparing a modified coating for a PEM electrolytic cell bipolar plate according to claim 1, characterized in that, The mass ratio of In2O3 to SnO2 in the molten salt solute is 5~10:

1.

4. The method for preparing a modified coating for a PEM electrolytic cell bipolar plate according to claim 1, characterized in that, The electrodeposition temperature is 350℃~750℃.

5. The method for preparing a modified coating for a PEM electrolytic cell bipolar plate according to claim 1, characterized in that, The current density is 0.01 to 0.2 A / dm 2 .

6. The method for preparing a modified coating for a PEM electrolytic cell bipolar plate according to claim 1, characterized in that, The electrodeposition time is greater than 0 and does not exceed 300 seconds.

7. The method for preparing a modified coating for a PEM electrolytic cell bipolar plate according to claim 1, characterized in that, The mass ratio of the molten salt solvent to the molten salt solute is 100:9~10.

8. The method for preparing a modified coating for a PEM electrolytic cell bipolar plate according to claim 1, characterized in that, The bipolar plate workpiece is a titanium alloy bipolar plate.

9. A titanium alloy bipolar plate for a PEM electrolytic cell, characterized in that, The indium tin oxide protective coating on the surface of the titanium alloy bipolar plate is prepared by the preparation method described in any one of claims 1 to 8.

10. The titanium alloy bipolar plate for the PEM electrolytic cell according to claim 9, characterized in that, The indium tin oxide protective coating of the titanium alloy bipolar plate surface has a resistivity of 3.9-9.3x10 -4 Ω·cm at 25°C.

Citation Information

Patent Citations

  • PEM electrolytic cell bipolar plate high-conductivity strong-corrosion-resistant coating and preparation method thereof

    CN117305878A

  • Preparation method of titanium nitride-based coating for surface of anode titanium-based bipolar plate of PEM electrolytic cell

    CN119932612A