A manufacturing process for aluminum alloy casings used in power batteries for new energy vehicles

By controlling the composition of the aluminum alloy matrix and optimizing the stamping process, combined with low-temperature annealing and sealing treatment, the problems of micropores and cracks after micro-arc oxidation of aluminum alloy shells were solved, thereby improving their corrosion resistance and fatigue resistance.

CN123108696APending Publication Date: 2026-11-17FUAOXIN INNOVATIVE ENERGY BATTERY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611360128.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Micro-arc oxidation treatment of aluminum alloy casings used in existing new energy vehicle power batteries results in micropores and cracks, leading to a decrease in corrosion resistance and fatigue resistance.

Method used

By controlling the composition of the aluminum alloy matrix, optimizing the stamping process parameters, and performing low-temperature annealing and sealing treatment after micro-arc oxidation, a dense ceramic film layer is formed, reducing micropores and cracks.

Benefits of technology

It improves the corrosion resistance and fatigue resistance of the aluminum alloy shell, and ensures the uniformity and adhesion of the film layer.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of lithium batteries, specifically to a manufacturing process for aluminum alloy casings used in power batteries for new energy vehicles. The process includes: first, stamping high-quality aluminum alloy sheet; second, stress-relief annealing; third, micro-arc oxidation; and fourth, sealing treatment to obtain the finished product. Starting with the composition design of the casing blank, this invention uses aluminum-scandium alloy as the raw material for high-quality aluminum alloy sheet, and combines adjustments to the stamping and micro-arc oxidation processes to improve the corrosion resistance and fatigue resistance of the aluminum alloy casing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium batteries, specifically to a manufacturing process for an aluminum alloy casing for power batteries used in new energy vehicles. Background Technology

[0002] The aluminum alloy casing for power batteries in new energy vehicles is one of the core components, and its quality directly affects the battery's safety, heat dissipation performance, and lifespan. Currently, aluminum alloy casings are typically manufactured using a stamping process, followed by micro-arc oxidation surface treatment to improve their corrosion resistance. Micro-arc oxidation treatment can generate a ceramic film layer mainly composed of alumina on the aluminum alloy surface in situ. This film layer has a metallurgical bond with the substrate, exhibiting strong adhesion and effectively improving the surface hardness and corrosion resistance of the casing.

[0003] However, the ceramic film surface after micro-arc oxidation treatment contains numerous micropores and cracks due to residual discharge. These micropores and cracks act as channels for corrosive media to penetrate into the aluminum alloy substrate, reducing the corrosion resistance of the film. Furthermore, the microscopic defects of micropores and microcracks, along with residual stress, can become crack initiation points, leading to premature crack initiation and propagation, ultimately impairing the fatigue performance of the aluminum alloy shell.

[0004] CN107755578A discloses a stamping method for aluminum battery cases of new energy vehicles. The method involves steps such as material selection, film application, chamfering, die application, stamping, and shaping to achieve the stamping of the aluminum battery case. It primarily addresses forming problems such as cracking, wrinkling, and springback during the cold stamping process of aluminum alloys. CN107326422A discloses a method for preparing a composite insulating layer on the surface of an aluminum alloy battery casing. The method comprises the following steps: Step 1: Cleaning the surface of the aluminum alloy battery casing with a cleaning agent to remove oil stains, completing the pretreatment of the aluminum alloy battery casing surface; Step 2: Preparing a micro-arc oxidation ceramic layer on the surface of the aluminum alloy battery casing obtained after the pretreatment in Step 1; Step 3: Mixing polymethylphenyl silicone resin with anhydrous ethanol to obtain a silicone resin spraying liquid, and using the silicone resin spraying liquid to spray and cure the micro-arc oxidation ceramic layer obtained in Step 2, thus preparing a composite insulating layer on the aluminum alloy battery casing. The properties of a material are determined by its composition and process. Although the above-mentioned technologies can cover up micropores and cracks to a certain extent, they have not been able to reduce the problems caused by the decline in fatigue resistance due to micropore and crack defects in the micro-arc oxide film. Summary of the Invention

[0005] To address the aforementioned problems, this invention provides a manufacturing process for aluminum alloy casings used in power batteries for new energy vehicles. By designing the composition of the casing blank and adjusting the stamping and micro-arc oxidation processes, the corrosion resistance and fatigue resistance of the aluminum alloy casing are improved.

[0006] In a first aspect, the present invention provides a manufacturing process for an aluminum alloy casing for a power battery in a new energy vehicle, comprising the following steps: Step 1, high-quality aluminum alloy sheet stamping: Using high-quality aluminum alloy sheet as raw material, the high-quality aluminum alloy sheet is processed into a shell blank through a stamping process. The chemical composition of the high-quality aluminum alloy sheet, by mass percentage, is Mg 1.8%-2.2%, Mn 0.05%-0.10%, Cr 0.10%-0.20%, Cu ≤0.05%, Si ≤0.10%, Fe ≤0.20%, Zn ≤0.05%, Ti 0.05%-0.10%, Sc 0.05%-0.10%, other impurity elements ≤0.03% individually and ≤0.10% in total, with the balance being Al; The second step is stress-relief annealing: the shell blank is kept at a temperature of 300℃-360℃ for 1-2 hours, followed by air cooling; The third step, micro-arc oxidation: After surface cleaning, the stress-relief annealed shell blank is placed in an electrolyte for micro-arc oxidation treatment to obtain a semi-finished product; the voltage of the micro-arc oxidation treatment is AC 350V-450V, and the current density is 15A / dm³. 2 -20A / dm 2 The frequency is 100Hz-200Hz, the duty cycle is 10%-30%, the processing time is 20min-30min, and the electrolyte temperature is 20℃-40℃. The fourth step is sealing treatment: the semi-finished product is annealed at low temperature, then immersed in a sealing agent for sealing treatment, and after drying and curing, the finished product is obtained.

[0007] Preferably, the stamping process includes blanking, drawing, trimming, flanging and punching. The blanking gap of the stamping process is 6%-8% of the thickness of the high-quality aluminum alloy sheet, the stamping speed is ≤60mm / s, and the blank holder force is 20t-40t.

[0008] Preferably, the thickness of the high-quality aluminum alloy sheet is 0.6mm-2.5mm.

[0009] Preferably, the surface cleaning is performed using an air blowing method.

[0010] Preferably, the electrolyte is prepared as follows: sodium hexametaphosphate is added to water and stirred until completely dissolved to obtain a primary solution; sodium silicate is added to the primary solution and stirred until completely dissolved to obtain a secondary solution; sodium tungstate is added to the secondary solution and stirred until completely dissolved to obtain the electrolyte; the pH of the electrolyte is adjusted to 9-12; the mass concentration of sodium silicate in the electrolyte is 5 g / L-15 g / L, the mass concentration of sodium hexametaphosphate is 5 g / L-15 g / L, and the mass concentration of sodium tungstate is 1 g / L-3 g / L. Sodium tungstate is used to provide a tungsten source, forming a tungsten-containing compound in the film layer, thereby improving the corrosion resistance of the film layer.

[0011] Preferably, the sealing agent comprises a bottom sealing agent and an outer sealing agent, and the fourth sealing process includes: first immersing the semi-finished product in the bottom sealing agent, taking it out and drying it to form a bottom sealing layer; then immersing it in the outer sealing agent, taking it out and drying and curing it to form an outer sealing layer.

[0012] Further, as a preferred embodiment, the bottom sealing agent comprises, by mass percentage, 10%-30% aluminum dihydrogen phosphate, 10%-30% silica sol, and 40%-80% deionized water. The impregnation time of the bottom sealing agent is 1 min-5 min, and after impregnation, it is dried at 80℃-120℃ for 10 min-20 min. The outer sealing agent is an epoxy resin solution, which comprises epoxy resin and a curing agent. The mass ratio of epoxy resin to curing agent is 5-3:1. The impregnation time of the outer sealing agent is 10 min-15 min, and after impregnation, it is cured at 60-80℃ for 30 min-60 min.

[0013] Preferably, the sealing agent is an epoxy resin solution, which contains epoxy resin and a curing agent, with a mass ratio of epoxy resin to curing agent of 5-3:1. The fourth step of sealing treatment includes: first immersing the semi-finished product in the sealing agent, then removing it and drying and curing it, with an immersion time of 10-20 minutes, and then curing it at 60-80℃ for 30-60 minutes after immersion.

[0014] Preferably, the low-temperature annealing process involves holding the semi-finished product at 150℃-250℃ for 1-2 hours, followed by air cooling. This temperature is lower than the recrystallization temperature of the aluminum alloy, so it will not affect the mechanical properties of the substrate, but it can provide sufficient activation energy to partially release the stress concentration at the interface between the micro-arc oxide film and the substrate.

[0015] Secondly, the present invention provides an aluminum alloy casing for a power battery of a new energy vehicle, which is prepared according to the manufacturing process described in any embodiment of the first aspect.

[0016] Micro-arc oxidation is a process of in-situ generation of ceramic films on an aluminum alloy substrate. The substrate is the source of raw materials for film growth; therefore, different elements in the substrate participate in or interfere with the reaction during micro-arc oxidation discharge, directly affecting the composition, structure, and density of the film. For example, scandium forms nano-Al3Sc in the substrate, which has a pinning effect on relative dislocations and grain boundaries, which is beneficial to the uniformity of discharge during micro-arc oxidation, making the generated ceramic film denser and synergistically improving the corrosion resistance of the shell. When the silicon content in the substrate increases, the average growth rate of the film decreases and the number of discharge channels increases. Copper exists in the aluminum alloy in the form of second phases such as Al2Cu, which will be preferentially oxidized into the film during micro-arc oxidation discharge, resulting in a decrease in corrosion resistance. Iron enters the film during discharge, forming iron-containing oxide phases. These phases have a large difference in thermal expansion coefficients with the alumina substrate, generating thermal stress during cooling, leading to a porous film. This invention controls silicon to below 0.10%, copper to below 0.05%, and iron to below 0.20%, reducing the conditions for film defect formation at the substrate level. Furthermore, during the stamping process, the blanking gap, stamping speed, and blank holder force jointly determine the surface quality and residual stress state of the shell blank. For example, if the blanking gap is too large, the cross-sectional collapse angle and burrs increase. Burrs become preferential discharge sites during micro-arc oxidation, causing abnormal local film growth. If the gap is too small, the cross-sectional work hardening is severe, and the reactivity in this area differs from other areas, resulting in uneven film thickness. When the stamping speed is too fast, scratches and aluminum adhesion are easily generated on the surface, becoming preferential discharge sites during micro-arc oxidation, causing local film abnormalities. Even an inappropriate blank holder force can lead to increased surface roughness and decreased film uniformity. After the micro-arc oxidation process, residual stress exists at the interface between the film and the substrate. This invention incorporates a low-temperature annealing step before sealing, holding the semi-finished product at 150℃-250℃ for 1-2 hours. This temperature is below the recrystallization temperature of aluminum alloys and will not affect the strength of the matrix, but it is sufficient to provide the activation energy required for atomic diffusion, so that the stress concentration at the interface can be partially released.

[0017] There is a logical progression among the various processes in this invention: substrate composition control reduces the conditions for the formation of micropores and cracks in the film; stamping process control ensures the surface quality and low residual stress state of the shell blank, providing a uniform substrate surface for micro-arc oxidation; optimized electrical parameters ensure the dense structure and suitable phase composition of the film; low-temperature annealing eliminates residual stress in the film; and sealing treatment fills the remaining micropore defects, ultimately ensuring the quality of the finished product.

[0018] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention starts with controlling the composition of the aluminum alloy matrix, controlling the silicon content to below 0.10%, the copper content to below 0.05%, and the iron content to below 0.20%, thereby reducing harmful elements in the matrix that hinder the formation of micro-arc oxidation films. This reduces the tendency of micropores and cracks in the micro-arc oxidation film layer from the source, and improves the density and corrosion resistance of the film layer.

[0019] 2. By controlling the blanking gap, stamping speed and blank holder force in the stamping process, this invention obtains a shell blank with good surface quality, reduces the risk that surface defects such as scratches and draw marks will become preferential discharge sites during micro-arc oxidation, and ensures the uniformity of film thickness.

[0020] 3. The present invention includes a low-temperature annealing step after micro-arc oxidation and before sealing treatment, which involves holding the micro-arc oxidation film at 150℃-250℃ for 1-2 hours to release residual stress at the interface between the micro-arc oxidation film and the substrate. This temperature is lower than the recrystallization temperature of aluminum alloy and does not affect the mechanical properties of the substrate.

[0021] 4. This invention optimizes the micro-arc oxidation process by controlling the composition of the aluminum alloy matrix and the stamping process, thereby reducing micropores and cracks in the micro-arc oxidation film and improving the corrosion resistance and fatigue performance of the shell. Detailed Implementation

[0022] It should be noted that, unless otherwise specified, the embodiments and features described in this invention can be combined with each other. The described embodiments are merely some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without inventive effort should fall within the scope of protection of this invention. Example 1

[0023] This embodiment provides a manufacturing process for aluminum alloy casings used in power batteries for new energy vehicles, specifically including the following steps: The first step is high-quality aluminum alloy sheet stamping: The selected high-quality aluminum alloy sheet has the following chemical composition by mass percentage: Mg 1.9%, Mn 0.08%, Cr 0.15%, Cu 0.03%, Si 0.08%, Fe 0.18%, Zn 0.03%, Ti 0.08%, Sc 0.07%, with other impurity elements individually ≤0.03% and the total of other impurities ≤0.10%, with the balance being Al. The thickness of the high-quality aluminum alloy sheet is 1.2mm.

[0024] High-quality aluminum alloy sheets are processed into shell blanks through a stamping process. The stamping process includes blanking, drawing, trimming, flanging, and punching, which are performed sequentially to form a complete shell blank shape. The blanking clearance in the stamping process is controlled to be 7% of the thickness of the high-quality aluminum alloy sheet, i.e., 0.084 mm, the stamping speed is controlled to be 50 mm / s, and the blank holder force is controlled to be 30 t.

[0025] The second step is stress-relief annealing: the shell blank is placed in an annealing furnace and held at 330°C for 1.5 hours, and then air-cooled to room temperature to eliminate residual stress generated during the stamping process.

[0026] The third step, micro-arc oxidation: the stress-relief annealed shell blank is cleaned by blowing air to remove surface impurities and oil. The electrolyte was prepared as follows: sodium hexametaphosphate was added to water and stirred until completely dissolved to obtain a primary solution; sodium silicate was added to the primary solution and stirred until completely dissolved to obtain a secondary solution; sodium tungstate was added to the secondary solution and stirred until completely dissolved to obtain the electrolyte. The pH of the electrolyte was adjusted to 10.5. The mass concentrations of sodium silicate, sodium hexametaphosphate, and sodium tungstate in the electrolyte were 10 g / L, 10 g / L, and 2 g / L, respectively. The shell blank was placed in an electrolyte for micro-arc oxidation treatment. The voltage of the micro-arc oxidation treatment was AC 400V, and the current density was 18A / dm³. 2 The frequency was 150Hz, the duty cycle was 20%, the processing time was 25min, and the electrolyte temperature was controlled at 30℃.

[0027] The fourth step is sealing: First, low-temperature annealing is performed, where the semi-finished product is held at 200℃ for 1.5 hours, followed by air cooling to partially release the stress concentration at the interface between the micro-arc oxide film and the substrate. Then, sealing is performed using a double-layer structure of a bottom sealing agent and an outer sealing agent. The bottom sealing agent contains 20% aluminum dihydrogen phosphate, 20% silica sol, and 60% deionized water by weight percentage. The semi-finished product is immersed in the bottom sealing agent for 3 minutes, then removed and dried at 100℃ for 15 minutes to form the bottom sealing layer.

[0028] The outer sealing agent is an epoxy resin solution. The mass ratio of epoxy resin (E-51) to curing agent (T31) is 4:1. The semi-finished product is immersed in the outer sealing agent for 12 minutes. After being removed, it is cured at 70°C for 45 minutes to form the outer sealing layer and obtain the finished product. Example 2

[0029] The only difference between this embodiment and Embodiment 1 is that the chemical composition and thickness of the high-quality aluminum alloy sheet are different, and the process parameters for stamping and micro-arc oxidation are adjusted: Specifically, in this embodiment, the chemical composition of the high-quality aluminum alloy sheet, by mass percentage, is: Mg 2.0%, Mn 0.06%, Cr 0.12%, Cu 0.04%, Si 0.06%, Fe 0.15%, Zn 0.04%, Ti 0.07%, Sc 0.05%, with other impurity elements individually ≤0.03% and the total of other impurity elements ≤0.10%, and the balance being Al. The thickness of the high-quality aluminum alloy sheet is 1.8 mm.

[0030] The blanking clearance of the stamping process is controlled at 6% of the thickness of the high-quality aluminum alloy sheet, the stamping speed is controlled at 45mm / s, and the blank holder force is controlled at 25t.

[0031] The voltage for micro-arc oxidation treatment is 380V AC, and the current density is 16A / dm³. 2 The frequency was 120Hz, the duty cycle was 15%, the processing time was 28min, and the electrolyte temperature was controlled at 35℃.

[0032] The other process steps are the same as in Example 1. Example 3

[0033] The only difference between this embodiment and Embodiment 1 is that in this embodiment, a single layer of epoxy resin sealing agent is used for the sealing process: After low-temperature annealing, the semi-finished product is immersed in a sealing agent, which is an epoxy resin solution. The mass ratio of epoxy resin (E-51) to curing agent (T31) is 5:1. The immersion time is 15 minutes. After removal, it is cured at 65°C for 50 minutes to obtain the finished product.

[0034] The other process steps are the same as in Example 1. Example 4

[0035] The only difference between this embodiment and Embodiment 1 is that the electrolyte formulation and the electrical parameters of the micro-arc oxidation treatment are adjusted in this embodiment: In this embodiment, the electrolyte contains sodium silicate at a mass concentration of 8 g / L, sodium hexametaphosphate at a mass concentration of 12 g / L, sodium tungstate at a mass concentration of 2.5 g / L, and the pH of the electrolyte is adjusted to 11.

[0036] The voltage for micro-arc oxidation was 420V AC, and the current density was 19A / dm³. 2 The frequency was 180Hz, the duty cycle was 25%, the processing time was 22min, and the electrolyte temperature was controlled at 25℃.

[0037] The other process steps are the same as in Example 1. Example 5

[0038] The only difference between this embodiment and Embodiment 1 is that the thickness of the high-quality aluminum alloy sheet, the stamping process parameters, and the electrical parameters of the micro-arc oxidation treatment are different in this embodiment: In this embodiment, the thickness of the high-quality aluminum alloy sheet is 2.2 mm. The blanking clearance of the stamping process is controlled to be 8% of the thickness of the high-quality aluminum alloy sheet, the stamping speed is controlled to be 55 mm / s, and the blank holder force is controlled to be 35 t. The voltage for micro-arc oxidation treatment is 450V AC, and the current density is 20A / dm³. 2 The frequency was 200Hz, the duty cycle was 30%, the processing time was 20min, and the electrolyte temperature was controlled at 40℃.

[0039] The other process steps are the same as in Example 1.

[0040] Comparative Example 1 The only difference from Example 1 is that 5052-H32 aluminum alloy was used, with the following composition: Mg 2.5%, Cr 0.25%, Cu 0.05%, Si 0.15%, Fe 0.25%, Mn 0.05%, Zn 0.05%, other impurity elements ≤0.05% individually and ≤0.15% in total, with the balance being aluminum.

[0041] The other process steps are the same as in Example 1.

[0042] Comparative Example 2 The only difference from Example 1 is that the blanking gap is controlled to be 10% of the thickness of the high-quality aluminum alloy sheet, the stamping speed is controlled to be 80 mm / s, and the blank holder force is controlled to be 15t.

[0043] The other process steps are the same as in Example 1.

[0044] Comparative Example 3 The only difference from Example 1 is that the low-temperature annealing step was not included in this comparative example; the sealing process was performed directly.

[0045] The other process steps are the same as in Example 1.

[0046] Comparative Example 4 The only difference from Example 1 is that no sealing treatment was performed in this comparative example.

[0047] The other process steps are the same as in Example 1.

[0048] Comparative Example 5 The only difference from Example 1 is that the electrolyte formulation in this comparative example does not contain sodium tungstate.

[0049] The other process steps are the same as in Example 1.

[0050] Comparative Example 6 The only difference from Example 1 is that the electrolyte preparation method is different in this comparative example, specifically: sodium silicate, sodium hexametaphosphate and sodium tungstate are added and stirred at the same time.

[0051] The other process steps are the same as in Example 1.

[0052] Comparative Example 7 The only difference from Example 1 is the electrical parameters of the micro-arc oxidation treatment in this comparative example: the voltage is AC 500V and the current density is 25A / dm³. 2 The frequency is 300Hz, the duty cycle is 50%, and the processing time is 40min.

[0053] The other process steps are the same as in Example 1.

[0054] Comparative Example 8 The only difference from Example 1 is that the low-temperature annealing temperature is different in this comparative example. Specifically, the semi-finished product is kept at 330°C for 1 hour and then air-cooled.

[0055] The other process steps are the same as in Example 1.

[0056] The aluminum alloy shells prepared in Examples 1-5 and Comparative Examples 1-8 were subjected to performance tests, including: Corrosion resistance, refer to GB / T 10125-2021 "Artificial Atmosphere Corrosion Test - Salt Spray Test"; For fatigue resistance, refer to GB / T 3075-2021 "Methods for controlling axial force in fatigue testing of metallic materials"; The adhesion of the micro-arc oxidation film and the sealing agent film shall be determined with reference to GB / T 9286-2021 "Cross-cut test for paints and varnishes".

[0057] The results are shown in Table 1.

[0058] Table 1. Test results of the examples and comparative examples. serial number Time to corrosion spots appear in salt spray test / h Fatigue life / weeks Adhesion rating Example 1 720 125000 Level 0 Example 2 680 112000 Level 0 Example 3 660 108000 Level 0 Example 4 750 132000 Level 0 Example 5 700 118000 Level 0 Comparative Example 1 460 72000 Level 1 Comparative Example 2 420 86000 Level 1 Comparative Example 3 650 72000 Level 0 Comparative Example 4 340 110000 / Comparative Example 5 480 105000 Level 1 Comparative Example 6 640 98000 Level 1 Comparative Example 7 380 56000 Level 3 Comparative Example 8 670 63000 Level 0 As shown in Table 1, the indicators of Examples 1 to 5 are significantly better than those of the comparative example. The time to corrosion points in the salt spray test for all examples exceeded 660 hours, the fatigue life exceeded 100,000 cycles, and the adhesion grade was 0 for all. Within the examples, there were some fluctuations in the indicators under different combinations of process parameters, but overall they remained at a high level, indicating that the component range and process parameter window defined by this invention have good adaptability. Furthermore, Example 3 shows that the single-layer sealing agent still exhibits good anti-corrosion effect.

[0059] Comparative Example 1 used 5052-H32 aluminum alloy sheet, whose silicon, copper, and iron contents were all higher than the limits specified in this invention, resulting in corrosion resistance and fatigue resistance far inferior to Examples 1-5. Comparative Example 2 had a larger blanking gap, faster stamping speed, and lower blank holder force, leading to decreased film uniformity, thinner films in some areas, or structural defects. Corrosive media could more easily penetrate into the substrate from these weak areas, resulting in a shorter time to corrosion points in the salt spray test compared to the examples. Comparative Example 3 did not include a low-temperature annealing step; after micro-arc oxidation, residual stress at the film-substrate interface resulted in a significantly shorter fatigue life than the examples. Comparative Example 4 lacked sealing treatment, leaving numerous discharge micropores. These micropores penetrated the film to reach the substrate, serving as channels for corrosive media penetration and significantly shortening the time to corrosion points in the salt spray test. In Comparative Example 5, the electrolyte lacked sodium tungstate, resulting in decreased film density and a shorter time to corrosion points in the salt spray test compared to the Example. However, the impact of sodium tungstate on film density was less than the impact of the silicon, copper, and iron content in the substrate, thus the salt spray test results were still higher than those of Comparative Example 1. In Comparative Example 6, the electrolyte preparation order was incorrect. Sodium hexametaphosphate dissolved slowly in water, and the addition of sodium silicate made the solution viscous, hindering dispersion and leading to uneven distribution of components in the electrolyte. This resulted in unstable discharge behavior during micro-arc oxidation and uneven local film structure, although the overall impact was relatively small. In Comparative Example 7, excessively high voltage led to excessive discharge energy and frequency, resulting in excessively rapid film growth and heat accumulation causing localized overheating. The film obtained through micro-arc oxidation became rough and porous, with numerous micropores and large cracks. Corrosive media could easily penetrate the substrate through these defects, significantly shortening the time to corrosion points in the salt spray test. The porous nature of the film obtained through micro-arc oxidation reduced adhesion. The low-temperature annealing temperature of Comparative Example 8 was increased to 330℃, which is close to the recrystallization temperature of aluminum alloy. Holding at this temperature will cause the matrix grains to grow and the strength to decrease. The reduction in the mechanical properties of the matrix is ​​directly reflected in the significant decrease in fatigue life.

[0060] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A manufacturing process for an aluminum alloy casing for a power battery in a new energy vehicle, characterized in that, Includes the following steps: Step 1, high-quality aluminum alloy sheet stamping: Using high-quality aluminum alloy sheet as raw material, the high-quality aluminum alloy sheet is processed into a shell blank through a stamping process. The chemical composition of the high-quality aluminum alloy sheet, by mass percentage, is Mg 1.8%-2.2%, Mn 0.05%-0.10%, Cr 0.10%-0.20%, Cu ≤0.05%, Si ≤0.10%, Fe≤0.20%, Zn ≤0.05%, Ti 0.05%-0.10%, Sc 0.05%-0.10%, other impurity elements ≤0.03% individually and ≤0.10% in total, with the balance being Al; The second step is stress-relief annealing: the shell blank is kept at a temperature of 300℃-360℃ for 1-2 hours, followed by air cooling; The third step, micro-arc oxidation: After surface cleaning, the stress-relief annealed shell blank is placed in an electrolyte for micro-arc oxidation treatment to obtain a semi-finished product; the voltage of the micro-arc oxidation treatment is AC 350V-450V, and the current density is 15A / dm³. 2 -20A / dm 2 The frequency is 100Hz-200Hz, the duty cycle is 10%-30%, the processing time is 20min-30min, and the electrolyte temperature is 20℃-40℃. The fourth step is sealing treatment: the semi-finished product is annealed at low temperature, then immersed in a sealing agent for sealing treatment, and after drying and curing, the finished product is obtained.

2. The manufacturing process for the aluminum alloy casing of a power battery for new energy vehicles according to claim 1, characterized in that, The stamping process includes blanking, drawing, trimming, flanging and punching. The blanking gap of the stamping process is 6%-8% of the thickness of the high-quality aluminum alloy sheet, the stamping speed is ≤60mm / s, and the blank holder force is 20t-40t.

3. The manufacturing process for the aluminum alloy casing of a power battery for new energy vehicles according to claim 1, characterized in that, The thickness of the high-quality aluminum alloy sheet is 0.6mm-2.5mm.

4. The manufacturing process for the aluminum alloy casing of a power battery for new energy vehicles according to claim 1, characterized in that, The surface was cleaned using an air blowing method.

5. The manufacturing process for the aluminum alloy casing of a power battery for new energy vehicles according to claim 1, characterized in that, The electrolyte is prepared by adding sodium hexametaphosphate to water and stirring until completely dissolved to obtain a primary solution; then adding sodium silicate to the primary solution and stirring until completely dissolved to obtain a secondary solution. Sodium tungstate is added to the secondary solution and stirred until completely dissolved to obtain an electrolyte. The pH of the electrolyte is adjusted to 9-12. The mass concentration of sodium silicate in the electrolyte is 5 g / L-15 g / L, the mass concentration of sodium hexametaphosphate is 5 g / L-15 g / L, and the mass concentration of sodium tungstate is 1 g / L-3 g / L.

6. The manufacturing process for the aluminum alloy casing of a power battery for new energy vehicles according to claim 1, characterized in that, The sealing agent comprises a bottom sealing agent and an outer sealing agent. The fourth sealing process includes: first, immersing the semi-finished product in the bottom sealing agent, taking it out and drying it to form a bottom sealing layer; then immersing it in the outer sealing agent, taking it out and drying and curing it to form an outer sealing layer.

7. The manufacturing process for the aluminum alloy casing of a power battery for new energy vehicles according to claim 6, characterized in that, The bottom sealing agent comprises, by mass percentage, 10%-30% aluminum dihydrogen phosphate, 10%-30% silica sol, and 40%-80% deionized water. The impregnation time of the bottom sealing agent is 1-5 minutes, followed by drying at 80-120°C for 10-20 minutes. The outer sealing agent is an epoxy resin solution comprising epoxy resin and a curing agent, with a mass ratio of epoxy resin to curing agent of 5-3:

1. The impregnation time of the outer sealing agent is 10-15 minutes, followed by curing at 60-80°C for 30-60 minutes.

8. The manufacturing process for the aluminum alloy casing of a power battery for new energy vehicles according to claim 1, characterized in that, The sealing agent is an epoxy resin solution, which contains epoxy resin and a curing agent. The mass ratio of epoxy resin to curing agent is 5-3:

1. The fourth step of sealing treatment includes: first, immersing the semi-finished product in the sealing agent, then taking it out and drying and curing it. The immersion time is 10-20 minutes, and after immersion, curing is carried out at 60-80℃ for 30-60 minutes.

9. The manufacturing process for the aluminum alloy casing of a power battery for new energy vehicles according to claim 1, characterized in that, The low-temperature annealing process is as follows: the semi-finished product is kept at a temperature of 150℃-250℃ for 1-2 hours, and then air-cooled.

10. An aluminum alloy casing for a power battery in a new energy vehicle, characterized in that, It is prepared according to any one of the production processes described in claims 1-9.

Citation Information

Patent Citations

  • Method for preparing composite insulation layer on surface of aluminum alloy battery shell

    CN107326422A

  • Punching method of new energy vehicle battery aluminum box

    CN107755578A