Single crystal silicon rods and their crystal pulling process

By optimizing the thermal field structure of the 0-degree guide tube and the pulling process parameters, the problems of high oxygen content, unstable temperature and safety in the production of large-size monocrystalline silicon rods were solved, and stable and efficient monocrystalline silicon rod production was achieved.

CN123108723APending Publication Date: 2026-11-17YIBIN YINGFA DEKUN TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611590396.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the production of large-size monocrystalline silicon rods, high oxygen content leads to concentric circle defects, production capacity loss, and safety hazards. Existing flow guide tube solutions cannot simultaneously solve the problems of high oxygen content, unstable temperature, and safety.

Method used

A 0-degree guide tube is adopted, combined with an improved thermal field structure, crystal rotation speed, crucible rotation speed, inert gas flow rate and furnace pressure control during the pulling process, and optimized distance between cooling medium and silicon liquid and height of water cooling screen, to adapt to the airflow characteristics of the 0-degree guide thermal field.

Benefits of technology

It effectively reduces oxygen content, minimizes crystal rod shaking and diameter fluctuations, improves production stability and yield, avoids rod breakage and drop accidents, and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108723A_ABST
    Figure CN123108723A_ABST
Patent Text Reader

Abstract

This disclosure relates to the field of monocrystalline silicon rod preparation technology, specifically to monocrystalline silicon rods and their crystal pulling process. The process employs 0-degree flow guidance for Czochralski-pulled monocrystalline silicon rod pulling; it increases the distance between the cooling medium and the molten silicon, and the length of the inert gas flow path within the water-cooled screen; and optimizes crystal rotation, crucible rotation, inert gas flow rate, and furnace pressure to adapt the crystal pulling process to the airflow characteristics of the 0-degree flow guidance thermal field. This solves problems such as uneven melt temperature, rod shaking, rod breakage, and large diameter fluctuations under 0-degree flow guidance conditions, thereby improving the production stability and yield of monocrystalline silicon rods.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of single-crystal silicon rod preparation technology, and more specifically, to single-crystal silicon rods and their crystal pulling process. Background Technology

[0002] With the rapid development of the photovoltaic and semiconductor industries, market competition is becoming increasingly fierce, and the trend of industry "involution" is intensifying. In pursuit of higher conversion efficiency and lower levelized cost of electricity (LCOE), market demand for large-size monocrystalline silicon rods continues to rise. However, a key technical bottleneck is commonly encountered in the production process of large-size monocrystalline silicon rods: the oxygen content in the rods is significantly higher than that of traditional small-size rods. Increased oxygen content can lead to defects such as oxygen precipitation and thermal donors, and may cause problems such as concentric circles on silicon wafers, severely affecting the conversion efficiency and product yield of solar cells. Therefore, effectively reducing the oxygen content in large-size monocrystalline silicon rods has become crucial for improving product quality and meeting the high standards demanded by the market.

[0003] In principle, there are two main ways to reduce the oxygen content of monocrystalline silicon rods: First, to inhibit oxygen generation at the source, such as reducing the reaction between the quartz crucible and the silicon melt; second, to enhance the exhaust efficiency of silicon monoxide gas by optimizing the thermal field and airflow design, so as to prevent it from re-dissolving into the melt.

[0004] In existing technologies, adjusting the guide tube in the hot zone is an important means of optimizing airflow and reducing oxygen content. Currently, the commonly used guide tube angles (the angle between the inner wall of the guide tube and the vertical direction) in the industry are mainly 45 degrees, 30 degrees, 15 degrees, and 0 degrees. The working principle is that the smaller the guide tube angle, the smaller the gap between its lower end and the molten surface, thus significantly increasing the airflow velocity across the liquid surface at the same argon flow rate. Higher airflow velocities can more quickly and effectively carry the silicon monoxide gas volatilized from the molten surface out of the furnace, thereby reducing the oxygen content in the silicon rod.

[0005] Currently, a 30-degree flow guide is commonly used in the production of large-size single-crystal silicon rods. However, this method has revealed a series of serious problems in practical applications, specifically in the following three aspects: (1) Quality issues: The oxygen content of silicon rods is still too high, often exceeding the shipment standard of 10.5 ppma. The high oxygen content significantly increases the probability of concentric circle defects in downstream silicon wafers, causing customer complaints and after-sales problems, and seriously damaging the product reputation.

[0006] (2) Production capacity issues: In order to meet the delivery standards, the silicon rods with excessive oxygen content must be reverse-cut, which directly leads to an effective production capacity loss of about 7.25%. At the same time, in order to deal with the high oxygen problem, the production process is forced to adopt "low oxygen processes" such as low crucible rotation and low furnace pressure. However, these processes will destroy the stability of the crystal pulling process, resulting in a significant increase in the breakage rate, which further reduces the overall rod yield.

[0007] (4) Cost issues: High oxygen content not only increases the amount of machining reverse cutting and the workload of oxygen strip testing, but also the increase in the breakage rate significantly increases the non-productive time for operators to handle abnormalities and re-crystallize, resulting in a significant increase in labor costs and material losses.

[0008] In theory, using a 0-degree guide tube with a smaller angle can further reduce the air gap and increase the airflow velocity, thereby achieving a better oxygen reduction effect. However, directly replacing it with a 0-degree guide tube introduces new and more severe technical challenges: First, the increased coverage area of ​​the 0-degree guide tube on the melt surface leads to poorer liquid surface temperature stability, resulting in drastic diameter fluctuations during silicon rod growth, making precise control difficult. Second, and most fatally, the extremely small air gap and excessively high airflow velocity can trigger strong gas turbulence, causing "crystal wobbling" in the growing monocrystalline silicon rod. Once the wobbling silicon rod impacts the guide tube, it can easily cause major safety accidents such as rod explosion or rod drop, resulting in huge economic losses and equipment damage.

[0009] In summary, existing technologies for producing large-size monocrystalline silicon rods face a dilemma: using a 30-degree flow tube results in high oxygen content, making it impossible to resolve quality and cost issues; while using a 0-degree flow tube directly poses risks of temperature runaway and safety hazards, hindering stable mass production. Therefore, providing a solution for preparing large-size monocrystalline silicon rods that can effectively reduce oxygen content while ensuring a stable and safe crystal pulling process has become a critical technical problem that the industry urgently needs to solve.

[0010] In view of this, this disclosure is hereby made. Summary of the Invention

[0011] The purpose of this disclosure is to provide a monocrystalline silicon rod and its crystal pulling process. The crystal pulling process for monocrystalline silicon rods provided in the embodiments of this disclosure can solve the problems of uneven temperature, rod shaking, rod breakage and drop, and large diameter fluctuations during 0-degree current conduction, thereby improving the production stability and yield of monocrystalline silicon rods.

[0012] This disclosure is implemented as follows: In a first aspect, this disclosure provides a crystal pulling process for a single-crystal silicon rod, including: pulling a single-crystal silicon rod using a 0-degree current guide; The 0-degree flow guide meets the following requirements: (1) increasing the distance between the cooling medium and the silicon liquid; (2) increasing the length of the flow path of the inert gas in the water-cooled screen; The pulling process must meet the following requirements: (1) The crystal rotation speed is: equal diameter stage < shoulder formation stage ≤ welding stage; (2) The crucible rotation speed is: shoulder-forming stage ≤ welding stage < equal diameter stage; (3) The inert gas flow rate is: constant diameter stage < shoulder formation stage < welding stage; (4) The furnace pressure is: shoulder stage < equal diameter stage < welding stage.

[0013] In an optional embodiment, the distance between the cooling medium and the molten silicon is 60-80 mm.

[0014] In an optional embodiment, the distance between the cooling medium and the molten silicon is increased by increasing the height from the lower edge of the water-cooled screen in the 0-degree guide tube to the lower edge of the guide tube. Preferably, the height is 30-50mm.

[0015] In an optional embodiment, the length of the inert gas flow path in the water-cooled screen is increased by increasing the height of the water-cooled screen in the 0-degree guide tube for 0-degree flow guidance. Preferably, the height of the screen is 750-850mm.

[0016] In an optional implementation, the crystal rotation speeds at each stage of the pulling process are as follows: 4-5 rpm for the constant diameter stage; 5-7 rpm for the shoulder formation stage; and 5-7 rpm for the welding stage.

[0017] In an optional implementation, the crucible rotation speeds at each stage of the drawing process are as follows: 6-8 rpm for the shoulder-forming stage; 6-8 rpm for the welding stage; and 7-9 rpm for the equal diameter stage.

[0018] In an optional implementation, the inert gas flow rate at each stage of the drawing process is as follows: 70-80 slpm for the constant diameter stage; 80-100 slpm for the shoulder formation stage; and 100-150 slpm for the welding stage.

[0019] In an optional implementation, the furnace pressure at each stage of the drawing process is as follows: 5-6.5T for the shoulder-forming stage; 6.5-9T for the equal diameter stage; and 12-15T for the welding stage.

[0020] In an optional embodiment, the pixel value of the liquid outlet distance in the constant diameter stage is ≥52, wherein the pixel value of the liquid outlet distance is obtained by conversion through the CCD imaging calibration ratio coefficient k, the target liquid outlet distance pixel p=d / k, d is the actual physical length of the liquid outlet distance, and k is the ratio of the actual length of the reference object to the pixel length of the CCD image; preferably 52-60.

[0021] Secondly, this disclosure provides a single-crystal silicon rod, which is prepared by the crystal pulling process of the single-crystal silicon rod described in the foregoing embodiments; Preferably, the size of the single crystal silicon rod is 260-310 mm, and more preferably 280-300 mm.

[0022] The present disclosure has the following beneficial effects: By improving the thermal field structure of the 0-degree flow-guided process and combining it with the control of crystal rotation, crucible rotation, inert gas flow rate and furnace pressure during the pulling process, the crystal pulling process is adapted to the airflow characteristics of the 0-degree flow-guided thermal field, solving the problems of uneven melt temperature, crystal rod shaking, rod breaking and falling off, and large diameter fluctuations under the 0-degree flow-guided working condition, thereby improving the production stability and yield of single crystal silicon rods. Attached Figure Description

[0023] To more clearly illustrate the technical solutions of the embodiments of this disclosure, the accompanying drawings used in the embodiments will be briefly described below. It should be understood that the following drawings only show some embodiments of this disclosure and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0024] Figure 1 A suitable diagram showing the height from the lower edge of the water-cooled screen to the lower edge of the guide tube in the 0-degree guide tube provided in this disclosure; Figure 2 This is a schematic diagram showing the increase in height of the water-cooled screen body in the 0-degree guide tube provided in this disclosure; Figure 3 This is a schematic diagram of the 30-degree guide tube provided in this disclosure; Figure 4 A graph showing the oxygen content at different flow angles provided in this disclosure; Figure 5 This is a comparison chart of energy consumption for different crystal pulling processes provided in this disclosure. Detailed Implementation

[0025] To make the objectives, technical solutions, and advantages of the embodiments of this disclosure clearer, the technical solutions in the embodiments of this disclosure will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0026] This disclosure reveals that the diameter of single-crystal silicon rods prepared using a 0-degree guide tube exhibits large fluctuations and is prone to crystal wobble. Specifically, this disclosure finds that when the 0-degree guide tube is used for 0-degree flow, temperature instability easily occurs, leading to large diameter fluctuations. Furthermore, the smaller the guide angle, the smaller the gap between the guide tube and the molten surface, resulting in increased gas flow velocity. This increased gas flow velocity causes crystal wobble in the single-crystal silicon rod, potentially leading to serious accidents such as rod breakage or breakage upon impact with the guide tube. This disclosure provides a new crystal pulling process for single-crystal silicon rods that improves upon the aforementioned defects. Details are as follows: The Czochralski single crystal silicon rod is pulled by using 0-degree flow channeling, where 0-degree flow channeling meets the following requirements: (1) increasing the distance between the cooling medium and the silicon liquid; (2) increasing the length of the flow path of the inert gas in the water-cooled screen.

[0027] The pulling process must meet the following requirements: (1) Crystal rotation speed: equal diameter stage < shoulder stage ≤ welding stage; (2) Crucible rotation speed: shoulder stage ≤ welding stage < equal diameter stage; (3) Inert gas flow rate: equal diameter stage < shoulder stage < welding stage; (4) Furnace pressure: shoulder stage < equal diameter stage < welding stage.

[0028] This disclosure improves the thermal field structure of the 0-degree flow field by combining the control of crystal rotation, crucible rotation, inert gas flow rate and furnace pressure during the pulling process. This makes the crystal pulling process adaptable to the airflow characteristics of the 0-degree flow field, solves the problems of uneven melt temperature, crystal rod shaking, rod breaking and falling off, and large diameter fluctuations under the 0-degree flow field, and improves the production stability and yield of monocrystalline silicon rods.

[0029] Specifically, the distance between the cooling medium and the molten silicon is 60-80 mm, for example, any value between 60 mm, 65 mm, 70 mm, 75 mm, 80 mm, or 60-80 mm. In this disclosure, the distance between the cooling medium and the molten silicon is increased by increasing the height from the lower edge of the water-cooled screen to the lower edge of the 0-degree guide tube (i.e., HD; see schematic diagram of HD). Figure 1Specifically, the height is 30-50 mm. For example, it can be any value between 30 mm, 35 mm, 40 mm, 45 mm, 50 mm, or 30-50 mm. Increasing the height from the lower edge of the water-cooled screen to the lower edge of the guide tube in the 0-degree guide tube can reduce the influence of the water-cooled screen on the surface temperature of the silicon liquid, making the temperature more uniform, thereby reducing temperature fluctuations and diameter fluctuations.

[0030] Furthermore, the length of the flow path of the inert gas in the water-cooled screen is increased by increasing the height of the water-cooled screen in the 0-degree guide tube for 0-degree flow (see the schematic diagram of increasing the height of the water-cooled screen). Figure 2 The screen height is 750-850 mm; for example, it can be any value between 750 mm, 760 mm, 770 mm, 780 mm, 790 mm, 800 mm, 810 mm, 820 mm, 830 mm, 840 mm, 850 mm, or 750-850 mm. Using the above screen height can extend the flow path of the inert gas (e.g., argon), thereby stabilizing the inert gas flow direction.

[0031] Furthermore, the conditions for the welding stage are as follows: Crystal rotation speed (i.e., crystal rotation) is 5-7 rpm, for example, any value between 5 rpm, 5.5 rpm, 6 rpm, 6.5 rpm, 7 rpm, or 5-7 rpm. Crucible rotation speed (i.e., crucible rotation) is 6-8 rpm, for example, any value between 6 rpm, 6.5 rpm, 7 rpm, 7.5 rpm, 8 rpm, or 6-8 rpm. Inert gas flow rate is 100-150 slpm, for example, any value between 100 slpm, 110 slpm, 120 slpm, 130 slpm, 140 slpm, 150 slpm, or 100-150 slpm. Furnace pressure is 12-15T, for example, any value between 12T, 13T, 14T, 15T, or 12-15T.

[0032] The conditions for the shoulder-setting stage are as follows: Crystal rotation speed is 5-7 rpm, for example, any value between 5 rpm, 5.5 rpm, 6 rpm, 6.5 rpm, 7 rpm, or 5-7 rpm. Crucible rotation speed is 6-8 rpm, for example, any value between 6 rpm, 6.5 rpm, 7 rpm, 7.5 rpm, 8 rpm, or 6-8 rpm. Inert gas flow rate is 80-100 slpm, for example, any value between 80 slpm, 85 slpm, 90 slpm, 95 slpm, 100 slpm, or 80-100 slpm. Furnace pressure is 5-6.5T, for example, any value between 5T, 5.5T, 6T, 6.5T, or 5-6.5T.

[0033] The conditions for the constant diameter stage are as follows: Crystal rotation 4-5 rpm; for example, any value between 4 rpm, 4.5 rpm, 5 rpm, or 4-5 rpm. Crucible rotation 7-9 rpm; for example, any value between 7 rpm, 7.5 rpm, 8 rpm, 8.5 rpm, 9 rpm, or 7-9 rpm. Inert gas flow rate 70-80 slpm; for example, any value between 70 slpm, 75 slpm, 80 slpm, or 70-80 slpm. Furnace pressure 6.5-9T; for example, any value between 6.5T, 7T, 7.5T, 8T, 8.5T, 9T, or 6.5-9T.

[0034] In this disclosure, selecting the aforementioned values ​​for crystal rotation, crucible rotation, inert gas flow rate, and furnace pressure can further reduce airflow disturbance caused by the 0-degree guide tube, decrease crystal wobble amplitude, reduce crystal rod diameter fluctuation, and improve single crystal yield. Simultaneously, the aforementioned crystal rotation, crucible rotation, inert gas flow rate, and furnace pressure still conform to the numerical variation patterns of these values ​​in each stage, ensuring their effectiveness.

[0035] Furthermore, in this disclosure, the pixel value of the liquid outlet distance in the medium-diameter stage is ≥52, for example, any value between ≥52 such as 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, etc., preferably 52-60. The pixel value of the liquid outlet distance is obtained by conversion using the CCD imaging calibration ratio coefficient k, where the target liquid outlet distance pixel p = d / k, d is the actual physical length of the liquid outlet distance, and k is the ratio of the actual length of the reference object to the pixel length of the CCD image.

[0036] In summary, the embodiments of this disclosure have the following effects: (1) This disclosure is not a single parameter adjustment, but a change in the thermal field structure (the distance between the cooling medium and the silicon liquid is combined with the increase in the length of the inert gas flow path in the water-cooled screen); at the same time, the entire process of crystal rotation, crucible rotation, inert gas, furnace pressure, liquid outlet distance and other parameters are coupled together in the welding stage, shoulder stage and equal diameter stage, which is specially adapted to the airflow and thermal field characteristics of the 0-degree guide tube, and is not a simple parameter trial and error under normal working conditions.

[0037] (2) This disclosure further controls the height from the lower edge of the water-cooled screen to the lower edge of the guide tube (denoted as HD) to 30-50mm, which weakens the direct cooling of the silicon liquid surface by the water-cooled screen and makes the temperature field of the melt surface uniform. In addition, by increasing the height of the water-cooled screen to 750-850mm, the downward path of the inert gas is lengthened, the airflow is more stable, and the crystal rod shaking caused by airflow disturbance is reduced.

[0038] (3) This disclosure reduces crystal rotation and increases crucible rotation speed during the welding and shoulder-forming stages. Combined with the reduction of argon gas, increase of furnace pressure and increase of liquid outlet distance during the shoulder-forming and equal-diameter stages, multiple effects work together to suppress airflow disturbance caused by the 0-degree guide tube, reduce crystal sway amplitude, reduce rod breakage and rod drop accidents, significantly reduce crystal rod diameter fluctuation, and improve single crystal yield.

[0039] It should be noted that the structure of the 0-degree guide tube provided in this disclosure is derived from Inner Mongolia Zhonghuan Photovoltaic Materials Co., Ltd.'s patent CN110484967A, "A Flat-bottom Guide Tube for a Czochralski Silicon Single Crystal Furnace," with corresponding increases in HD height and water-cooled screen height, thus modifying the structure of patent CN110484967A. Figure 3 The middle structure 3 is extended, while other structures and connections remain unchanged.

[0040] Inert gases include, but are not limited to, argon and nitrogen.

[0041] The performance testing method disclosed herein is as follows: Crystal wobble amplitude: The operating software TDR Crystal Single Crystal Furnace Control Interface v3.21.1 software, CCD version v3.26.0115.111BV, judges crystal wobble through the equal diameter capture frame.

[0042] The formula for calculating the frying rate is: number of furnaces where frying occurred / total number of furnaces.

[0043] Diameter fluctuation: Using the TDR Jingsheng single crystal furnace control interface v3.21 software, the diameter value is recorded once every 10 seconds in the historical data file.

[0044] Production capacity is calculated as: weight of monocrystalline silicon rods produced by the monocrystalline furnace / number of days.

[0045] The features and performance of this disclosure will be further described in detail below with reference to embodiments.

[0046] Example 1 This disclosure provides a crystal pulling process for monocrystalline silicon rods, including: pulling monocrystalline silicon rods using a 0-degree current guide; wherein, the basic structure of the 0-degree current guide tube for the 0-degree current guide is described in Inner Mongolia Zhonghuan Photovoltaic Materials Co., Ltd.'s patent CN110484967A "A Flat Bottom Current Guide Tube for a Czochralski Silicon Monocrystalline Furnace", where the height from the lower edge of the water-cooled screen to the lower edge of the current guide tube is adjusted to 35mm (i.e., HD is 35mm), and the height of the water-cooled screen is adjusted to 810mm.

[0047] The process parameters for the entire crystal pulling process are as follows: Welding stage: crystal rotation 7 rpm, crucible rotation 7 rpm, argon flow rate 120 slpm, furnace pressure 13T.

[0048] Shoulder-forming stage: crystal rotation 7 rpm, crucible rotation 7 rpm, argon flow rate 80 slpm, furnace pressure 6T.

[0049] Constant diameter stage: crystal rotation 5 rpm, crucible rotation 7.5 rpm, argon flow rate 70 slpm, furnace pressure 7.5T, liquid outlet distance 56 pixels.

[0050] Performance test results: Crystal wobble amplitude <1mm; breakage rate 0%; diameter fluctuation ±1mm; production capacity 195kg / d.

[0051] Examples 2-4 Examples 2-4 each provide a crystal pulling process for a single-crystal silicon rod. This crystal pulling process is basically the same as that in Example 1, with the only difference being the specific parameters, as follows: Example 2: HD is 45mm, and the height of the water-cooled screen is 850mm; Welding stage: crystal rotation 6 rpm, crucible rotation 6 rpm, argon flow rate 150 slpm, furnace pressure 15T.

[0052] Shoulder-forming stage: crystal rotation 5 rpm, crucible rotation 6 rpm, argon flow rate 90 slpm, furnace pressure 6.5T.

[0053] Constant diameter stage: crystal rotation 4.5 rpm, crucible rotation 8.5 rpm, argon flow rate 75 slpm, furnace pressure 8T, liquid outlet distance 60 pixels.

[0054] Performance test results: Crystal wobble amplitude <1mm; breakage rate 0%; diameter fluctuation ±1mm; production capacity 190kg / d.

[0055] Example 3 The HD screen is 50mm high, and the water-cooled screen is 750mm high. Welding stage: crystal rotation 5 rpm, crucible rotation 8 rpm, argon flow rate 110 slpm, furnace pressure 12T.

[0056] Shoulder-forming stage: crystal rotation 4.5 rpm, crucible rotation 8 rpm, argon flow rate 100 slpm, furnace pressure 5T.

[0057] Constant diameter stage: crystal rotation 4 rpm, crucible rotation 9 rpm, argon flow rate 70 slpm, furnace pressure 6.5T, liquid outlet distance 52 pixels.

[0058] Performance test results: Crystal wobble amplitude <1mm; breakage rate 0%; diameter fluctuation ±1mm; production capacity 185kg / d.

[0059] Example 4 The HD screen is 40mm high, and the water-cooled screen is 820mm high. Welding stage: crystal rotation 7 rpm, crucible rotation 7 rpm, argon flow rate 150 slpm, furnace pressure 13T.

[0060] Shoulder formation stage: crystal rotation 6 rpm, crucible rotation 8 rpm, argon flow rate 80 slpm, furnace pressure 7.5-6T.

[0061] Constant diameter stage: crystal rotation 5 rpm, crucible rotation 9 rpm, argon flow rate 70 slpm, furnace pressure 9T, liquid outlet distance 56 pixels.

[0062] Performance test results: Crystal wobble amplitude <1mm; breakage rate 0%; diameter fluctuation ±1mm; production capacity 193kg / d.

[0063] Comparative Examples 1-4 Comparative Examples 1-4 each provide a crystal pulling process for a single-crystal silicon rod. This crystal pulling process is basically the same as that in Example 1, with the only difference being the specific parameters, as follows: Comparative Example 1 The HD is 35mm, the water-cooled screen height is 645mm, and other operations and parameters are consistent with Example 1. That is to say, Comparative Example 1 did not improve the 0-degree airflow.

[0064] Performance test results: Crystal wobble amplitude > 4mm; breakage rate 5%; diameter fluctuation ± 1mm; production capacity 190kg / d.

[0065] Comparative Example 2 The process parameters for the entire crystal pulling process are as follows: Welding stage: crystal rotation 9 rpm, crucible rotation 5 rpm, argon flow rate 120 slpm, furnace pressure 12T.

[0066] Shoulder-forming stage: crystal rotation 9 rpm, crucible rotation 4.5 rpm, argon flow rate 120 lpm, furnace pressure 6 T.

[0067] Constant diameter stage: crystal rotation 7 rpm, crucible rotation 6 rpm, argon flow rate 120 slpm, furnace pressure 5T. Other operations and parameters were consistent with Example 1. That is to say, Comparative Example 2 did not optimize the process parameters of the entire crystal pulling process, only the 0-degree flow path was optimized.

[0068] Performance test results: Crystal wobble amplitude > 6mm; breakage rate 8%; diameter fluctuation ± 1mm; production capacity 170kg / d.

[0069] Comparative Example 3 The HD screen is 35mm high, and the water-cooled screen is 645mm high.

[0070] The process parameters for the entire crystal pulling process are as follows: Welding stage: crystal rotation 9 rpm, crucible rotation 5 rpm, argon flow rate 120 slpm, furnace pressure 12T.

[0071] Shoulder-forming stage: crystal rotation 9 rpm, crucible rotation 4.5 rpm, argon flow rate 120 lpm, furnace pressure 6 T.

[0072] Constant diameter stage: crystal rotation 7 rpm, crucible rotation 6 rpm, argon flow rate 120 slpm, furnace pressure 5T.

[0073] In other words, this comparative model did not improve the 0-degree current conduction nor optimize the process parameters for the entire crystal pulling process.

[0074] Performance test results: swaying amplitude > 6mm; breakage rate 8%; diameter fluctuation ± 2mm; production capacity 160kg / d.

[0075] Comparing the test results of Example 1 and Comparative Examples 1-3, it can be seen that only when the improvement of 0-degree flow and the optimization of the process parameters of the entire crystal pulling process are implemented simultaneously can lower crystal wobble, breakage rate and higher production capacity be achieved.

[0076] Comparative Example 4 The HD screen is 35mm thick, and the water-cooled screen is 810mm tall. Welding stage: crystal rotation 9 rpm, crucible rotation 5 rpm, argon flow rate 120 slpm, furnace pressure 13T.

[0077] Shoulder-forming stage: crystal rotation 9 rpm, crucible rotation 5 rpm, argon flow rate 80 slpm, furnace pressure 6T.

[0078] Constant diameter stage: crystal rotation 8 rpm, crucible rotation 6 rpm, argon flow rate 70 slpm, furnace pressure 7.5T, liquid outlet distance 56 pixels.

[0079] Performance test results: Crystal wobble amplitude > 4mm; breakage rate 4%; diameter fluctuation ± 2mm; production capacity 165kg / d.

[0080] Comparative Example 5 This disclosure provides a crystal pulling process for a single-crystal silicon rod, including: pulling a single-crystal silicon rod using a 30-degree current guide; wherein the 30-degree current guide tube (HD) is 25mm long, the water-cooled screen is 645mm high, and the assembly scheme is the same as that of the 0-degree current guide tube, the main difference being the angle. The structure of the 30-degree current guide tube is shown in the figure below. Figure 3 .

[0081] The process parameters for the entire crystal pulling process are as follows: Welding stage: crystal rotation 9 rpm, crucible rotation 5 rpm, argon flow rate 120 slpm, furnace pressure 12T.

[0082] Shoulder-forming stage: crystal rotation 9 rpm, crucible rotation 4.5 rpm, argon flow rate 120 lpm, furnace pressure 6 T.

[0083] Constant diameter stage: crystal rotation 7 rpm, crucible rotation 6 rpm, argon flow rate 120 slpm, furnace pressure 5T.

[0084] Performance test results: Crystal wobble amplitude <1mm; breakage rate 0%; diameter fluctuation ±1mm; production capacity 155kg / d.

[0085] Comparing the test results of Example 1 and Comparative Example 5, it can be seen that the production capacity is significantly improved when 0-degree flow is used.

[0086] Meanwhile, comparing the concentric circles of Example 1 and Comparative Example 5, using a 0-degree flow path with oxygen content lower than that of a 30-degree flow path, and without the risk of reverse shearing and concentric circles, the concentric circle count decreased by 15.9%, as shown in Table 1. The concentric circles are derived from customer feedback at the cell end. Essentially, the concentric circles are swirling oxygen deposition rings on the monocrystalline silicon rod. In mass production, dark concentric rings are directly captured by PL infrared imaging. After PL detects anomalies, the laboratory uses low-temperature EBIC, copper decoration corrosion, and FTIR oxygen testing for traceability confirmation. Oxygen content is obtained by radially sampling the head of the monocrystalline silicon rod, slicing it into thin slices, polishing both sides, and then testing it using Fourier transform infrared spectroscopy. The test results are entered into the MES system database to obtain the oxygen content. Figure 4 .

[0087] Table 1 Test Results

[0088] Furthermore, the energy consumption of Comparative Example 1 and Comparative Example 5 (see...) Figure 5 The energy consumption of Example 1 is 55 kW, and the energy consumption of Comparative Example 5 is 64 kW (energy consumption is obtained through crystal pulling power, which refers to maintaining the molten silicon surface in a stable thermal field slightly above the melting point; the crystal pulling power varies depending on the thermal field used for seed crystal preheating, seed welding, and necking). It is evident that the embodiments of this disclosure can significantly reduce energy consumption.

[0089] The above description is merely a preferred embodiment of this disclosure and is not intended to limit this disclosure. Various modifications and variations can be made to this disclosure by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this disclosure should be included within the scope of protection of this disclosure.

Claims

1. A crystal pulling process for single-crystal silicon rods, characterized in that, include: Czochralski single-crystal silicon rods are pulled using a 0-degree current-carrying method. The 0-degree flow guide meets the following requirements: (1) increasing the distance between the cooling medium and the silicon liquid; (2) increasing the length of the flow path of the inert gas in the water-cooled screen; The pulling process must meet the following requirements: (1) The crystal rotation speed is: equal diameter stage < shoulder formation stage ≤ welding stage; (2) The crucible rotation speed is: shoulder-forming stage ≤ welding stage < equal diameter stage; (3) The inert gas flow rate is: constant diameter stage < shoulder formation stage < welding stage; (4) The furnace pressure is: shoulder stage < equal diameter stage < welding stage.

2. The crystal pulling process for a single-crystal silicon rod according to claim 1, characterized in that, The distance between the cooling medium and the molten silicon is 60-80 mm.

3. The crystal pulling process for a single-crystal silicon rod according to claim 1 or 2, characterized in that, The distance between the cooling medium and the molten silicon is increased by increasing the height from the lower edge of the water-cooled screen in the 0-degree guide tube to the lower edge of the guide tube. Preferably, the height is 30-50mm.

4. The crystal pulling process for a single-crystal silicon rod according to claim 1, characterized in that, The method to increase the length of the flow path of the inert gas in the water-cooled screen is to increase the height of the water-cooled screen in the 0-degree guide tube for 0-degree flow guidance; Preferably, the height of the screen is 750-850mm.

5. The crystal pulling process for a single-crystal silicon rod according to claim 1, characterized in that, The crystal rotation speeds at each stage of the pulling process are as follows: 4-5 rpm for the constant diameter stage; 5-7 rpm for the shoulder formation stage; and 5-7 rpm for the welding stage.

6. The crystal pulling process for a single-crystal silicon rod according to claim 1, characterized in that, The crucible rotation speeds at each stage of the drawing process are as follows: 6-8 rpm for the shoulder-forming stage; 6-8 rpm for the welding stage; and 7-9 rpm for the equal diameter stage.

7. The crystal pulling process for a single-crystal silicon rod according to claim 1, characterized in that, The inert gas flow rates at each stage of the drawing process are as follows: 70-80 slpm for the constant diameter stage; 80-100 slpm for the shoulder formation stage; and 100-150 slpm for the welding stage.

8. The crystal pulling process for a single-crystal silicon rod according to claim 1, characterized in that, The furnace pressure at each stage of the drawing process is as follows: 5-6.5T for the shoulder-forming stage; 6.5-9T for the equal diameter stage; and 12-15T for the welding stage.

9. The crystal pulling process for a single-crystal silicon rod according to claim 1, characterized in that, The pixel value of the liquid outlet distance in the constant diameter stage is ≥52, wherein the pixel value of the liquid outlet distance is obtained by converting the CCD imaging calibration ratio coefficient k, the target liquid outlet distance pixel p=d / k, d is the actual physical length of the liquid outlet distance, and k is the ratio of the actual length of the reference object to the pixel length of the CCD image; The preferred value is 52-60.

10. A single-crystal silicon rod, characterized in that, The single-crystal silicon rod is prepared by the crystal pulling process of the single-crystal silicon rod as described in claim 1. Preferably, the size of the single crystal silicon rod is 260mm-310mm, and more preferably 280-300mm.

Citation Information

Patent Citations

  • Flat-bottom guide cylinder of czochralski silicon single crystal furnace

    CN110484967A