Zinc-resistant whisker ceramic zinc plating rust-preventive composition and surface treatment method for steel materials

By using a ceramic zinc plating anti-rust composition composed of ethyl silicate and other materials and a micro-etching process, the problem of zinc whisker formation in ultra-precision environments has been solved, achieving excellent corrosion resistance and rust prevention, and reducing equipment failure and pollution risks.

CN123108743APending Publication Date: 2026-11-17KANFU CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511136457.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2025-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing chromium-free surface treatment compositions cannot effectively prevent the formation of zinc whiskers in ultra-precise controlled environments, leading to problems such as short circuits and microparticle contamination, while also involving the use of environmental pollutants such as chromium.

Method used

A ceramic zinc plating anti-rust composition containing ethyl silicate, hydrochloric acid, ethanol, isopropanol, methoxysilane compounds, whisker inhibitors and deionized water is used. The composition inhibits the formation and growth of zinc whiskers through nano-ceramic particles, organothiol compounds and flexibility modifiers, and improves adhesion by combining micro-etching process.

Benefits of technology

It effectively inhibits the formation of zinc whiskers, improves corrosion resistance, white rust resistance, blackening resistance and rust prevention, significantly reduces equipment failure and microparticle contamination risk, and is suitable for ultra-precision environments such as semiconductor factories and data centers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to an anti-zinc whisker ceramic galvanizing anti-rust composition and a surface treatment method for steel materials using the same. It provides an anti-zinc whisker ceramic galvanizing anti-rust composition for steel components used in ultra-precise controlled environments sensitive to microparticles and electromagnetic interference, such as semiconductor manufacturing plants, data centers, and AI factories, and imparts excellent corrosion resistance, white rust resistance, blackening resistance, and rust prevention. The anti-zinc whisker ceramic galvanizing anti-rust composition for ultra-precise controlled environments comprises ethyl silicate, hydrochloric acid, ethanol, isopropanol, methoxysilane compounds, whisker inhibitors, and deionized water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a ceramic zinc plating rust-preventive composition for preventing the formation of zinc whiskers in steel components used in ultra-precise controlled environments sensitive to microparticles and electromagnetic interference, such as semiconductor manufacturing plants, data centers, and AI factories, and to a surface treatment method for steel materials utilizing the same. Background Technology

[0002] Typically, chromate treatment is applied to prevent corrosion of galvanized metal surfaces such as galvanized steel sheets and bolts. While chromate treatment improves corrosion resistance and gloss, it also releases hexavalent chromium (Cr) during the process, which is harmful to the environment. 6+ ) and trivalent chromium (Cr 3+ The problem of chromium corrosion has led to ongoing development of chromium-free surface treatment compositions for preventing corrosion of galvanized metals by forming thin films using polymers, molybdenum anions, silica, pyrophosphates, etc. For example, Korean Patent No. 10-2174200 discloses a chromium-free surface treatment composition for improving the corrosion resistance of galvanized metals, comprising ethyl silicate, hydrochloric acid, ethanol, isopropanol, methoxysilane compounds, and deionized water. This surface treatment composition, even without the use of chromium, can improve the galvanized metal's resistance to blackening, white rust, corrosion, and rust prevention while exhibiting excellent adhesion to the galvanized metal.

[0003] However, even with existing chromium-free surface treatment compositions, there are limitations in effectively preventing zinc whisker problems arising in ultra-precise controlled environments. Zinc whiskers are elongated crystals that spontaneously grow on galvanized metal surfaces, typically reaching diameters of several micrometers and lengths of several millimeters. Once cut from the galvanized metal surface, they float and can cause various problems. In particular, in environments requiring extremely high cleanliness, such as semiconductor manufacturing plants, data centers, microelectronic devices, precision measuring instruments, and environments controlling high-purity gases or airflow, airborne zinc whiskers can cause critical issues such as short circuits, microparticle contamination, and product defects.

[0004] Therefore, there is an urgent need to develop anti-zinc whisker rust-preventing compositions that effectively suppress zinc whisker formation in galvanized metals while eliminating chromium, a harmful substance in the environment, and possess corrosion resistance, pollution resistance, and electrical properties suitable for ultra-precise controlled environments, as well as surface treatment methods for steel materials utilizing the same. Summary of the Invention

[0005] Technical issues

[0006] The technical problem to be solved by the present invention is to provide the following anti-zinc whisker ceramic zinc plating anti-rust composition: while eliminating the harmful substance chromium in the use environment, it effectively inhibits the formation of zinc whiskers in zinc plating metal, and has excellent corrosion resistance, white rust resistance, blackening resistance and rust prevention, making it suitable for ultra-precision controlled environments that are sensitive to microparticles and electromagnetic interference, such as semiconductor process factories, data centers, AI factories, etc.

[0007] Furthermore, another technical problem to be solved by the present invention is to provide a surface treatment method for steel materials using the zinc-resistant whisker ceramic zinc plating anti-rust composition.

[0008] Technical solution

[0009] An embodiment of the present invention for solving the aforementioned technical problem provides a zinc-resistant, whisker-resistant ceramic zinc-plated rust-preventing composition for ultra-precision controlled environments, which may contain ethyl silicate, hydrochloric acid, ethanol, isopropanol, methoxysilane compounds, whisker inhibitors, and deionized water.

[0010] The methoxysilane compounds may include glycidoxypropyltrimethoxysilane and methyltrimethoxysilane.

[0011] The whisker inhibitor may comprise nano-ceramic particles, organothiol compounds, and a flexibility modifier, wherein the flexibility modifier may comprise one or more of the group consisting of polydimethylsiloxane derivatives, organosilicon-modified polyacrylates, polyurethane dispersions, and mixtures thereof.

[0012] The zinc-resistant whisker ceramic zinc plating anti-rust composition for ultra-precision controlled environments may contain 48-55% by weight of ethyl silicate, 0.5-2% by weight of hydrochloric acid, 12-18% by weight of ethanol, 3-6% by weight of isopropanol, 12-18% by weight of methoxysilane compounds, 2-5% by weight of whisker inhibitors, and 12-18% by weight of deionized water.

[0013] Furthermore, the surface treatment method for steel materials using a zinc-resistant whisker ceramic zinc-plated rust-preventive composition for ultra-precision controlled environments, according to an embodiment of the present invention for solving the other technical problem, includes: a step of preparing an accessory made of steel material; a step of electroplating the accessory made of steel material to form an electroplated zinc layer; a step of pretreating the electroplated zinc layer; and a step of coating with the ceramic zinc-plated rust-preventive composition.

[0014] In the pretreatment step, a weak acid solution can be used to create an uneven surface on the electroplated zinc layer.

[0015] The effects of the invention

[0016] The zinc whisker-resistant ceramic zinc plating anti-rust composition of the present invention for ultra-precision controlled environments effectively inhibits the formation of zinc whiskers in zinc-plated metals even without the use of chromium. It provides excellent corrosion resistance, white rust resistance, blackening resistance, and rust prevention properties. In particular, by introducing a whisker inhibitor containing nano-ceramic particles, organothiol compounds, and flexibility modifiers to inhibit the surface diffusion of zinc ions and relieve the internal stress of the coating, it can effectively prevent the formation and growth of zinc whisker nuclei. This results in the low particle release characteristics required for ultra-precision controlled environments sensitive to microparticles and electromagnetic interference, such as semiconductor manufacturing plants, data centers, and AI factories. It can significantly reduce the risk of equipment failure or product defects caused by short circuits or microparticle contamination. Detailed Implementation

[0017] The following describes various embodiments of the present invention. It should be understood that the present invention is not limited to the specific embodiments, but should also include various modifications, equivalents, and / or alternatives to the embodiments of the present invention.

[0018] In this article, expressions such as “have,” “may have,” “include,” or “may include” refer to the presence of relevant features (e.g., structural elements such as numerical values, functions, operations, or accessories), rather than excluding the presence of additional features.

[0019] In this document, expressions such as “A or B”, “at least one of A and / or B”, or “one or more of A and / or B” can include all possible combinations of the listed items. For example, “A or B”, “at least one of A and B”, or “at least one of A or B” can include all of the following: (1) including at least one A; (2) including at least one B; or (3) including at least one A and at least one B.

[0020] The expression “configured to” as used herein may be used interchangeably with, for example, “suitable for”, “having the capacity to”, “designed to”, “adapted to”, “made to”, or “capable of”, depending on the context. The term “configured to” does not necessarily refer only to “specifically designed to”.

[0021] The terminology used herein is for illustrative purposes only and may not be intended to limit the scope of other embodiments. Singular expressions may include plural expressions unless explicitly stated in the context. Terms used herein, including technical or scientific terms, may have the same meaning as commonly understood by one of ordinary skill in the art to which the content described herein pertains. Terms used herein that are defined in a common dictionary may be interpreted as having the same or similar meaning as they have in the context of the relevant description, and should not be over-interpreted as having a formal meaning unless explicitly defined herein. Depending on the context, even terms defined herein may not preclude interpretation based on the embodiments described herein.

[0022] The embodiments disclosed herein are provided for illustration and understanding of the disclosed technical content, and are not intended to limit the scope of the invention. Therefore, the scope of this document should be interpreted to include all modifications or various other embodiments based on the technical concept of the invention.

[0023] The present invention will now be described in detail.

[0024] An embodiment of the present invention provides a zinc-resistant whisker ceramic zinc plating anti-rust composition comprising ethyl silicate, hydrochloric acid, ethanol, isopropanol, methoxysilane compounds, whisker inhibitors, and deionized water.

[0025] Ethyl silicate improves the density of the structure by hydrolyzing to form polysilicate. It can also improve adhesion, corrosion resistance, rust prevention, resistance to blackening, and resistance to white rust by forming chemical bonds with the electroplated zinc layer. In particular, ethyl silicate inhibits the surface diffusion of zinc ions by forming a zinc-silicon bond layer that is directly bonded to the surface of the electroplated zinc layer. Thus, it can work together with zinc whisker inhibitors to prevent the formation of zinc whiskers.

[0026] The ceramic zinc-plated anti-rust composition may contain 48-55% ethyl silicate by weight, specifically 50-52% by weight. If the ethyl silicate content is less than 48% by weight, it will reduce the adhesion, corrosion resistance, rust prevention, blackening resistance, and white rust resistance between the electroplated zinc layer and the ceramic zinc-plated anti-rust composition coating. If it is greater than 55% by weight, it will easily cause cracking and damage to the ceramic zinc-plated anti-rust composition coating.

[0027] Hydrochloric acid can act as a catalyst to promote the hydrolysis of ethyl silicate. Based on the total weight of the ceramic zinc-plated anti-rust composition, it can contain 0.5–2% by weight, specifically 0.7–1.5% by weight. If the amount of hydrochloric acid is less than 0.5% by weight, it will reduce the adhesion, corrosion resistance, rust prevention, resistance to blackening, and resistance to white rust between the electroplated zinc layer and the ceramic zinc-plated anti-rust composition coating. If it is greater than 2% by weight, it will reduce the formulation stability, storage stability, and usability of the ceramic anti-rust solution, and may promote the corrosion of the electroplated zinc layer.

[0028] Ethanol can adjust the fluidity and viscosity of the ceramic zinc-plated rust-preventive composition. Based on the total weight of the ceramic zinc-plated rust-preventive composition, it can contain 12-18% by weight, specifically 14-16% by weight. If the ethanol content is less than 12% by weight, the increased viscosity of the ceramic zinc-plated rust-preventive composition will increase the thickness of the coating, potentially leading to cracking and damage. If it is greater than 18% by weight, it will reduce the adhesion, corrosion resistance, rust prevention, resistance to blackening, and resistance to white rust of the coating.

[0029] Isopropanol can improve the stability of the ceramic zinc-plated anti-rust composition and adjust its flowability and viscosity. Based on the total weight of the ceramic zinc-plated anti-rust composition, it can contain 3-6% by weight, specifically 4-5% by weight. If the isopropanol content is less than 3% by weight, it will reduce the stability and flowability of the ceramic zinc-plated anti-rust composition and increase viscosity. If it is greater than 6% by weight, it will reduce the adhesion, corrosion resistance, rust prevention, resistance to blackening, and resistance to white rust of the ceramic zinc-plated anti-rust composition coating.

[0030] The methoxysilane compound can contain glycidyl etheroxypropyltrimethoxysilane and methyltrimethoxysilane in a weight ratio of 1:1.5 to 2, specifically, a weight ratio of 1:1.8. The glycidyl etheroxypropyltrimethoxysilane improves the adhesion of the ceramic zinc-plated anti-rust composition and improves flowability by preventing excessive viscosity increase. The methyltrimethoxysilane improves the water resistance of the ceramic zinc-plated anti-rust composition coating and gives the coating a self-cleaning effect. The total weight of the ceramic zinc-plated anti-rust composition can contain 12 to 18% by weight of the methoxysilane compound, specifically, 14 to 16% by weight. If the methoxysilane compound contained is less than 12% by weight, problems will occur in reducing the adhesion, bonding, flowability, water resistance and self-cleaning ability of the ceramic zinc-plated anti-rust composition coating. If it is greater than 18% by weight, the ceramic zinc-plated anti-rust composition coating is prone to cracking and damage, and white powder will precipitate on the surface of the coating.

[0031] Whisker inhibitors are the core components that inhibit the formation and growth of zinc whiskers, and may include nano-ceramic particles, organothiol compounds, and flexibility modifiers.

[0032] Based on the total weight of the aforementioned ceramic zinc-plated rust-preventive composition, 2 to 5% by weight of whisker inhibitor may be included, specifically, 3 to 4% by weight.

[0033] If the whisker inhibitor content is less than 2% by weight, the zinc whisker inhibition effect cannot be fully utilized, and the long-term stability will be reduced due to the negligible effect on improving the internal stress relief and mechanical strength of the ceramic zinc-plated anti-rust composition coating. Conversely, if the content is greater than 5% by weight, the stability of the ceramic zinc-plated anti-rust composition will be reduced, and the uniformity of the coating will be reduced due to excessive agglomeration of nano-ceramic particles, resulting in reduced economic efficiency due to increased costs.

[0034] The nano-ceramic particles can be selected from the group consisting of SiO2, Al2O3, TiO2, ZrO2, and mixtures thereof, preferably a mixture of SiO2 and Al2O3. The nano-ceramic particles act as a physical barrier within the ceramic zinc-plated anti-rust composition coating, inhibiting the surface expansion of zinc ions and improving the mechanical strength of the coating. Furthermore, the surface properties of the nano-ceramic particles can also provide an antistatic effect.

[0035] The size of the nano-ceramic particles is 10–50 nm, preferably in the range of 15–30 nm. If the particle size is less than 10 nm, the dispersibility will be reduced due to particle aggregation, and if it is greater than 50 nm, the whisker suppression effect will be reduced due to uneven distribution within the coating.

[0036] The total weight of the ceramic zinc-plated rust-preventive composition may contain 0.8 to 2% by weight of the nano-ceramic particles, specifically 1 to 1.5% by weight.

[0037] The organothiol compound can be selected from the group consisting of 3-mercaptopropyltrimethoxysilane (MPTMS), mercaptoacetic acid, and mixtures thereof, preferably 3-mercaptopropyltrimethoxysilane. The organothiol compound significantly reduces the surface mobility of zinc ions by forming strong chemical bonds with the electroplated zinc layer surface through its thiol group (-SH), thereby inhibiting whisker nucleation.

[0038] The total weight of the ceramic zinc-plated rust-preventive composition may contain 0.5 to 1.5% by weight of the organothiol compound, specifically 0.8 to 1.2% by weight.

[0039] The flexibility modifier can be selected from the group consisting of polydimethylsiloxane derivatives, organosilicon-modified polyacrylates, polyurethane dispersions, and mixtures thereof. Preferably, polydimethylsiloxane derivatives containing siloxane functional groups can be used. The flexibility modifier relieves the internal stress of the ceramic zinc-plated anti-rust composition coating and disperses external mechanical pressure to prevent cracking or damage to the coating, thereby improving the long-term stability of the coating and maintaining whisker suppression performance.

[0040] The total weight of the ceramic zinc-plated rust-preventive composition may contain 0.7 to 1.5% by weight of the flexibility modifier, specifically 0.9 to 1.3% by weight.

[0041] Deionized water helps hydrolyze ethyl silicate. Ethyl silicate is hydrolyzed by deionized water to form polysilicate, thus achieving the effects described above.

[0042] The total weight of the ceramic zinc-plated rust-preventive composition may contain 12-18% by weight of deionized water, preferably 14-16% by weight. If the total weight of the ceramic zinc-plated rust-preventive composition contains less than 12% by weight of deionized water, insufficient hydrolysis of ethyl silicate will cause a decrease in the adhesion, resistance to blackening, resistance to white rust, corrosion resistance, rust prevention, stability, and zinc whisker inhibition performance of the ceramic zinc-plated rust-preventive composition. If the total weight of deionized water is greater than 18% by weight, the stability of the ceramic zinc-plated rust-preventive composition will decrease, and it will deteriorate.

[0043] Furthermore, the present invention can provide a surface treatment method for steel materials utilizing the aforementioned ceramic zinc plating anti-rust composition.

[0044] Specifically, the surface treatment method for steel materials according to an embodiment of the present invention consists of a step of preparing accessories made of steel materials, an electroplating zinc step, a pretreatment step, and a step of coating with a ceramic zinc-plated anti-rust composition.

[0045] The step of preparing accessories made of steel materials involves preparing and cleaning steel material accessories used in ultra-precise controlled environments sensitive to microparticles and electromagnetic interference, such as semiconductor manufacturing plants, data centers, and AI factories. The steel material accessories are not particularly limited, but may include equipment brackets, iron frame structures, roof grilles, cable trays, wiring conduits, cooling equipment frames, air conditioning ducts, electromagnetic interference shielding panels, etc.

[0046] In the electroplating zinc step, the cleaned steel fittings can be electroplated zinc according to known methods. Specifically, in the electroplating zinc step of this embodiment, an alkaline electroplating solution containing 7-20 g / L zinc oxide, 110-150 g / L sodium hydroxide, 5-15 mL / L complexing agent, 0.5-5 mL / L brightener, 1-10 mL / L impurity remover, 1-10 mL / L water softener, and 0.1-1 mL / L nonionic surfactant can be used at 20-40°C and a current density of 1-5 A / dm³. 2 Electroplating of zinc can be performed under certain conditions, but is not limited to these. The electroplated zinc layer can be formed with a thickness of approximately 8 μm to 30 μm.

[0047] The pretreatment step may include a micro-etching process that uses a weak acid solution (citric acid, acetic acid, oxalic acid, etc.) with pH 4.5 to 5.5 to form fine surface irregularities on the surface of the electroplated zinc layer to improve adhesion to the ceramic zinc anti-rust composition.

[0048] In the step of coating with the ceramic-zinc anti-rust composition, a coating of approximately 1 μm to 7 μm thickness is formed on the upper part of the electroplated zinc layer using the ceramic-zinc anti-rust composition of an embodiment of the present invention, which can prevent the formation of zinc whiskers and improve corrosion resistance and rust prevention. Specifically, in the step of coating with the ceramic-zinc anti-rust composition, the ceramic-zinc anti-rust composition coating can be formed on the upper part of the electroplated zinc layer by immersing the electroplated zinc fitting made of steel material in the ceramic-zinc anti-rust composition, followed by drying and curing.

[0049] The drying and curing can be carried out without particular restriction using known drying and curing methods. Preferably, the ceramic zinc-plated anti-rust composition coating is uniformly formed on the entire surface area of ​​the fitting made of steel material by means of free fall after deposition. Alternatively, the remaining ceramic zinc-plated anti-rust composition can be blown off with high-pressure air as needed.

[0050] The following examples, comparative examples, and experimental examples illustrate in detail the surface treatment method for steel materials using a zinc-resistant whisker ceramic zinc plating composition for ultra-precision controlled environments. These examples are for illustrative purposes only and the scope of the invention should not be construed as limited to these examples.

[0051] Example

[0052] A zinc-whisker-resistant ceramic zinc-plating rust-preventive composition for ultra-precision controlled environments was prepared according to the composition shown in Table 1 (unit: weight %). Furthermore, in Table 1, the methoxysilane compounds used are those shown in Table 2 (unit: weight ratio), and the whisker inhibitors used are those shown in Table 3 (unit: weight ratio). Then, after degreasing the electroplated zinc steel fittings (electroplated zinc steel sheets) with isopropanol, they were immersed in a citric acid aqueous solution (1 wt%) at pH 5.0 for 1 minute for micro-etching, followed by washing with deionized water and drying with hot air. The surface-treated electroplated zinc steel fittings were then immersed in the ceramic zinc-plating rust-preventive composition for 25 seconds and dried and cured by free fall. The final coating thickness was approximately 3 μm.

[0053] Table 1

[0054] Composition of ceramic zinc plating anti-rust composition

[0055] Element Example 1 Example 2 Example 3 Example 4 Example 5 Ethyl silicate 50 51 52 50 50 hydrochloric acid 1 1 1 0.8 1.2 ethanol 15 14 15 16 14 Isopropanol 5 4 4 4 5 Methoxysilane compounds 15 16 14 15 15 whisker inhibitors 3 3.5 4 3 3.3 Deionized water 11 10.5 10 11.2 11.5

[0056] Table 2

[0057] Composition of methoxysilane compounds

[0058] Element Example 1 Example 2 Example 3 Example 4 Example 5 GPTMS 1 1 1 1 1 MTMS 1.5 1.8 2.0 1.5 1.6

[0059] Table 3

[0060] Whisker inhibitor composition

[0061]

[0062] Comparative example

[0063] Comparative Example 1

[0064] According to existing chromate treatment processes, electroplated galvanized steel fittings are washed with water and then immersed in a 0.5%–1% oxalic acid solution, followed by further washing and chromate treatment. In this case, the chromate treatment involves immersing the washed electroplated galvanized steel fittings in a 20 g / L KCr(SO4)2 solution (with Cr...) as described above. 3+ The process involves drying the chromate-treated steel fittings in a solution containing 2.344 g / L. Following this, the steel fittings are washed with water and hot water, and then dried at approximately 60°C to produce chromate-treated electroplated zinc steel fittings.

[0065] Comparative Example 2

[0066] Except for the absence of whisker inhibitors and the presence of 14% by weight of deionized water, the surface-treated electroplated steel fittings were manufactured using the same method as in Example 1.

[0067] Comparative Example 3

[0068] Except that glycidoxypropyltrimethoxysilane is used only as a methoxysilane compound, surface-treated electroplated steel fittings are manufactured in the same manner as in Example 1.

[0069] Comparative Example 4

[0070] Except that only methyltrimethoxysilane is used as a methoxysilane compound, the surface-treated electroplated steel fittings are manufactured in the same manner as in Example 1.

[0071] Comparative Example 5

[0072] Except for using only nano-ceramic particles as whisker inhibitors, the surface-treated electroplated steel fittings were manufactured using the same method as in Example 1.

[0073] Comparative Example 6

[0074] The surface-treated electroplated steel fittings were manufactured using the same method as in Example 1, except that only 3-mercaptopropyltrimethoxysilane was used as a whisker inhibitor.

[0075] Comparative Example 7

[0076] The surface-treated electroplated steel fittings were manufactured using the same method as in Example 1, except that only polydimethylsiloxane derivatives were used as whisker inhibitors.

[0077] Experimental Example

[0078] Experimental Example 1: Evaluation of Zinc Whisker Formation Inhibition

[0079] Test pieces (50mm × 50mm × 1mm) of electroplated galvanized steel fittings from Examples 1 to 5 and Comparative Examples 1 to 7 were prepared and subjected to temperature cycling tests. The temperature cycling was performed for 500 cycles, starting at -40°C and increasing to 85°C in one-hour intervals. After the test, the surface of the test pieces was observed using a scanning electron microscope (SEM), and the average whisker density, average whisker length, and maximum whisker length per unit area were measured. The results are shown in Table 4 below. The average whisker density per unit area was converted to the value per unit area (mm²) by counting the number of whiskers found in five regions (each 2mm × 2mm) of each test piece. 2 The average whisker length is calculated by measuring the length of all whiskers found and averaging the results. The whisker length is the measured vertical distance from the surface of the specimen to the tip of the whisker. The maximum whisker length is the longest whisker length found among all the specimens measured.

[0080] Table 4

[0081]

[0082]

[0083] Referring to Table 4, it can be confirmed that the ceramic zinc plating anti-rust compositions of Examples 1 to 5 of the present invention significantly inhibit the formation of zinc whiskers. In particular, it can be confirmed that Example 2 has the best zinc whisker formation inhibition effect in all aspects, including average whisker density, average whisker length, and maximum whisker length.

[0084] Experimental Example 2: Corrosion Resistance Assessment

[0085] According to the salt spray test method (KSD 9502 test standard), the electroplated galvanized steel fittings (50mm×50mm×1mm) of Examples 1 to 5 and Comparative Examples 1 to 7 were subjected to a continuous salt spray test for 1000 hours using 5% salt water. The occurrence of rust (white rust or red rust) was observed visually, and the results are shown in Table 5 below. In this case, the occurrence of rust (white rust or red rust) is indicated by ○, and the absence of rust (white rust or red rust) is indicated by X.

[0086] Table 5

[0087]

[0088]

[0089] Experimental Example 3: Adhesion Assessment

[0090] According to the cross-cut test method (ASTM D 3359 test standard), the adhesion between the electroplated zinc layer and the ceramic zinc anti-rust composition coating of the electroplated zinc steel fittings of Examples 1 to 5 and Comparative Examples 1 to 7 was repeatedly evaluated 5 times, and the average values ​​are shown in Table 6. The adhesion was evaluated in terms of OB to 5B, with the closer to 5B indicating better adhesion.

[0091] 5B: The separated area is 0%.

[0092] 4B: The separated area is less than 5%.

[0093] 3B: The separated area is 5-15%.

[0094] 2B: The separated area is 15-35%.

[0095] 1B: The separated area is 35-65%.

[0096] 0B: The separated area is over 65%.

[0097] Table 6

[0098] distinguish Adhesion Example 1 4.8B Example 2 5.0B Example 3 4.9B Example 4 4.5B Example 5 4.6B Comparative Example 1 2.6B Comparative Example 2 4.2B Comparative Example 3 3.8B Comparative Example 4 3.5B Comparative Example 5 3.9B Comparative Example 6 4.0B Comparative Example 7 3.2B

[0099] Referring to Table 6, it can be confirmed that the adhesion of the electroplated galvanized steel fittings coated with the ceramic zinc-plating anti-rust compositions of Examples 1 to 5 of the present invention is excellent, ranging from 4.5 to 5.0B. In particular, Example 2 shows the highest level of adhesion at 5.0B. Conversely, it can be confirmed that the adhesion of Comparative Example 1 (chromate treatment) is very low at 2.6B, and the other comparative examples also show relatively lower adhesion than the examples of the present invention.

[0100] The invention has been described in relation to the preferred embodiments mentioned above. Various modifications or variations can be made without departing from the spirit and scope of the invention. Therefore, these modifications or variations falling within the spirit of the invention should also be included within the scope of the claims.

Claims

1. A zinc-resistant, whisker-based, galvanized ceramic anti-rust composition for use in ultra-precision controlled environments, characterized in that, It contains ethyl silicate, hydrochloric acid, ethanol, isopropanol, methoxysilane compounds, whisker inhibitors, and deionized water.

2. The zinc-whisker-resistant ceramic zinc-plated rust-preventive composition for ultra-precision controlled environments according to claim 1, characterized in that, The methoxysilane compounds include glycidoxypropyltrimethoxysilane and methyltrimethoxysilane.

3. The zinc-whisker-resistant ceramic zinc-plated rust-preventive composition for ultra-precision controlled environments according to claim 1, characterized in that, The whisker inhibitor comprises nano-ceramic particles, organic thiol compounds, and a flexibility modifier. The flexible modifier comprises one or more selected from the group consisting of polydimethylsiloxane derivatives, organosilicon-modified polyacrylates, polyurethane dispersions, and mixtures thereof.

4. The zinc-whisker-resistant ceramic zinc-plated rust-preventive composition for ultra-precision controlled environments according to claim 1, characterized in that, The zinc-resistant whisker ceramic zinc-plated rust-preventing composition for ultra-precision controlled environments comprises 48-55% by weight of ethyl silicate, 0.5-2% by weight of hydrochloric acid, 12-18% by weight of ethanol, 3-6% by weight of isopropanol, 12-18% by weight of methoxysilane compounds, 2-5% by weight of whisker inhibitors, and 12-18% by weight of deionized water.

5. A method for surface treatment of steel materials using a zinc-resistant whisker ceramic zinc-plated rust-preventing composition for ultra-precision controlled environments, characterized in that, include: Steps for preparing fittings made of steel materials; The step of electroplating zinc onto the fittings made of steel to form an electroplated zinc layer; The step of pretreating the electroplated zinc layer; as well as The steps of coating a ceramic zinc-plated anti-rust composition, In the pretreatment step, a weak acid solution is used to create an uneven surface on the electroplated zinc layer.