A positive electrode active material and its preparation method, and a positive electrode sheet.
By modifying manganese silicate materials and introducing metal sulfides, a porous positive electrode active material is formed, which solves the problems of poor conductivity and slow ion transport of manganese silicate materials and improves the electrochemical performance of supercapacitors.
Patent Information
- Application Number
- CN202611375625.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-17
AI Technical Summary
Existing manganese silicate materials have poor conductivity and slow ion transport rate in supercapacitor cathode materials, making it difficult to meet the needs of practical applications.
By modifying manganese silicate material with Mxene and introducing metal sulfides, a positive electrode active material with a porous structure is formed through mixing and reaction at a specific temperature, thereby improving conductivity and ion transport rate.
This achieves high conductivity, structural stability, and high ion transport rate in the positive electrode active material, thereby improving the rate performance and chemical stability of the positive electrode sheet.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery technology, specifically relating to a positive electrode active material and its preparation method, and a positive electrode sheet. Background Technology
[0002] With the continuous development of new energy technologies, users are placing higher demands on the energy density and power density of energy storage devices. Lithium-ion batteries, as a relatively mature energy storage device, still have significant room for improvement in power density. Supercapacitors, as an emerging energy storage device, combine the high power density of traditional capacitors with the high energy density of batteries, and have been widely used in specific fields.
[0003] In the research of cathode materials for supercapacitors, manganese silicate materials prepared by hydrothermal synthesis from silicon and manganese sources have poor intrinsic conductivity and slow ion transport rate, which makes it difficult for their electrochemical performance to meet the needs of practical applications and limits their large-scale use. Summary of the Invention
[0004] This invention provides a positive electrode active material and its preparation method, as well as a positive electrode sheet. The positive electrode active material provided by this invention has good conductivity, structural stability, and high ion transport rate.
[0005] According to one aspect of the present invention, a positive electrode active material is provided, wherein the raw materials for preparing the positive electrode active material include manganese silicate material and Mxene material; the chemical formula of Mxene material is M n+1 X n T x , 2≤n≤3, where M represents a transition metal element, X represents a C or N element, and T x T represents the surface functional groups of Mxene materials; x It includes at least one of -O, -OH, -F, -Cl, -Br, -I, -NH, and -CH3.
[0006] In this invention, Mxene material possesses good conductivity, enabling the establishment of high-speed transport channels for the positive electrode active material. The surface functional groups of Mxene material reduce particle aggregation and volume expansion after long cycling, while simultaneously improving the wettability between the positive electrode sheet made from this active material and the electrolyte. Therefore, this invention uses Mxene-modified manganese silicate as the positive electrode active material, which exhibits good conductivity, structural stability, and a high ion transport rate.
[0007] Preferably, M includes at least one of Ti, V, and Nb.
[0008] Preferably, M includes Ti.
[0009] Preferably, the Mxene material includes Ti3C2T x V4C3T x and Nb4C3T x At least one of them.
[0010] Preferably, the raw materials used to prepare the positive electrode active material also include metal sulfides. The introduction of metal sulfides allows some metal ions to replace Mn in the manganese silicate material. 2+ This process introduces oxygen vacancies into the positive electrode active material. These vacancies provide additional active sites, which not only adsorb ions and increase capacitance but also provide more channels for ion diffusion, lowering the ion migration barrier and thus improving the rate performance of the positive electrode sheet made from this active material. Furthermore, the bond energy of the chemical bond formed between the metal element and oxygen in the metal sulfide is higher than that of the Mn-O bond, enabling the structural stability of the positive electrode active material to be maintained under high current charge-discharge conditions, thereby enhancing the chemical stability of the electrode.
[0011] Preferably, the metal sulfide includes at least one of NiS, Ni3S2, NiS2, MoS2, CoS, Co3S2, and CoS2.
[0012] According to another aspect of the present invention, a method for preparing a positive electrode active material is provided, comprising the following steps: mixing manganese silicate material, Mxene material, and metal sulfide to obtain mixture A, and then reacting mixture A at a temperature of 170~190°C for 9~11 hours. The positive electrode active material prepared by the method provided by the present invention has good porous structure integrity, effectively reducing the obstruction of ion transport channels, thereby improving the ion transport rate.
[0013] Preferably, the manganese silicate material is prepared from silicon source material and manganese source material; the silicon source material includes Na2SiO3·9H2O; the manganese source material includes MnCl2·4H2O.
[0014] Preferably, the molar ratio is calculated as follows: silicon source material: manganese source material = (0.5~1.5):1.
[0015] Preferably, manganese silicate material, Mxene material, and metal sulfide are mixed to obtain mixture A, and then mixture A is reacted at a temperature of 170~190°C for 9~11 hours.
[0016] Preferably, the mass ratio of Mxene material to metal sulfide is (7~13):(4~7). By adjusting the mass ratio of metal sulfide to silicon source material within the above range, the doping amount of metal elements in the positive electrode active material can be effectively controlled, effectively balancing the structural stability of the positive electrode active material with the rate performance of the positive electrode sheet made from the positive electrode active material.
[0017] Preferably, the mass ratio of Mxene material to silicon source material is (5-13):100.
[0018] According to another aspect of the present invention, a positive electrode sheet is provided, comprising a current collector and a positive electrode active material layer disposed on the surface of the current collector; the positive electrode active material layer comprises the above-described positive electrode active material or a positive electrode active material prepared by the above-described preparation method.
[0019] Applying the positive electrode active material provided by this invention to the positive electrode sheet can simultaneously improve the rate performance and chemical stability of the positive electrode sheet. Detailed Implementation
[0020] To enable those skilled in the art to better understand the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.
[0021] Example 1 This embodiment provides a positive electrode sheet, the preparation method of which includes the following steps: S1. Preparation of positive electrode active material: Silicon source material, manganese source material, Mxene material, and metal sulfide are dissolved in deionized water to obtain mixture A. Among the materials used above, the silicon source material is Na2SiO3·9H2O, the manganese source material is MnCl2·4H2O, and the Mxene material is Ti3C2T. x (Xianfeng Nano XFK01-1), the metal sulfide is NiS, calculated by molar ratio, Na2SiO3·9H2O:MnCl2·4H2O=1:1, calculated by mass ratio, Ti3C2T x The mass ratio of NiS to Na2SiO3·9H2O is 11:100, and the mass ratio of NiS to Na2SiO3·9H2O is 6:100. The mixture A was then reacted at 180°C for 10 hours, followed by centrifugation. The resulting solid was then vacuum-dried in a vacuum drying oven at 60°C for 12 hours to obtain the positive electrode active material.
[0022] S2. Preparation of the positive electrode sheet: The above-mentioned positive electrode active material, binder, and conductive agent are stirred evenly to obtain a positive electrode slurry. Among the materials used above, the binder is PVDF and the conductive agent is SuperP. The mass ratio of positive electrode active material: binder: conductive agent is 8:1:1. Subsequently, the above-mentioned positive electrode slurry is coated on carbon paper and dried at a temperature of 60°C for 12 hours, thereby forming a positive electrode active material layer on the surface of the carbon paper, thus obtaining the positive electrode sheet of this embodiment.
[0023] Example 2 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that, in the process of preparing the positive electrode active material, while maintaining Ti3C2T x With the total amount of Na2SiO3·9H2O remaining constant, Ti3C2T x The mass ratio of Na2SiO3·9H2O to Na2SiO3·9H2O was adjusted to 5:100. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0024] Example 3 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that, in the process of preparing the positive electrode active material, while maintaining Ti3C2T x With the total amount of Na2SiO3·9H2O remaining constant, Ti3C2T x The mass ratio of Na2SiO3·9H2O to Na2SiO3·9H2O was adjusted to 7:100. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0025] Example 4 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that, in the process of preparing the positive electrode active material, while maintaining Ti3C2T x With the total amount of Na2SiO3·9H2O remaining constant, Ti3C2T x The mass ratio of Na2SiO3·9H2O to Na2SiO3·9H2O was adjusted to 13:100. Apart from the above differences, the materials, formulation ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0026] Example 5 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that, in the process of preparing the positive electrode active material, while maintaining Ti3C2T x With the total amount of Na2SiO3·9H2O remaining constant, Ti3C2T x The mass ratio of Na2SiO3·9H2O to Na2SiO3·9H2O was adjusted to 15:100. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0027] Example 6 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that, in the process of preparing the positive electrode active material, while keeping the total amount of NiS and Na2SiO3·9H2O unchanged, the mass ratio of NiS to Na2SiO3·9H2O is adjusted to 3:100. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0028] Example 7 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that, in the process of preparing the positive electrode active material, while keeping the total amount of NiS and Na2SiO3·9H2O unchanged, the mass ratio of NiS to Na2SiO3·9H2O is adjusted to 4:100. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0029] Example 8 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that, in the process of preparing the positive electrode active material, while keeping the total amount of NiS and Na2SiO3·9H2O unchanged, the mass ratio of NiS to Na2SiO3·9H2O is adjusted to 7:100. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0030] Example 9 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that, in the process of preparing the positive electrode active material, while keeping the total amount of NiS and Na2SiO3·9H2O unchanged, the mass ratio of NiS to Na2SiO3·9H2O is adjusted to 8:100. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0031] Example 10 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that, in the process of preparing the positive electrode active material, an equal mass of Ti3C2T is used. x The materials, formulation ratios, and preparation operations used in this embodiment are strictly consistent with those in Example 1, except for the differences mentioned above, which replace NiS in Example 1.
[0032] Example 11 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that in the process of preparing the positive electrode active material, an equal mass of VS2 is used to replace NiS in Example 1. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0033] Example 12 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that the reaction temperature of mixture A is adjusted to 170°C and the reaction time is adjusted to 11 hours during the preparation of the positive electrode active material. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0034] Example 13 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that the reaction temperature of mixture A is adjusted to 190°C and the reaction time is adjusted to 9 hours during the preparation of the positive electrode active material. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0035] Example 14 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that the reaction temperature of mixture A is adjusted to 160°C and the reaction time is adjusted to 12 hours during the preparation of the positive electrode active material. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0036] Example 15 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that the reaction temperature of mixture A is adjusted to 200°C and the reaction time is adjusted to 8 hours during the preparation of the positive electrode active material. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0037] Example 16 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that, in the process of preparing the positive electrode active material, an equal mass of V4C3T is used. x (Brand name: Xianfeng Nano XFK19) Replaces Ti3C2T in Example 1 xApart from the differences mentioned above, the materials, formulation ratios, and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0038] Example 17 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that in the process of preparing the positive electrode active material, an equal mass of Nb4C3T is used. x (Brand name: Xianfeng Nano XFK15) Replaces Ti3C2T in Example 1 x Apart from the differences mentioned above, the materials, formulation ratios, and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0039] Example 18 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that, in the process of preparing the positive electrode active material, an equal mass of MoS2 is used to replace NiS in Example 1. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0040] Example 19 This embodiment prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this embodiment and Example 1 is that in the process of preparing the positive electrode active material, an equal mass of CoS is used to replace NiS in Example 1. Apart from the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.
[0041] Comparative Example 1 This comparative example prepares a positive electrode sheet according to the preparation method provided in Example 1. The difference between this comparative example and Example 1 is that, in the process of preparing the positive electrode active material, an equal mass of NiS is used to replace Ti3C2T in Example 1. x Apart from the differences mentioned above, the materials, formulation ratios, and preparation operations used in this comparative example are strictly consistent with those in Example 1.
[0042] Comparative Example 2 This comparative example provides a positive electrode sheet, the preparation method of which includes the following steps: S1. Preparation of the positive electrode active material: Silicon source material and manganese source material were dissolved in deionized water to obtain mixture A. In the materials used above, the silicon source material was Na₂SiO₃·9H₂O, and the manganese source material was MnCl₂·4H₂O. The molar ratio of Na₂SiO₃·9H₂O to MnCl₂·4H₂O was 1:1. Subsequently, mixture A was reacted at 180℃ for 10 hours, followed by centrifugation. The resulting solid was then placed in a vacuum drying oven at 60℃ and vacuum-dried for 12 hours to obtain the positive electrode active material.
[0043] S2. Preparation of the positive electrode sheet: The above-mentioned positive electrode active material, binder, and conductive agent are stirred evenly to obtain a positive electrode slurry. Among the materials used above, the binder is PVDF and the conductive agent is SuperP. The mass ratio of positive electrode active material: binder: conductive agent is 8:1:1. Subsequently, the above-mentioned positive electrode slurry is coated on carbon paper and dried at a temperature of 60°C for 12 hours, thereby forming a positive electrode active material layer on the surface of the carbon paper, thus obtaining the positive electrode sheet of this comparative example.
[0044] Test case 1. Test objects: The positive electrode sheets provided in Examples 1 to 19 and Comparative Examples 1 to 2 are used as the test objects in this test example.
[0045] 2. Test items: (1) Specific capacitance value: A three-electrode testing system was used. The electrolyte in the electrolytic cell was 0.5M Na2SO4 solution. The reference electrode was Ag / AgCl electrode, the counter electrode was Pt electrode, and the working electrode was the above-mentioned test object. Under the condition of working voltage range of 0V-0.8V, GCD (constant current charge-discharge) test was performed on the electrochemical workstation to test the specific capacitance value of the test object at current densities of 1, 2, and 5A / g.
[0046] (2) Capacitance retention rate: The capacitance retention rate is calculated as shown in Equation 1: Capacitance retention rate (%) = ×100% Formula 1 3. Test Results: Table 1. Relevant performance test results of the test subjects
[0047] The specific capacitance and capacitance retention rates of the positive electrode sheets provided in Examples 1-19 and Comparative Examples 1-2, measured at current densities of 1, 2, and 5 A / g, are shown in Table 1. It can be seen that the specific capacitance and capacitance retention rates of the positive electrode sheets provided in Examples 1-19, measured at current densities of 1, 2, and 5 A / g, are higher than those of Comparative Examples 1-2.
[0048] Compared to Example 1, the difference in the positive electrode composition of Comparative Examples 1 and 2 lies in the positive electrode active material. Test data shows that the specific capacitance and capacitance retention of the positive electrode provided in Example 1 at current densities of 1, 2, and 5 A / g are higher than those in Comparative Examples 1 and 2. This indicates that in this invention, Mxene material possesses good conductivity, enabling the establishment of high-speed transport channels for the positive electrode active material. The surface functional groups of Mxene material reduce particle aggregation and volume expansion after long cycling, while simultaneously improving the wettability between the positive electrode made from this active material and the electrolyte. Therefore, this invention uses manganese silicate material modified with Mxene as the positive electrode active material, which possesses good conductivity, structural stability, and a high ion transport rate.
[0049] Compared to Example 1, the difference in the composition of the positive electrode sheet provided in Example 10 is that the addition of metal sulfide (NiS) is omitted during the preparation of the positive electrode active material. Test data shows that the specific capacitance and capacitance retention of the positive electrode sheet provided in Example 1 at current densities of 1, 2, and 5 A / g are higher than those in Example 10. This indicates that the introduction of metal sulfide allows some metal ions to replace Mn²⁺ in the manganese silicate material, introducing oxygen vacancies within the positive electrode active material. These oxygen vacancies provide additional active sites, which not only adsorb ions and increase capacitance but also provide more channels for ion diffusion, reducing the ion migration barrier and thus improving the rate performance of the positive electrode sheet made from this active material. Furthermore, the bond energy of the chemical bond formed between the metal element and oxygen in the metal sulfide is higher than that of the Mn-O bond, maintaining the structural stability of the positive electrode active material under high current charge-discharge conditions, thereby improving the chemical stability of the electrode.
[0050] Compared with Example 1, the difference in the composition of the positive electrode sheets provided in Examples 12-15 lies in the reaction time and reaction temperature used in the preparation of the positive electrode active material. From the test data, the specific capacitance and capacitance retention of the positive electrode sheet provided in Example 1 at current densities of 1, 2, and 5 A / g are all higher than those in Examples 12-15. This indicates that when the reaction time is 10 hours and the reaction temperature is 180°C, the resulting positive electrode active material possesses better porous structure integrity, effectively reducing ion transport channel obstruction and thus improving the ion transport rate.
[0051] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention, but such modifications or substitutions are all within the scope of protection of the present invention.
Claims
1. A positive electrode active material, characterized by, The raw materials used to prepare the positive electrode active material include manganese silicate and Mxene. The chemical formula of the Mxene material is M n+1 X n T x , 2≤n≤3, wherein M represents a transition metal element, X represents a C element or an N element, T x represents a surface functional group of the Mxene material; The T x comprises at least one of -O, -OH, -F, -Cl, -Br, -I, -NH, -CH3.
2. The positive electrode active material according to claim 1, wherein: The M includes at least one of Ti, V, and Nb.
3. The positive electrode active material according to claim 2, wherein: The M includes Ti.
4. The positive electrode active material according to claim 1, wherein: The raw materials used to prepare the positive electrode active material also include metal sulfides.
5. The positive electrode active material according to claim 4, wherein: The metal sulfide includes at least one of NiS, Ni3S2, NiS2, MoS2, CoS, Co3S2, and CoS2.
6. A method for preparing the positive electrode active material according to any one of claims 1 to 5, characterized in that, Includes the following steps: The manganese silicate material, the Mxene material, and the metal sulfide are mixed to obtain mixture A, and then mixture A is reacted at a temperature of 170~190℃ for 9~11 hours.
7. The method for preparing the positive electrode active material as described in claim 6, characterized in that: The manganese silicate material is prepared from silicon source material and manganese source material; the silicon source material includes Na2SiO3·9H2O; the manganese source material includes MnCl2·4H2O.
8. The method for preparing the positive electrode active material as described in claim 7, characterized in that: The molar ratio of silicon source material to manganese source material is (0.5~1.5):
1.
9. The method for preparing the positive electrode active material as described in claim 6, characterized in that: The mass ratio of the Mxene material to the metal sulfide is (7~13): (4~7).
10. A positive electrode plate, characterized in that: It includes a current collector and a positive electrode active material layer disposed on the surface of the current collector; the positive electrode active material layer includes the positive electrode active material according to any one of claims 1 to 5 or the positive electrode active material prepared by the preparation method according to any one of claims 6 to 9.