A dual-color infrared detector chip for mercury cadmium telluride and its fabrication method
By using indium pillar array flip bonding and epoxy adhesive layer to combine through-holes, blind holes and metal layers in a three-dimensional interconnect structure, the etching stability and alignment accuracy problems in mercury cadmium telluride infrared dual-color detector were solved, and high-performance and high-yield dual-color focal plane array fabrication was achieved.
Patent Information
- Application Number
- CN202611629890.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-17
AI Technical Summary
The existing high-density vertically integrated photodiode structure of mercury cadmium telluride infrared dual-color detectors suffers from problems such as poor stability of through-hole etching, difficulty in three-dimensional micron-level alignment of multi-layer interfaces, and limited pixel duty cycle, which affect device yield and performance.
A three-dimensional interconnect structure combining indium pillar array flip bonding and epoxy adhesive layers with vias, blind vias and metal layers is adopted. High-density interconnects are achieved by vertically stacking two mercury cadmium telluride layers and placing metal layers and n-type layers in the vias and blind vias.
It improves pixel integration and duty cycle, enhances mechanical stability and pixel-level alignment accuracy, simplifies fabrication process, and is suitable for the reliable fabrication of high-performance multispectral infrared focal plane arrays.
Smart Images

Figure CN123124472A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of semiconductor infrared detector technology, and particularly relates to a mercury cadmium telluride infrared dual-color detector chip and its preparation method. Background Technology
[0002] Infrared dual-color detectors can simultaneously respond to and distinguish light radiation in two different wavelength bands, and have important application value in fields such as precision guidance, meteorological remote sensing, resource exploration, and threat identification. Mercury cadmium telluride (MCH) is the preferred material for fabricating high-performance infrared dual-color detectors due to its excellent properties such as continuously tunable bandgap, high quantum efficiency, and fast response speed.
[0003] Currently, the mainstream integration scheme for mercury cadmium telluride (HCd) dual-color detectors involves growing multilayer heterojunction materials on a substrate using molecular beam epitaxy (MBE) or metal-organic chemical vapor deposition (MOCVD) to form a back-to-back photodiode structure. Dual-color detection is then achieved through mesa etching, passivation, and metallization contacts. This approach places stringent requirements on the longitudinal uniformity of the multilayer epitaxial materials and involves multi-step deep etching and heterojunction interface defect control, resulting in complex processes and high costs. Another technological approach is the high-density vertically integrated photodiode (HDVIP) structure developed by DRS. This structure bonds two independent, passivated HCd layers with epoxy resin and uses ion etching to form vertical vias for interconnection with the readout circuitry. It eliminates the need for indium pillar flip-chip interconnects and has been successfully applied in large-area, high-reliability dual-color focal plane arrays. However, this structure, though seemingly simple, actually requires extremely high process precision. In its domestic engineering implementation, it still faces the following challenges: (1) Poor stability of via etching: When etching vias in the composite structure of mercury cadmium telluride and epoxy adhesive, the etching characteristics of the two are significantly different, and the thickness and uniformity of the epoxy adhesive patch directly affect the morphology and process stability of the vias; (2) Difficulty in three-dimensional micron-level alignment: In order to achieve reliable interconnection between the upper and lower diodes and the readout circuit, three-dimensional micron-level precision alignment is required across multiple material interfaces. This not only requires extremely high lateral overlay precision, but also requires overcoming the longitudinal position deviation introduced by the uneven thickness of the epoxy adhesive. The process window is narrow, which restricts the improvement of the yield of large-area array devices; (3) Limited pixel fill factor: The mercury cadmium telluride signal needs to be led out through the annular channel that runs through the entire epoxy adhesive layer. This lead-out structure occupies the pixel area, reducing the effective fill factor of the detector.
[0004] Therefore, there is an urgent need to develop a new mercury cadmium telluride infrared dual-color detector chip and its fabrication method. Summary of the Invention
[0005] To overcome the challenges in HDVIP dual-color stacked interconnect structures, such as insufficient stability of via process due to the difference in etching characteristics between mercury cadmium telluride and epoxy resin, difficulties in three-dimensional micron-level alignment due to multi-layer interface stacking, and limited pixel duty cycle due to the ring-hole channel lead-out method, this invention provides a mercury cadmium telluride infrared dual-color detector chip and its fabrication method, aiming to provide an effective technical approach for high-performance, high-yield, and high-reliability dual-color focal plane arrays.
[0006] To achieve the above objectives, the present invention adopts the following technical solution:
[0007] A mercury cadmium telluride infrared dual-color detector chip includes a readout circuit, a first detector chip layer, and a second detector chip layer; both the upper and lower surfaces of the first and second detector chip layers are provided with CdTe layers.
[0008] The first detection chip layer is flip-bonded to the readout circuit via a first indium pillar array, and the first indium pillar array is surrounded by a first epoxy resin layer; the second detection chip layer is flip-bonded to the first detection chip layer via a second indium pillar array, and the second indium pillar array is surrounded by a second epoxy resin layer.
[0009] The first detection chip layer has a first through hole and a second through hole penetrating the first detection chip layer; the inner wall of the first through hole is provided with a first metal layer, and the bottom of the first through hole is a first indium pillar array; the inner wall of the second through hole is provided with a second metal layer, and the bottom of the second through hole is a readout circuit; a third metal layer is also provided on the first detection chip layer.
[0010] The second detector chip layer is provided with a first blind hole and a second blind hole that do not penetrate the second detector chip layer. The sidewalls and bottom of the first blind hole and the second blind hole are provided with continuous n-type layers. The n-type layers of the second detector chip layer extend to the first surface of the second detector chip layer and are electrically connected to the second indium pillar array.
[0011] The response wavelength of the first detection chip layer is greater than the response wavelength of the second detection chip layer.
[0012] The fabrication method of the above-mentioned mercury cadmium telluride infrared dual-color detector chip includes the following steps:
[0013] S1: Fabricate indium pillars on the first detector chip layer;
[0014] S2: The readout circuit with indium pillars is flip-bonded to the first probe chip layer with indium pillars to form the first indium pillar array, and then epoxy resin is filled and cured to form the first epoxy resin layer.
[0015] S3: Etch a first via and a second via on the first probe chip layer, wherein the bottom of the first via is etched to expose the first indium pillar array, and the bottom of the second via is etched to expose the first epoxy adhesive layer.
[0016] S4: Deposit a first metal layer in the first via, and the first metal layer is connected to the first indium pillar array; deposit a second metal layer in the second via, and the second metal layer is connected to the readout circuit; deposit a third metal layer in the p electrode contact region on the second surface of the first probe chip layer; fabricate indium pillars on the second metal layer and the third metal layer respectively;
[0017] S5: The indium pillars on the second surface of the first detector chip layer are flip-bonded to the indium pillars of the second detector chip layer to form a second indium pillar array, and then epoxy resin is filled and cured to form a second epoxy resin layer;
[0018] S6: Etching the second probe chip layer to form a first blind hole and a second blind hole that do not penetrate the second probe chip layer; during the etching process, an n-type layer is induced to form on the sidewalls and bottom of the first and second blind holes.
[0019] The beneficial effects of this invention are as follows:
[0020] (1) By vertically stacking two mercury cadmium telluride layers and combining them with a three-dimensional interconnection structure of through holes, blind holes and indium pillar arrays, the present invention significantly improves the pixel integration and effectively solves the technical problems of complex etching process and low three-dimensional alignment accuracy in high-density vertically integrated dual-color structure.
[0021] (2) The blind hole design adopted in this invention improves the duty cycle, which is beneficial to achieving high pixel density and high quantum efficiency.
[0022] (3) The preparation method of the present invention not only realizes the two-color stacked structure, but also significantly improves the mechanical stability of the stacked interface and the pixel-level alignment accuracy.
[0023] (4) The preparation process of the present invention is simple and has strong process compatibility, providing an effective way for the reliable preparation of high-performance multispectral infrared focal plane arrays. Attached Figure Description
[0024] Figure 1 This is a cross-sectional structural diagram of the mercury cadmium telluride infrared dual-color detector chip of the present invention.
[0025] In the attached figures, the reference numerals are as follows: 101-readout circuit; 201-first detector chip layer; 202a-first CdTe layer; 202b-second CdTe layer; 203-first via; 204-second via; 205-first metal layer; 206-second metal layer; 207-third metal layer; 208-first passivation layer; 209-first ohmic contact layer; 210-n-type layer of the first detector chip layer; 211-p-type layer of the first detector chip layer; 301-second detector chip layer; 302a-third ...2c-second CdTe layer; 202d-second CdTe layer; 202d-second CdTe layer; 202d-second CdTe layer; 202d-second CdTe layer; 202d-second CdTe layer; 202d-second CdTe layer; 202d-second CdTe layer; 202d-second CdTe layer; 202d-second CdTe layer; 202d-second CdTe layer; 202d-second CdTe layer; 202d-second CdTe layer; 202d-second CdTe layer; 202d-second CdTe layer; 202d-second Cd dTe layer; 302b - fourth CdTe layer; 303 - first blind via; 304 - second blind via; 305 - fourth metal layer; 306 - second passivation layer; 307 - second ohmic contact layer; 308 - third ohmic contact layer; 309 - n-type layer of second probe chip layer; 310 - p-type layer of second probe chip layer; 401 - first indium pillar array; 402 - first epoxy adhesive layer; 403a - first subset of second indium pillar array; 403b - second subset of second indium pillar array; 404 - second epoxy adhesive layer. Detailed Implementation
[0026] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.
[0027] See Figure 1 This invention provides a mercury cadmium telluride infrared dual-color detection chip, which includes a readout circuit 101, a first detection chip layer 201, and a second detection chip layer 301. CdTe layers are disposed on the upper and lower surfaces (first and second surfaces) of both the first and second detection chip layers 201 and 301. In this embodiment, the first and second detection chip layers 201 are vertically stacked. The first detection chip layer 201 is flip-chip bonded to the readout circuit 101 via a first indium pillar array 401, and a first epoxy resin layer 402 surrounds the first indium pillar array 401. The second detection chip layer 301 is flip-chip bonded to the first detection chip layer 201 via a second indium pillar array, and a second epoxy resin layer 404 surrounds the second indium pillar array.
[0028] See Figure 1 The first side of the first detection chip layer 201 is provided with a first CdTe layer 202a, and the first side of the first detection chip layer 201 is bonded to the readout circuit 101. The second side of the first detection chip layer 201 is provided with a second CdTe layer 202b, and the second side of the first detection chip layer 201 is bonded to the second detection chip layer 301.
[0029] The first detection chip layer 201 is provided with a first through hole 203 and a second through hole 204 penetrating the first detection chip layer 201; the inner wall of the first through hole 203 is provided with a first metal layer 205, and the bottom of the first through hole 203 is a first indium pillar array 401; the inner wall of the second through hole 204 is provided with a second metal layer 206, and the bottom of the second through hole 204 is a readout circuit 101; a third metal layer 207 is also provided on the first detection chip layer 201; the third metal layer 207 is located in the second CdTe layer 202b.
[0030] The n-type layer 210 of the first detector chip layer is electrically connected to the readout circuit 101 through the first metal layer 205 and the first indium pillar array 401 in the first via 203; the third metal layer 207 is electrically connected to the p-type layer 211 of the first detector chip layer.
[0031] Preferably, the first detection chip layer 201 further comprises a first passivation layer 208; wherein the first passivation layer 208 at the location of the first via 203 is located above the first metal layer 205, the first passivation layer 208 at the location of the second via 204 is located between the second metal layer 206 and the n-type layer 210 of the first detection chip layer, and the remaining portion of the first passivation layer 208 is located on the surface of the first detection chip layer 201; that is, on the surface of the second CdTe layer 202b. The first passivation layer 208 and the first epoxy adhesive layer 402 together constitute an electrical isolation structure. In this embodiment, the third metal layer 207 is located between the second CdTe layer 202b and the first passivation layer 208, and the third metal layer 207 protrudes from the first passivation layer 208.
[0032] In this embodiment, the inner wall surface of the first through hole 203 is a first passivation layer 208, and the inner wall surface of the second through hole 204 is a second metal layer 206.
[0033] See Figure 1 The second detection chip layer 301 is disposed above the first detection chip layer 201. The second detection chip layer 301 is provided with a first blind hole 303 and a second blind hole 304 that do not penetrate the second detection chip layer 301. The sidewalls and bottom of the first blind hole 303 and the second blind hole 304 are provided with continuous n-type layers. This part of the region is the n-type layer 309 of the second detection chip layer. The n-type layer 309 of the second detection chip layer extends to the first surface of the second detection chip layer 301 and is electrically connected to the second indium pillar array.
[0034] See Figure 1The second probe chip layer 301 is flip-bonded to the first probe chip layer 201 via a second indium pillar array. The second indium pillar array includes a first subset 403a and a second subset 403b of the second indium pillar array; the n-type layer 309 of the second probe chip layer is electrically connected to the first subset 403a of the second indium pillar array; the n-type layer 309 of the second probe chip layer is electrically connected to the readout circuit 101 via the first subset 403a of the second indium pillar array and the second metal layer 206 within the second via 204.
[0035] See Figure 1 The second detector chip layer 301 is further provided with a fourth metal layer 305 that is electrically connected to the p-type layer 310 of the second detector chip layer. The p-type layer 211 of the first detector chip layer and the p-type layer 310 of the second detector chip layer are electrically connected through the third metal layer 207 and the second subset 403b of the second indium pillar array.
[0036] Similarly, a third CdTe layer 302a is disposed on the first surface of the second detector chip layer 301, and a fourth CdTe layer 302b is disposed on the second surface of the second detector chip layer 301.
[0037] In this embodiment, the surface of the second detection chip layer 301 is also provided with a second passivation layer 306. Specifically, the inner surfaces of the first blind hole 303 and the second blind hole 304 are provided with the second passivation layer 306, and the surface of the remaining part of the fourth CdTe layer 302b is provided with the second passivation layer 306.
[0038] Preferably, in this embodiment, the response wavelength of the first detection chip layer 201 is greater than the response wavelength of the second detection chip layer 301.
[0039] Furthermore, the first CdTe layer 202a of the first detector chip layer 201 is provided with a first ohmic contact layer 209 connected to the first indium pillar array 401; the third CdTe layer 302a of the second detector chip layer 301 is provided with a second ohmic contact layer 307 connected to the first subset 403a of the second indium pillar array, and the third CdTe layer 302a of the second detector chip layer 301 is provided with a third ohmic contact layer 308 connected to the second subset 403b of the second indium pillar array.
[0040] Preferably, both the first detector chip layer 201 and the second detector chip layer 301 are made of mercury cadmium telluride. The first passivation layer 208 and the second passivation layer 306 are zinc sulfide; the first metal layer 205 and the second metal layer 206 are indium-gold composite layers; and the third metal layer 207 and the fourth metal layer 305 are chromium-gold composite layers.
[0041] The above-mentioned method for fabricating a mercury cadmium telluride infrared dual-color detector chip includes the following steps:
[0042] S1: Indium pillars are fabricated on the first detector chip layer 201.
[0043] S2: The readout circuit 101 with indium pillars is flip-bonded with the first probe chip layer 201 with indium pillars to form the first indium pillar array 401, and then filled with epoxy resin and cured to form the first epoxy resin layer 402.
[0044] S3: Etch a first via 203 and a second via 204 on the first detector chip layer 201, wherein the bottom of the first via 203 is etched to expose the first indium pillar array 401, and the bottom of the second via 204 is etched to expose the first epoxy adhesive layer 402. The specific operation of step S3 is as follows: First, remove the zinc cadmium telluride substrate to expose the second surface of the mercury cadmium telluride epitaxial layer, which is the second surface of the first detector chip layer 201, and grow a second CdTe layer 202b on this surface; then, define the first via region and the second via region on the second surface of the first detector chip layer 201, and use an ion etching process to prepare the first via 203 and the second via 204 penetrating the first detector chip layer 201.
[0045] S4: Deposit a first metal layer 205 in the first via 203, the first metal layer 205 being connected to the first indium pillar array 401; deposit a second metal layer 206 in the second via 204, the second metal layer 206 being connected to the readout circuit 101; deposit a third metal layer 207 in the p-electrode contact region on the second surface of the first probe chip layer 201; fabricate indium pillars on the second metal layer 206 and the third metal layer 207 respectively.
[0046] S5: The indium pillars on the second surface of the first detector chip layer 201 are flip-bonded to the indium pillars of the second detector chip layer 301 to form a second indium pillar array. Then, epoxy resin is filled and cured to form a second epoxy resin layer 404. The second indium pillar array includes a first subset 403a of the second indium pillar array and a second subset 403b of the second indium pillar array.
[0047] S6: A first blind via 303 and a second blind via 304 that do not penetrate the second detector chip layer 301 are etched. During the etching process, an n-type layer is induced to form on the sidewalls and bottom of the first blind via 303 and the second blind via 304. Specifically, the zinc zinc cadmium substrate used to prepare the second detector chip layer 301 is removed to expose the second surface of the mercury cadmium telluride epitaxial layer, which is the second surface of the second detector chip layer 301. A fourth CdTe layer 302b is grown on this surface. A first blind via region and a second blind via region are defined on the second surface of the second detector chip layer 301. The fourth CdTe layer 302b is etched sequentially from the second surface of the second detector chip layer 301 and penetrates into the interior of the second detector chip layer 301 using an ion etching process to form a first blind via 303 and a second blind via 304 that do not penetrate the layer. During the etching process, an n-type layer 309 of the second detector chip layer is induced to form on the sidewalls and bottom of the first blind via 303 and the second blind via 304.
[0048] Specifically, step S1 includes the following steps:
[0049] S11: Growing a mercury cadmium telluride epitaxial layer on a zinc cadmium telluride substrate, the mercury cadmium telluride epitaxial layer is used to prepare the first detector chip layer 201;
[0050] S12: The first CdTe layer 202a is grown on the first surface of the mercury cadmium telluride epitaxial layer;
[0051] S13: Etch the first CdTe layer 202a to form the first opening, exposing the first surface of the mercury cadmium telluride epitaxial layer; prepare an indium pillar within the first opening.
[0052] Preferably, step S4 specifically includes the following steps:
[0053] S41: Deposit a first metal in the first through hole 203 to form a first metal layer 205;
[0054] S42: Deposit a first passivation layer 208 on the second CdTe layer 202b on the second side of the first probe chip layer 201, then remove the first passivation layer 208 at the bottom of the second via 204, and then continue etching to remove the exposed first epoxy adhesive layer 402 until the pads of the readout circuit 101 are exposed.
[0055] S43: Deposit a second metal in the second through hole 204 to form a second metal layer 206;
[0056] S44: Define a p-electrode contact area on the second surface of the first probe chip layer 201, selectively etch away the first passivation layer 208 and the second CdTe layer 202b in the area to expose the first probe chip layer 201, and then deposit a third metal to form a third metal layer 207.
[0057] S45: Indium pillars are fabricated on the second metal layer 206 and the third metal layer 207, respectively. Specifically, the indium pillars fabricated on the second metal layer 206 are used to form a first subset 403a of the second indium pillar array, and the indium pillars fabricated on the third metal layer 207 are used to form a second subset 403b of the second indium pillar array.
[0058] The indium pillars of the second detector chip layer 301 in step S5 are prepared using the following steps:
[0059] S51: A mercury cadmium telluride epitaxial layer is grown on a cadmium zinc telluride substrate, and the mercury cadmium telluride epitaxial layer is used to prepare the second detector chip layer 301;
[0060] S52: A third CdTe layer 302a is grown on the first surface of the mercury cadmium telluride epitaxial layer;
[0061] S53: Etch the third CdTe layer 302a to form a second opening, exposing the first surface of the mercury cadmium telluride epitaxial layer; prepare an indium pillar within the second opening.
[0062] More preferably, before fabricating the indium pillar, the CdTe passivation layer is selectively etched to form an opening, and then an ohmic contact metal layer is deposited within the opening. The ohmic contact metal layer is an In / Au stack or a Cr / Au stack.
[0063] Specifically, before fabricating the indium pillar within the first opening, the process includes a step of depositing a first ohmic contact layer 209 within the first opening; then, the indium pillar is fabricated on the first ohmic contact layer 209.
[0064] Before fabricating indium pillars within the second opening, the process includes depositing a second ohmic contact layer 307 and a third ohmic contact layer 308 within the second opening, respectively; then, indium pillars are fabricated on the second ohmic contact layer 307 and the third ohmic contact layer 308, respectively. The second ohmic contact layer 307 is used to contact the n-type layer 309 of the subsequently formed second detector chip layer, and the third ohmic contact layer 308 is used to contact the p-type layer 310 of the second detector chip layer. During bonding, the first subset 403a of the second indium pillar array is correspondingly connected to the second ohmic contact layer 307, and the second subset 403b of the second indium pillar array is correspondingly connected to the third ohmic contact layer 308.
[0065] Preferably, the following steps are included after step S6:
[0066] S7: A second passivation layer 306 is deposited on the entire surface of the second side of the second probe chip layer 301, covering the inner surfaces of the first blind hole 303 and the second blind hole 304 and the fourth CdTe layer 302b of the second probe chip layer 301.
[0067] S8: Define a p-electrode contact area on the second surface of the second probe chip layer 301, selectively etch away the second passivation layer 306 and the fourth CdTe layer 302b of the p-electrode contact area of the second probe chip layer 301 to expose the second probe chip layer 301, and then deposit a fourth metal to form a fourth metal layer 305.
[0068] Preferably, ion etching is achieved by plasma etching, and the process gas used is selected from one of Ar, Ar / CH4 mixed gas and Ar / CH4 / H2 mixed gas.
[0069] Example 1:
[0070] This embodiment provides a mercury cadmium telluride infrared dual-color detection chip (short-wave / mid-wave dual-color detection chip), wherein the second detection chip layer 301 responds to short-wave infrared (SWIR, 1~3 μm) and the first detection chip layer 201 responds to mid-wave infrared (MWIR, 3~5 μm).
[0071] The specific preparation steps are as follows:
[0072] (1) Fabrication of the first detector chip layer 201 and formation of the first indium pillar: A mid-wave mercury cadmium telluride epitaxial layer (Cd composition is 0.30, Cd composition refers to Hg) is grown on a cadmium zinc telluride substrate. 1-x Cd x (x value in Te) A first CdTe layer 202a with a diameter of 200 nm is grown on the first surface of the mercury cadmium telluride epitaxial layer; the first CdTe layer 202a is etched by photolithography to form a first opening, exposing the surface of the mercury cadmium telluride epitaxial layer; In / Au (where In is 10 nm and Au is 50 nm) is deposited in the first opening to form a first ohmic contact layer 209; then an indium pillar with a diameter of 6 μm and a height of 5 μm is prepared on the first ohmic contact layer 209 by photolithography and evaporation.
[0073] (2) Provide a readout circuit 101: Specifically, provide a readout circuit 101 with corresponding indium pillars (5 μm in height and 6 μm in diameter).
[0074] (3) Flip bonding and filling: The readout circuit 101 is flip-bonded with the first surface of the mercury cadmium telluride epitaxial layer in step (1) to form the first indium pillar array 401, and then epoxy glue is filled in the gap to form the first epoxy glue layer 402.
[0075] (4) Removal of substrate and growth of back passivation layer: The zinc cadmium telluride substrate is removed by mechanical grinding combined with chemical etching to expose the second side of the mercury cadmium telluride epitaxial layer, and a second CdTe layer 202b with a diameter of 200 nm is grown on this side.
[0076] (5) Etching vias: On the second surface of the first detector chip layer 201, photolithography is used to define the first via region and the second via region with a diameter of 5 μm; through-holes are prepared by inductively coupled plasma etching (ICP), and the etching gas is a mixture of Ar / CH4 / H2 gas (flow ratio 8:3:1); the bottom of the first via 203 is etched to expose the first indium pillar array 401, and the bottom of the second via 204 is etched to expose the first epoxy adhesive layer 402. During the etching process, ion bombardment induces a change in the conductivity type of the mercury cadmium telluride material in the sidewalls and surrounding areas of the vias, forming an n-type layer.
[0077] (6) Deposit the first metal layer 205: Photolithography exposes the first via 203, and sputter In / Au (In 20 nm / Au 200 nm) into the first via 203 to cover the inner surface of the first via 203, forming the first metal layer 205, and making the first metal layer 205 connected to the first indium pillar array 401.
[0078] (7) Etching the passivation layer and epoxy adhesive at the bottom of the second via: Deposit 300nm ZnS as the first passivation layer 208 on the entire surface of the second side of the first probe chip layer 201, then expose the second via 204 by photolithography, perform anisotropic etching by inductively coupled plasma etching (ICP), and analyze the etching process by endpoint detection until the metal layer on the pad of the readout circuit 101 is exposed.
[0079] (8) Deposit the second metal layer 206: Deposit In / Au (In 20nm / Au 200nm) in the second via 204 to form the second metal layer 206, so that it is connected to the pad of the readout circuit 101.
[0080] (9) Forming the p-type electrode of the first detector chip layer 201: The p-electrode contact area is defined by photolithography on the second surface of the first detector chip layer 201, and the first passivation layer 208 and the second CdTe layer 202b in the area are removed by etching to expose the surface of the first detector chip layer 201. Then, Cr / Au (Cr 20 nm / Au 500 nm) is deposited to form the third metal layer 207.
[0081] (10) Fabrication of indium pillars for the second indium pillar array: Indium pillars (5 μm in height) are fabricated on the second metal layer 206 and the third metal layer 207, respectively. The indium pillars located on the second metal layer 206 are used to form the first subset 403a of the second indium pillar array, corresponding to n-type signal extraction; the indium pillars located on the third metal layer 207 are used to form the second subset 403b of the second indium pillar array, corresponding to p-type interconnection.
[0082] (11) Fabrication of the second detector chip layer 301 and indium pillars: A short-wavelength mercury cadmium telluride epitaxial layer (Cd composition 0.40) with a thickness of 8 μm is grown on a cadmium zinc telluride substrate as the second detector chip layer 301; a third CdTe layer 302a with a thickness of 200 nm is grown on the first side of the second detector chip layer 301 (i.e. the side that will subsequently bond with the first detector chip layer); two opening regions are formed by photolithography etching: one corresponding to an n-type ohmic contact and the other corresponding to a p-type ohmic contact. The two opening regions are the second openings on the first side of the second detector chip layer 301. A second ohmic contact layer 307 that will subsequently contact the n-type layer 309 of the second detector chip layer and a third ohmic contact layer 308 that will contact the p-type layer 310 of the second detector chip layer are deposited in the second openings, respectively; wherein the second ohmic contact layer 307 is In / Au (In 10 nm / 50 Au nm), and the third ohmic contact layer 308 is Cr / Au (Cr 10 nm / Au 50 nm). nm); then, indium pillars with a height of 5 μm were prepared on the second ohmic contact layer 307 and the third ohmic contact layer 308, respectively.
[0083] (12) Bonding the second probe chip layer 301 to the first probe chip layer 201: The indium pillars on the first surface of the second probe chip layer 301 and the indium pillars on the second surface of the first probe chip layer 201 are flip-chip bonded to form a second indium pillar array. The first subset 403a of the second indium pillar array is connected to the second ohmic contact layer 307, and the second subset 403b of the second indium pillar array is connected to the third ohmic contact layer 308. The bonding conditions are the same as in step (3). Then, epoxy resin is filled and cured to form a second epoxy resin layer 404.
[0084] (13) Removing the substrate of the second detector chip layer 301 and growing the fourth CdTe layer 302b: The zinc cadmium telluride substrate used to prepare the second detector chip layer 301 is removed by mechanical grinding combined with chemical etching, exposing the second side (i.e. the upper surface) of the mercury cadmium telluride epitaxial layer, and a 200nm fourth CdTe layer 302b is grown on this side.
[0085] (14) Etching blind vias and forming an n-type layer in situ: On the second surface of the second detector chip layer 301, a first blind via region and a second blind via region with a diameter of 5 μm are defined by photolithography; using an ion etching process, the fourth CdTe layer 302b is sequentially etched from the second surface and penetrates into the interior of the second detector chip layer 301 to form a first blind via 303 and a second blind via 304 with a depth of approximately 6 μm that do not penetrate through. During the etching process, ions bombard the mercury cadmium telluride material, inducing a change in its conductivity type, thereby forming a continuous n-type layer on the sidewalls and bottom of the blind vias.
[0086] (15) Deposit a second passivation layer 306: Deposit a ZnS layer with a thickness of 200 nm as a second passivation layer 306 on the surface of the second side of the entire second detector chip layer 301. The passivation layer covers the inner surfaces of the first blind hole 303 and the second blind hole 304 and the surface of the second detector chip layer 301.
[0087] (16) Forming the p-type electrode of the second detector chip layer 301: Photolithographically define the p-electrode contact area on the second surface of the second detector chip layer 301, etch away the second passivation layer 306 and the fourth CdTe layer 302b in the area, expose the surface of the second detector chip layer 301, and then deposit Cr / Au (Cr20 nm / Au 200 nm) to form the fourth metal layer 305.
[0088] The mercury cadmium telluride infrared dual-color detector chip finally obtained in Example 1 has an upper short-wave channel with a response cutoff wavelength of 2.9 μm and a lower medium-wave channel with a response cutoff wavelength of 5.2 μm at 77K.
[0089] Example 2:
[0090] This embodiment provides a mercury cadmium telluride infrared dual-color detection chip (mid-wave / long-wave dual-color detection chip), wherein the second detection chip layer 301 responds to mid-wave infrared (MWIR, 3~5 μm), and the first detection chip layer 201 responds to long-wave infrared (LWIR, 8~12 μm).
[0091] The specific preparation steps are basically the same as in Example 1. The differences are as follows:
[0092] In step (1), a long-wavelength mercury cadmium telluride epitaxial layer (Cd composition of 0.22) is grown on a cadmium zinc telluride substrate.
[0093] The ICP etching gas in step (5) is an Ar / CH4 mixture with a flow rate ratio of 10:1.5.
[0094] In step (11), the Cd component in the mercury cadmium telluride epitaxial layer of the second detector chip layer 301 corresponds to the medium wave (Cd component is 0.30).
[0095] In step (14), the etching gas is an Ar / CH4 mixture with a flow rate ratio of 10:1.5.
[0096] The mercury cadmium telluride infrared dual-color detector chip finally obtained in Example 2 has an upper mid-wave channel with a response cutoff wavelength of 5.2 μm and a lower long-wave channel with a response cutoff wavelength of 10.2 μm at 77 K.
[0097] Those skilled in the art will readily understand that the above are merely preferred embodiments of the present invention. The above embodiments are provided only for the purpose of describing the present invention and are not intended to limit the present invention. The parts of the present invention not described in detail are well known in the art and are not intended to limit the scope of the present invention. The scope of the present invention is defined by the appended claims. All equivalent substitutions and modifications made without departing from the spirit and principle of the present invention should be covered within the scope of the present invention.
Claims
1. A mercury cadmium telluride infrared dual-color detection chip, characterized in that, It includes a readout circuit, a first detector chip layer, and a second detector chip layer; both the upper and lower surfaces of the first and second detector chip layers are provided with a CdTe layer. The first detection chip layer is flip-bonded to the readout circuit via a first indium pillar array, and the first indium pillar array is surrounded by a first epoxy resin layer; the second detection chip layer is flip-bonded to the first detection chip layer via a second indium pillar array, and the second indium pillar array is surrounded by a second epoxy resin layer. The first detection chip layer has a first through hole and a second through hole penetrating the first detection chip layer; the inner wall of the first through hole is provided with a first metal layer, and the bottom of the first through hole is a first indium pillar array; the inner wall of the second through hole is provided with a second metal layer, and the bottom of the second through hole is a readout circuit; a third metal layer is also provided on the first detection chip layer. The second detector chip layer is provided with a first blind hole and a second blind hole that do not penetrate the second detector chip layer. The sidewalls and bottom of the first blind hole and the second blind hole are provided with continuous n-type layers. The n-type layers of the second detector chip layer extend to the first surface of the second detector chip layer and are electrically connected to the second indium pillar array. The response wavelength of the first detection chip layer is greater than the response wavelength of the second detection chip layer.
2. The mercury cadmium telluride infrared dual-color detection chip according to claim 1, characterized in that, The n-type layer of the first detector chip layer is electrically connected to the readout circuit through the first metal layer and the first indium pillar array in the first through-hole. The third metal layer is electrically connected to the p-type layer of the first detector chip layer.
3. The mercury cadmium telluride infrared dual-color detection chip according to claim 1, characterized in that, The first detection chip layer is also provided with a first passivation layer, wherein the first passivation layer at the second via location is located between the second metal layer and the n-type layer of the first detection chip layer; The inner surfaces of the first and second blind holes are provided with a second passivation layer.
4. The mercury cadmium telluride infrared dual-color detection chip according to claim 2, characterized in that, The second indium pillar array includes a first subset and a second subset; the n-type layer of the second probe chip layer is electrically connected to the first subset of the second indium pillar array; the n-type layer of the second probe chip layer is electrically connected to the readout circuit through the first subset of the second indium pillar array and the second metal layer in the second via.
5. The mercury cadmium telluride infrared dual-color detection chip according to claim 4, characterized in that, The second detector chip layer is further provided with a fourth metal layer that is electrically connected to the p-type layer of the second detector chip layer. The p-type layer of the first detector chip layer and the p-type layer of the second detector chip layer are electrically connected through the third metal layer and the second subset of the second indium pillar array.
6. The mercury cadmium telluride infrared dual-color detection chip according to claim 4, characterized in that, A first ohmic contact layer connected to the first indium pillar array is disposed on the first CdTe layer of the first detector chip layer; The third CdTe layer of the second detector chip layer is provided with a second ohmic contact layer connected to the first subset of the second indium pillar array.
7. The method for preparing the mercury cadmium telluride infrared dual-color detection chip according to any one of claims 1 to 6, characterized in that, Includes the following steps: S1: Fabricate indium pillars on the first detector chip layer; S2: The readout circuit with indium pillars is flip-bonded to the first probe chip layer with indium pillars to form the first indium pillar array, and then epoxy resin is filled and cured to form the first epoxy resin layer. S3: Etch a first via and a second via on the first probe chip layer, wherein the bottom of the first via is etched to expose the first indium pillar array, and the bottom of the second via is etched to expose the first epoxy adhesive layer. S4: Deposit a first metal layer in the first via, and the first metal layer is connected to the first indium pillar array; deposit a second metal layer in the second via, and the second metal layer is connected to the readout circuit; deposit a third metal layer in the p electrode contact region on the second surface of the first probe chip layer; fabricate indium pillars on the second metal layer and the third metal layer respectively; S5: The indium pillars on the second surface of the first detector chip layer are flip-bonded to the indium pillars of the second detector chip layer to form a second indium pillar array, and then epoxy resin is filled and cured to form a second epoxy resin layer; S6: Etching the second probe chip layer to form a first blind hole and a second blind hole that do not penetrate the second probe chip layer; during the etching process, an n-type layer is induced to form on the sidewalls and bottom of the first and second blind holes.
8. The method for preparing the mercury cadmium telluride infrared dual-color detection chip according to claim 7, characterized in that, Step S1, which involves fabricating indium pillars on the first detector chip layer, specifically includes the following steps: S11: Growing a mercury cadmium telluride epitaxial layer on a cadmium zinc telluride substrate, the mercury cadmium telluride epitaxial layer is used to prepare the first detector chip layer; S12: The first CdTe layer is grown on the first surface of the mercury cadmium telluride epitaxial layer; S13: Etch the first CdTe layer to form the first opening, exposing the first surface of the mercury cadmium telluride epitaxial layer; fabricate an indium pillar within the first opening; Step S4 specifically includes the following steps: S41: Deposit metal in the first through-hole to form a first metal layer; S42: Deposit a first passivation layer on the second side of the first probe chip layer, then remove the first passivation layer at the bottom of the second via, and then continue etching to remove the exposed first epoxy adhesive layer until the pads of the readout circuit are exposed; S43: Deposit a second metal in the second through hole to form a second metal layer; S44: Define a p-electrode contact region on the second surface of the first probe chip layer, selectively etch away the first passivation layer and the second CdTe layer in the region to expose the first probe chip layer, and then deposit a third metal to form a third metal layer. S45: Indium pillars are fabricated on the second and third metal layers, respectively; The indium pillars of the second detector chip layer in step S5 are prepared using the following steps: S51: A mercury cadmium telluride epitaxial layer is grown on a zinc cadmium telluride substrate, and the mercury cadmium telluride epitaxial layer is used to prepare the second detector chip layer; S52: A third CdTe layer is grown on the first surface of the mercury cadmium telluride epitaxial layer; S53: Etch the third CdTe layer to form a second opening, exposing the first surface of the mercury cadmium telluride epitaxial layer; prepare an indium pillar within the second opening.
9. The method for preparing the mercury cadmium telluride infrared dual-color detection chip according to claim 8, characterized in that, The process includes a step of depositing a first ohmic contact layer within the first opening before fabricating the indium pillar within the first opening; then, the indium pillar is fabricated on the first ohmic contact layer. Before fabricating the indium pillar within the second opening, the process includes depositing a second ohmic contact layer and a third ohmic contact layer within the second opening, respectively; then, indium pillars are fabricated on the second ohmic contact layer and the third ohmic contact layer, respectively.
10. The method for preparing the mercury cadmium telluride infrared dual-color detection chip according to claim 7, characterized in that, The following steps are included after step S6: S7: Deposit a second passivation layer on the entire surface of the second side of the second probe chip layer; S8: Define a p-electrode contact area on the second surface of the second probe chip layer, selectively etch away the second passivation layer and the fourth CdTe layer of the p-electrode contact area of the second probe chip layer to expose the second probe chip layer, and then deposit to form the fourth metal layer.